Preparation method and application of micro-nano fluorosilicone polymer coated color hard ball digital ink-jet ink

By introducing micro-nano-grade fluorosilicone polymer coated colored hard balls into digital inkjet ink, the problems of uneven particle size and low solubility of pigment ink are solved, and the preparation of high-solubility dyes is achieved, which improves the hydrophobicity of printed fabrics and It feels suitable for a variety of digital printing equipment and has broad market prospects.

CN118994969APending Publication Date: 2024-11-22ZHEJIANG NAMEI MATERIAL TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411234324.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Pigment inks in traditional digital inkjets have problems such as uneven particle size, complex distribution, and easy to block the nozzle. The solubility of reactive anthraquinone dye in monomers is low, resulting in lighter printing color, fabric feel and breathable performance. Not good.

Method used

通过引入微纳级氟硅聚合物包覆彩色硬球,采用蒽醌型分散染料、苯乙烯共聚单体、有机氟硅单体和软单体进行阳离子开环聚合,制备高溶解度可聚合染料,形成微纳级氟硅聚合物包覆彩色硬球墨水,解决了颗粒大小和分布不均的问题,并提高了印花织物的疏水性和手感。

Benefits of technology

It has achieved micro-nano-grade fluorosilic polymer-coated colored hard ball ink with small particle size and good storage stability. It has excellent wet and dry friction properties and hydrophobicity of printed fabrics. It has a good feel and breaks the monopoly of foreign inks and is suitable for Various digital printing equipment have good market application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994969A_ABST
    Figure CN118994969A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of micro-nano fluorosilicone polymer coated color hard ball digital ink-jet ink, and belongs to the field of fine chemical engineering. The preparation method of the fluorosilicone polymer coated colored hard ball digital ink-jet ink comprises the following steps: dissolving a high-solubility reactive dye in a styrene monomer, and preparing a polystyrene colored hard ball seed emulsion through free radical polymerization; and injecting an organic fluorosilicone monomer and an acrylate monomer as shell layers into the seed emulsion, and preparing the fluorosilicone polymer coated color hard ball digital ink-jet ink through free radical polymerization and cation ring-opening polymerization. The fluorosilicone polymer coated color hard ball digital ink-jet ink has the advantages of small particle size, good storage stability, controllable latex ink structure and the like, and the micro-nano fluorosilicone polymer coated color hard ball digital ink-jet ink can be applied to digital printing and endows fabrics with excellent waterproofness, air permeability and softness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of textiles, and in particular to a preparation method and application of a micro-nano fluorosilicone polymer coated color hard ball digital inkjet ink Background Art

[0002] Inkjet printing technology makes up for the technical defects and gaps of traditional printing due to its high printing precision, excellent color design, and green environmental protection. In recent years, the consumption of digital inkjet ink has been growing continuously, and the cost of inkjet ink accounts for 30% of the inkjet cost. In order to adapt to this technology, the development of inkjet ink has become the research focus of many scholars and enterprises. High-speed ink research and development is an inevitable trend in the development of inkjet printing. Compared with dye ink, pigment ink has great development potential due to its versatility. However, pigment ink still has problems to be solved. Pigment ink has large and small particles and uneven distribution, which makes the formation of ink droplets complicated and easy to clog the nozzles of traditional printing. Color hard balls can become new colorants to replace pigments due to their nano-particle size and high stability.

[0003] Color hard balls, which convert low-molecular dyes into polymers, are directly attached to the fabric surface with the help of the adhesion of polymers. No external dyes and film-forming agents are required. The process is simple and meets the market demand for safety and environmental protection. It is considered to be one of the effective ways to solve the above-mentioned pigment ink problems. The dye matrix is ​​introduced into the polymer main chain or side group through polymerization reaction, which not only retains the characteristics of dye absorption and color development, but also has the characteristics of high-resolution materials such as migration resistance and processability. However, the solubility of reactive dyes in polymer monomers is low, resulting in a lighter printing color depth; the printed fabric has poor hand feel and air permeability, which limits the large-scale use of hard ball inks.

[0004] Introducing fluorine-silicon segments into colored hard balls can significantly improve the feel of printed fabrics and give them good hydrophobic properties. For example, Yang Yi et al. successfully introduced vinyl trimethoxysilane and anthraquinone dye monomers into acrylate segments through emulsion polymerization to obtain self-crosslinking silicone-modified self-coloring latex, but did not introduce organic fluorine segments, resulting in poor migration ability of the latex film. The feel, color fastness and air permeability of the coated fabric still need to be improved. In addition, due to the poor solubility of reactive anthraquinone dyes in monomers, the color depth of printed fabrics is relatively shallow. Li Shaoqi et al. first synthesized fluorine-silicon macromolecular monomers with vinyl end-capping, prepared fluorine-silicon-modified polyacrylate emulsions through emulsion polymerization, and used them for liquid disperse dye printing, which improved the hydrophobicity and softness of printed fabrics. However, due to the thermal migration of small dye molecules, the friction fastness of the printed fabrics was poor. Summary of the invention

[0005] The present invention provides a method for preparing a digital inkjet ink of micro-nano fluorosilicone polymer-coated colored hard balls, wherein the traditional disperse dyes are modified to prepare highly soluble polymerizable dyes; subsequently, a colored hard ball emulsion is prepared by free radical copolymerization; then, an organic fluorosilicone monomer and a soft monomer are introduced as a shell layer to coat the hard ball seed emulsion by cationic ring-opening polymerization and free radical polymerization, and finally, the micro-nano fluorosilicone polymer-coated colored hard ball ink is obtained by adjusting the inkjet parameters. The micro-nano fluorosilicone polymer-coated colored hard ball ink has the advantages of small particle size, good storage stability, excellent dry and wet friction performance, good hydrophobicity of printed fabrics, good hand feel, etc. It can be adapted to various digital printing equipment, breaking the monopoly of foreign inks, and has good market application prospects.

[0006] A method for preparing a micro-nano-level fluorosilicone polymer-coated color hard ball digital inkjet ink comprises the following steps: (1) Anthraquinone disperse dyes are used as raw materials, double bond-containing monomers and aromatic hydrocarbon monomers are introduced to synthesize reactive anthraquinone dyes composed of anthraquinone matrix, linker group and polymerizable group; (2) Styrene is used as a comonomer, highly soluble reactive anthraquinone dyes, initiators, water and emulsifiers are added and fully ultrasonically dissolved, and a seed color hard ball emulsion is prepared by a free radical polymerization process; (3) The styrene color hard ball seed emulsion is transferred to a reactor, and organic fluorosilicone monomers and soft monomers are used as shell layers, and initiators, crosslinkers, water, emulsifiers and cationic ring openers are injected into the reactor for free radical polymerization and cationic ring opening mini-emulsion polymerization to prepare micro-nano fluorosilicone polymer coated color hard ball emulsion. (4) Moisturizers, pH regulators and surface tension regulators are added to the fluorosilicone polymer coated color hard ball emulsion for regulation, and finally a micro-nano fluorosilicone polymer coated color hard ball digital inkjet ink is prepared.

[0007] Furthermore, a method for preparing a micro-nano-level fluorosilicone polymer-coated color hard ball digital inkjet ink comprises the following steps:

[0008] (1) Preparation of highly soluble reactive anthraquinone dyes: Weigh one of the hydroxyethyl methacrylates, an acid binder, and toluene into a reactor equipped with a stirrer, a nitrogen inlet and outlet line, and a thermometer. The solution is cooled to nearly 0°C under a nitrogen atmosphere. Add cyanuric chloride at a temperature of 0-5°C and stir for 48 hours. Then add CI Disperse Red 60, stir at 40-50°C for 48 hours, then heat to 100°C, add phenol, maintain the temperature for reaction for 8 hours, cool to room temperature, filter with a sand core funnel, and evaporate the filtrate. Stir the residue with distilled water, filter with a sand core funnel, and evaporate the filtrate to dryness to obtain a highly soluble reactive anthraquinone dye. The structure of the highly soluble reactive anthraquinone dye is as follows:

[0009] (2) Preparation of colored hard ball emulsion: highly soluble reactive anthraquinone dye and initiator are dissolved in acrylic monomer to form oil phase, emulsifier is dissolved in deionized water to form water phase, oil phase is poured into water phase for pre-emulsification for 20 min to form a coarse emulsion. After pre-emulsification, the emulsion is placed in an ice water bath for ultrasonic treatment for 20 min. The obtained pre-emulsion is transferred to a reaction vessel equipped with a condenser and a mechanical stirrer and N2 is introduced for 15 min. Finally, the emulsion is reacted in a 70°C water bath for 8 h to prepare a colored hard ball seed emulsion.

[0010] (3) Preparation of micro-nano fluorosilicone polymer-coated colored hard ball emulsion: The colored hard ball seed emulsion is added into a reactor, with organic fluorosilicone monomer, soft monomer, initiator, and cross-linking agent as the oil phase; water, emulsifier, and cationic ring-opener as the aqueous phase. The oil phase is poured into the aqueous phase and emulsified for 20 minutes. After pre-emulsification, the emulsion is placed in an ice water bath and ultrasonicated for 20 minutes, then injected into the reactor and reacted at 75°C for 8 hours to prepare micro-nano fluorosilicone polymer-coated colored hard ball emulsion.

[0011] (4) Regulation of digital inkjet ink for micro-nano fluorosilicone polymer coated color hard ball: Moisturizer, pH regulator, and surface tension regulator are added to the fluorosilicone polymer coated color hard ball emulsion for regulation, and finally, digital inkjet ink for micro-nano fluorosilicone polymer coated color hard ball is prepared.

[0012] Furthermore, in steps (2) and (3), the concentration of the colored hard ball seed emulsion is 15 wt% to 30 wt%, and the concentration of the shell emulsion is 10 wt% to 25 wt%.

[0013] Furthermore, in steps (2) and (3), the emulsifier is an anionic surfactant, which is one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate, and the amount used is 3wt% to 5wt% of the monomer.

[0014] Furthermore, in steps (2) and (3), the initiator is one or two of azobiscyanovaleric acid, azobisisobutylamidine hydrochloride, azobisisobutyronitrile, and potassium persulfate. The amount of the initiator in steps (2) and (3) is 1% to 5% of the hard monomer and the reactive dye, and the amount of the initiator in steps (3) and (3) is 1% to 3% of the organic fluorine silicon monomer and the soft monomer.

[0015] Furthermore, in step (2), the amount of the reactive anthraquinone dye used is 9 wt % of the total monomers.

[0016] Furthermore, the emulsifier in step (2) is an anionic surfactant, which is any one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate, and the amount used is 3wt% to 5wt% of the total monomers.

[0017] Furthermore, in step (2), the organic fluorine monomer and the organic silicon monomer are octamethylcyclotetrasiloxane and trifluoropropylmethylcyclotrisiloxane in a ratio of 1:0-0:1, the cationic ring opener is dodecylbenzenesulfonic acid, and the crosslinking agent is vinyltrimethoxysilane or one of vinyltrimethoxysilane.

[0018] Furthermore, the moisturizing agent in step (3) is stearyl alcohol polyoxyethylene ether, and the total dosage is 3wt%-5wt% of the fluorosilicone coated seed colored hard ball ink; the surfactant regulator is a non-ionic defoaming wetting agent, and the dosage is 0.05wt%-1wt% of the colored fluorosilicone coated seed colored hard ball ink; the pH regulator is any one of sodium carbonate, sodium bicarbonate, sodium hydroxide, and potassium carbonate, and the pH of the micro-nano fluorosilicone polymer coated colored hard ball ink is controlled to be 7-9.

[0019] Furthermore, the surface tension of the fluorosilicone coated seed color hard ball ink in step (3) is controlled to be 20mN / m-35mN / m, and the viscosity is controlled to be 2-5cp.

[0020] In detail, the present invention provides a method for preparing a color hard ball ink for digital inkjet printing, which mainly comprises the following steps:

[0021] (1) Preparation of colored hard-ball emulsion: 9wt% of highly soluble reactive anthraquinone dye and 1wt% to 5wt% of initiator of the total monomers were dissolved in styrene to form an oil phase, 3wt% to 5wt% of emulsifier of the total monomers were dissolved in deionized water to form an aqueous phase, and the oil phase was poured into the aqueous phase for pre-emulsification for 20min (power of 650W) to form a coarse emulsion. After pre-emulsification, the emulsion was placed in an ice-water bath and ultrasonicated for 20min. The obtained pre-emulsion was transferred to a three-necked round-bottom flask equipped with a condenser and a mechanical stirrer for reaction and N2 was introduced for 15min. Finally, the emulsion was reacted in a 70℃ water bath for 8h to prepare a colored hard-ball emulsion.

[0022] (2) Preparation of micro-nano fluorosilicone polymer coated colored hard ball emulsion: The colored hard ball seed emulsion is added into a reactor, and the organic fluorosilicone monomer, soft monomer, 1wt% to 3wt% of the monomer initiator and cross-linking agent are used as the oil phase; water, 3wt% to 5wt% of the emulsifier and the cationic ring-opener are used as the aqueous phase. The oil phase is poured into the aqueous phase and emulsified for 20 minutes. After pre-emulsification, the emulsion is placed in an ice water bath and ultrasonicated for 20 minutes, and then injected into the reactor and reacted at 75°C for 8 hours to prepare the micro-nano fluorosilicone polymer coated colored hard ball emulsion.

[0023] (3) Regulation of micro-nano fluorosilicone polymer coated colored hard ball ink: Add 3wt%-5wt% of moisturizing agent, 0.05wt%-1wt% of surfactant, and Ph regulator (adjusted to 7-9) to the fluorosilicone polymer coated colored hard ball emulsion (balance) to prepare micro-nano fluorosilicone polymer coated colored hard ball ink (total mass percentage 100%).

[0024] The present invention provides a micro-nano fluorosilicone polymer coated color hard ball ink for digital inkjet printing, which has the following five main advantages:

[0025] (1) The present invention uses a highly soluble reactive anthraquinone dye, which has a high solubility in styrene monomers, so that the colored hard ball emulsion prepared by polymerization reaction has a higher color depth, thus solving the key problem of low content and light coloring of traditional colored hard ball dyes.

[0026] (2) The prepared reactive anthraquinone dye has an active carbon-carbon double bond and can copolymerize with styrene monomer to form a strong chemical bond, which greatly improves the color fastness of hard ball ink. With the help of the adhesion effect of the low glass transition temperature of acrylic soft monomer, it can be directly attached to the surface of the fabric without the need for additional dyes and film-forming agents. The process is simple and meets the market demand for safety and environmental protection.

[0027] (3) The micro-nano-grade fluorosilicone polymer-coated colored hard ball ink prepared by the present invention has a regular spherical shape and is evenly dispersed, without any extremely large particles, which has little effect on the morphology of the ink droplets and effectively solves the problem of easy clogging of the nozzle.

[0028] (4) The present invention uses organic fluorine silicon monomers and acrylic ester soft monomers as shell monomers to cover styrene colored hard balls. The introduction of organic fluorine silicon chain segments gives the inkjet printed fabric excellent hydrophobicity, softness and color fastness.

[0029] (5) The present invention uses octadecyl alcohol polyoxyethylene ether as a moisturizer. Compared with alcohol moisturizers, a smaller amount can make the ink obtain excellent moisturizing properties, relatively increase the content of fluorosilicone-coated colored hard balls, and further improve the wearability of inkjet printed fabrics.

[0030] The preparation method and application of micro-nano-grade fluorosilicone polymer-coated colored hard ball ink for digital inkjet printing meet the development needs of the times for textiles. The preparation process is wastewater-free, does not require chemical colorants, is green and pollution-free, and has huge development potential and broad market prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the NMR characterization and infrared spectrum of the highly soluble reactive anthraquinone dye;

[0032] Figure 2It is the reaction flow chart of styrene seed colored hard ball emulsion and fluorosilicone shell emulsion;

[0033] Figure 3 TEM transmission electron microscope images of styrene seed colored hard sphere emulsion and fluorosilicone shell emulsion;

[0034] Figure 4 Print hydrophobic images on fabrics using micro-nano-scale fluorosilicone polymer-coated colored hard ball ink. DETAILED DESCRIPTION

[0035] The following description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

[0036] The dye preparation method used in this application is as follows:

[0037] Preparation of highly soluble reactive anthraquinone dye: Weigh 0.52g HEMA, 10g anhydrous sodium carbonate, and 200ml toluene into a three-necked round-bottom flask equipped with an overhead stirrer, nitrogen inlet and outlet lines, and a thermometer. The solution was cooled to nearly 0°C under a nitrogen atmosphere. At a temperature of 0-5°C, 1.48g of cyanuric chloride was added and stirred for 48h. Then 2.64g CI Disperse Red 60 was added, stirred at 40-50°C for 48h, then the temperature was raised to 100°C, 0.753g of phenol was weighed and added to continue the reaction for 8h, and after cooling to room temperature, it was filtered with a sand core funnel, and the filtrate was evaporated to obtain a red solid, which was purified by column chromatography, and the developing solvent was ethyl acetate: dichloromethane = 2:1 (v / v), and a highly soluble reactive anthraquinone dye was purified (the structural characterization is shown in the attached figure Figure 1 shown).

[0038] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with specific implementation methods and drawings.

[0039] Example 1

[0040] (1) Preparation of colored hard ball seed emulsion: 1.08g (9wt%) of the total monomers of highly soluble reactive anthraquinone dye and 0.2616g (1wt%) of azobisisobutyronitrile were dissolved in 12g of styrene to form an oil phase, 0.36g of sodium dodecyl sulfonate was dissolved in 68g of deionized water (15wt%) to form an aqueous phase, and the oil phase was poured into the aqueous phase for pre-emulsification for 20min (power was 650W) to form a coarse emulsion. After pre-emulsification, the emulsion was placed in an ice water bath and ultrasonicated for 20min. The obtained pre-emulsion was transferred to a three-necked round-bottom flask equipped with a condenser and a mechanical stirrer for reaction and N2 was introduced for 15min. Finally, the emulsion was reacted in a 70°C water bath for 8h to prepare a colored hard ball seed emulsion.

[0041] (2) Preparation of micro-nano fluorosilicone polymer-coated colored hard ball emulsion: 40.72 g of the above-mentioned colored hard ball seed emulsion was transferred to a reactor, with 4.8 g of octamethylcyclotetrasiloxane, 1.2 g of trifluoropropylmethylcyclotrisiloxane, 3 g of butyl acrylate, 0.18 g of azobisisobutyronitrile, and 0.18 g of vinyltrimethoxysilane as the oil phase; 34 g of water (15 wt%), 0.27 g of sodium dodecyl sulfate and 0.6 g of dodecylbenzenesulfonic acid as the aqueous phase. The oil phase was poured into the aqueous phase and emulsified for 20 min. After pre-emulsification, the emulsion was placed in an ice-water bath and ultrasonicated for 20 min (650 W) and then injected (10 ml / h) into the reactor and reacted at 75 °C for 8 h to prepare micro-nano fluorosilicone polymer-coated colored hard ball emulsion.

[0042] (3) Preparation of micro-nano fluorosilicone polymer coated colored hard ball ink: Based on the total mass percentage of colored hard ball ink as 100%, the micro-nano fluorosilicone polymer coated colored hard ball (balance) was added with 3 wt % of octadecyl alcohol polyoxyethylene ether (FDC, Guangzhou Yangsong Technology), 0.05 wt % of non-ionic defoaming wetting agent surfactant 104e (Evonik Base Material), and sodium carbonate Ph regulator (adjusted to 8), and the mixture was filtered through a PVDF membrane with a pore size of 1 um to prepare micro-nano fluorosilicone polymer coated colored hard ball ink for inkjet printing.

[0043] Example 2

[0044] (1) Preparation of colored hard ball seed emulsion: 1.08g (9wt%) of the total monomers of highly soluble reactive anthraquinone dye and 0.2616g (1wt%) of azobisisobutyronitrile were dissolved in 12g of styrene to form an oil phase, 0.36g of sodium dodecyl sulfonate was dissolved in 36g of deionized water (25wt%) to form an aqueous phase, and the oil phase was poured into the aqueous phase for pre-emulsification for 20min (power was 650W) to form a coarse emulsion. After pre-emulsification, the emulsion was placed in an ice water bath and ultrasonicated for 20min. The obtained pre-emulsion was transferred to a three-necked round-bottom flask equipped with a condenser and a mechanical stirrer for reaction and N2 was introduced for 15min. Finally, the emulsion was reacted in a 70°C water bath for 8h to prepare a colored hard ball seed emulsion.

[0045] (2) Preparation of micro-nano fluorosilicone polymer-coated colored hard ball emulsion: 24.72 g of the above-mentioned colored hard ball seed emulsion was transferred to a reactor, with 6 g of octamethylcyclotetrasiloxane, 0 g of trifluoropropylmethylcyclotrisiloxane, 3 g of butyl acrylate, 0.18 g of azobisisobutyronitrile, and 0.18 g of vinyltrimethoxysilane as the oil phase; 27 g of water (25 wt%), 0.27 g of sodium dodecyl sulfate and 0.6 g of dodecylbenzenesulfonic acid as the aqueous phase. The oil phase was poured into the aqueous phase and emulsified for 20 min. After pre-emulsification, the emulsion was placed in an ice water bath and ultrasonicated for 20 min (650 W) and then injected (10 ml / h) into the reactor and reacted at 75 °C for 8 h to prepare micro-nano fluorosilicone polymer-coated colored hard ball emulsion.

[0046] (3) Preparation of micro-nano fluorosilicone polymer coated colored hard ball ink: Based on the total mass percentage of colored hard ball ink as 100%, the micro-nano fluorosilicone polymer coated colored hard ball (balance) was added with 3 wt % of octadecyl alcohol polyoxyethylene ether (FDC, Guangzhou Yangsong Technology), 0.05 wt % of non-ionic defoaming wetting agent surfactant 104e (Evonik Base Material), and sodium carbonate Ph regulator (adjusted to 8), and the mixture was filtered through a PVDF membrane with a pore size of 1 um to prepare micro-nano fluorosilicone polymer coated colored hard ball ink for inkjet printing.

[0047] Example 3

[0048] (1) Preparation of colored hard ball seed emulsion: 1.08g (9wt%) of the total monomers of highly soluble reactive anthraquinone dye and 0.2616g (1wt%) of azobisisobutyronitrile were dissolved in 12g of styrene to form an oil phase, 0.36g of sodium dodecyl sulfonate was dissolved in 36g of deionized water (25wt%) to form an aqueous phase, and the oil phase was poured into the aqueous phase for pre-emulsification for 20min (power was 650W) to form a coarse emulsion. After pre-emulsification, the emulsion was placed in an ice water bath and ultrasonicated for 20min. The obtained pre-emulsion was transferred to a three-necked round-bottom flask equipped with a condenser and a mechanical stirrer for reaction and N2 was introduced for 15min. Finally, the emulsion was reacted in a 70°C water bath for 8h to prepare a colored hard ball seed emulsion.

[0049] (2) Preparation of micro-nano fluorosilicone polymer coated colored hard ball emulsion: 24.72 g of the above colored hard ball seed emulsion was transferred to a reactor, with 4.8 g of octamethylcyclotetrasiloxane, 1.2 g of trifluoropropylmethylcyclotrisiloxane, 3 g of butyl acrylate, 0.18 g of azobisisobutyronitrile, and 0.18 g of vinyltrimethoxysilane as the oil phase; 27 g of water (25 wt%), 0.27 g of sodium dodecyl sulfate and 0.6 g of dodecylbenzenesulfonic acid as the aqueous phase. The oil phase was poured into the aqueous phase and emulsified for 20 min. After pre-emulsification, the emulsion was placed in an ice water bath and ultrasonicated for 20 min (650 W) and then injected (10 ml / h) into the reactor and reacted at 75 °C for 8 h to prepare micro-nano fluorosilicone polymer coated colored hard ball emulsion.

[0050] (3) Preparation of micro-nano fluorosilicone polymer coated colored hard ball ink: Based on the total mass percentage of colored hard ball ink as 100%, the micro-nano fluorosilicone polymer coated colored hard ball (balance) was added with 3 wt % of octadecyl alcohol polyoxyethylene ether (FDC, Guangzhou Yangsong Technology), 0.05 wt % of non-ionic defoaming wetting agent surfactant 104e (Evonik Base Material), and sodium carbonate Ph regulator (adjusted to 8), and the mixture was filtered through a PVDF membrane with a pore size of 1 um to prepare micro-nano fluorosilicone polymer coated colored hard ball ink for inkjet printing.

[0051] Example 4

[0052] (1) Preparation of colored hard ball seed emulsion: 1.08g (9wt%) of the total monomers of highly soluble reactive anthraquinone dye and 0.2616g (1wt%) of azobisisobutyronitrile were dissolved in 12g of styrene to form an oil phase, 0.36g of sodium dodecyl sulfonate was dissolved in 36g of deionized water (25wt%) to form an aqueous phase, and the oil phase was poured into the aqueous phase for pre-emulsification for 20min (power was 650W) to form a coarse emulsion. After pre-emulsification, the emulsion was placed in an ice water bath and ultrasonicated for 20min. The obtained pre-emulsion was transferred to a three-necked round-bottom flask equipped with a condenser and a mechanical stirrer for reaction and N2 was introduced for 15min. Finally, the emulsion was reacted in a 70°C water bath for 8h to prepare a colored hard ball seed emulsion.

[0053] (2) Preparation of micro-nano fluorosilicone polymer-coated colored hard ball emulsion: 24.72 g of the above-mentioned colored hard ball seed emulsion was transferred to a reactor, with 3 g of octamethylcyclotetrasiloxane, 3 g of trifluoropropylmethylcyclotrisiloxane, 3 g of butyl acrylate, 0.18 g of azobisisobutyronitrile, and 0.18 g of vinyltrimethoxysilane as the oil phase; 27 g of water (25 wt%), 0.27 g of sodium dodecyl sulfate and 0.6 g of dodecylbenzenesulfonic acid as the aqueous phase. The oil phase was poured into the aqueous phase and emulsified for 20 min. After pre-emulsification, the emulsion was placed in an ice-water bath and ultrasonicated for 20 min (650 W) and then injected (10 ml / h) into the reactor and reacted at 75 °C for 8 h to prepare micro-nano fluorosilicone polymer-coated colored hard ball emulsion.

[0054] (3) Preparation of micro-nano fluorosilicone polymer coated colored hard ball ink: Based on the total mass percentage of colored hard ball ink as 100%, the micro-nano fluorosilicone polymer coated colored hard ball (balance) was added with 3 wt % of octadecyl alcohol polyoxyethylene ether (FDC, Guangzhou Yangsong Technology), 0.05 wt % of non-ionic defoaming wetting agent surfactant 104e (Evonik Base Material), and sodium carbonate Ph regulator (adjusted to 8), and the mixture was filtered through a PVDF membrane with a pore size of 1 um to prepare micro-nano fluorosilicone polymer coated colored hard ball ink for inkjet printing.

[0055] Example 5

[0056] (1) Preparation of colored hard ball seed emulsion: 1.08g (9wt%) of the total monomers of highly soluble reactive anthraquinone dye and 0.2616g (1wt%) of azobisisobutyronitrile were dissolved in 12g of styrene to form an oil phase, 0.36g of sodium dodecyl sulfonate was dissolved in 36g of deionized water (25wt%) to form an aqueous phase, and the oil phase was poured into the aqueous phase for pre-emulsification for 20min (power was 650W) to form a coarse emulsion. After pre-emulsification, the emulsion was placed in an ice water bath and ultrasonicated for 20min. The obtained pre-emulsion was transferred to a three-necked round-bottom flask equipped with a condenser and a mechanical stirrer for reaction and N2 was introduced for 15min. Finally, the emulsion was reacted in a 70°C water bath for 8h to prepare a colored hard ball seed emulsion.

[0057] (2) Preparation of micro-nano fluorosilicone polymer-coated colored hard ball emulsion: 24.72 g of the above-mentioned colored hard ball seed emulsion was transferred to a reactor, with 0 g octamethylcyclotetrasiloxane, 6 g trifluoropropylmethylcyclotrisiloxane, 3 g butyl acrylate, 0.18 g azobisisobutyronitrile, and 0.18 g vinyltrimethoxysilane as the oil phase; 27 g water (25 wt%), 0.27 g sodium dodecyl sulfate and 0.6 g dodecylbenzenesulfonic acid as the aqueous phase. The oil phase was poured into the aqueous phase and emulsified for 20 min. After pre-emulsification, the emulsion was placed in an ice water bath and ultrasonicated for 20 min (650 W) and then injected (10 ml / h) into the reactor and reacted at 75 °C for 8 h to prepare micro-nano fluorosilicone polymer-coated colored hard ball emulsion.

[0058] (3) Preparation of micro-nano fluorosilicone polymer coated colored hard ball ink: Based on the total mass percentage of colored hard ball ink as 100%, the micro-nano fluorosilicone polymer coated colored hard ball (balance) was added with 3 wt % of octadecyl alcohol polyoxyethylene ether (FDC, Guangzhou Yangsong Technology), 0.05 wt % of non-ionic defoaming wetting agent surfactant 104e (Evonik Base Material), and sodium carbonate Ph regulator (adjusted to 8), and the mixture was filtered through a PVDF membrane with a pore size of 1 um to prepare micro-nano fluorosilicone polymer coated colored hard ball ink for inkjet printing.

[0059] Comparative Example 1

[0060] (1) Preparation of colored hard ball seed emulsion: 0.36g (9wt%) of the total monomers, highly soluble reactive anthraquinone dye and 0.3924g of AIBN were dissolved in 12g of styrene to form the oil phase, 0.6g of sodium dodecyl sulfonate was dissolved in 36g (25wt%) of deionized water to form the water phase, the oil phase was poured into the water phase and pre-emulsified for 20min (power was 650W) to form a coarse emulsion. After pre-emulsification, the emulsion was placed in an ice water bath and ultrasonicated for 20min. The obtained pre-emulsion was transferred to a three-necked round-bottom flask equipped with a condenser and a mechanical stirrer for reaction and N2 was introduced for 15min. Finally, the emulsion was reacted in a 70°C water bath for 8h to prepare a colored hard ball emulsion.

[0061] (2) Regulation of color hard ball ink for digital inkjet printing: 3 wt % of octadecyl alcohol polyoxyethylene ether (FDC, Guangzhou Yangsong Technology), 0.05 wt % of non-ionic defoaming wetting agent surfactant 104e (Evonik Base Material), and sodium carbonate Ph regulator (adjusted to 8) were added to the color hard ball emulsion, and filtered through a PVDF membrane with a pore size of 1 μm to prepare micro-nano-grade fluorosilicone polymer-coated color hard ball ink for inkjet printing.

[0062] Comparative Example 1 is a fluorine-free silicone-coated color hard ball ink.

[0063] Table 2 shows the performance of different formulations of micro-nano fluorosilicone polymer coated color hard ball ink

[0064] Particle size (nm) PDI Potential (mv) Water contact angle of cotton fabric (°) Example 1 74.31 0.058 -45.7 90.1 Example 2 73.46 0.046 -67.4 100.5 Example 3 76.55 0.052 -68.5 110.6 Example 4 75.45 0.088 -66.5 124.5 Example 5 77.81 0.076 -70.6 138.3 Comparative Example 1 65.22 0.092 -48.7 65.2

[0065] As can be seen from Table 2, the particle size of the micro-nano fluorosilicone polymer-coated colored hard ball emulsion is less than 100 nm. The particle size distribution index is low, the absolute potential is high, and the stability is excellent.

[0066] Figure 1 The NMR and IR characterization of the highly soluble reactive anthraquinone dye proves that the dye has been successfully synthesized.

[0067] Figure 3 The styrene colored hard spheres prepared in Example 5 were characterized by transmission, and the results are shown in Table 1. The particle size of the micro-nano fluorosilicone polymer coated colored hard sphere emulsion is 77.81nm, the PDI is 0.076, and the particle size meets the requirements of inkjet printing (≤200nm). It can be seen from the transmission electron microscope photo that the prepared colored hard spheres are uniformly spherical and evenly distributed.

[0068] Figure 4 The inkjet printed cotton cloth prepared in Example 5 shows that the cloth sample printed with the micro-nano fluorosilicone polymer-coated colored hard ball ink has an excellent water contact angle.

[0069] The above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.

Claims

1. A method for preparing a digital inkjet ink of micro-nano fluorosilicone polymer-coated color hard balls, It is characterized in that The following steps are involved: (1) Using anthraquinone matrix as raw material, introducing polymerizable double bonds and solubilizing groups to synthesize a reactive anthraquinone dye consisting of anthraquinone matrix-linker-polymerizable group-solubilizing group; (2) dissolving the reactive anthraquinone dye in styrene monomer, adding water, an emulsifier and an initiator, and preparing a colored hard ball seed emulsion by free radical polymerization; (3) The colored hard ball seed emulsion is transferred to a reactor, and the organic fluorosilicone monomer and the soft monomer are used as the shell layer. An initiator, a crosslinking agent, water, an emulsifier and a cationic ring-opening agent are added to the reactor to carry out free radical polymerization and cationic ring-opening miniemulsion polymerization to prepare a micro-nano-scale fluorosilicone polymer-coated colored hard ball emulsion; (4) A moisturizer, a pH regulator, and a surface tension regulator are added to the micro-nano fluorosilicone polymer coated color hard ball emulsion for regulation, and finally a micro-nano fluorosilicone polymer coated color hard ball digital inkjet ink is prepared.

2. The preparation method according to claim 1, It is characterized in that In step (2), the concentration of the colored hard ball seed emulsion is 15wt% to 30wt%; In step (3), the concentration of the micro-nano-grade fluorosilicone polymer-coated colored hard ball emulsion is 10wt% to 25wt%.

3. The preparation method according to claim 1, It is characterized in that In step (2), the emulsifier is one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate, and the amount used is 3wt% to 5wt% of the styrene monomer; In step (3), the emulsifier is one of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate, and the amount used is 3wt% to 5wt% of the total mass of the organic fluorine silicon monomer and the soft monomer.

4. The preparation method according to claim 1, It is characterized in that In step (2), the initiator is one or two of azobiscyanovaleric acid, azobisisobutylamidine hydrochloride, azobisisobutyronitrile, and potassium persulfate, and the amount of the initiator is 1% to 5% by mass of the styrene monomer and the reactive anthraquinone dye; In step (3), the initiator is one or two of azobiscyanovaleric acid, azobisisobutylamidine hydrochloride, azobisisobutyronitrile, and potassium persulfate, and the amount of the initiator is 1% to 3% of the total mass of the organic fluorine silicon monomer and the soft monomer.

5. The method for preparing core-shell color hard ball ink according to claim 1, It is characterized in that In step (3), the soft monomer is one or more of butyl acrylate, ethyl acrylate, and isooctyl acrylate.

6. The preparation method according to claim 1, It is characterized in that In step (3), the organic fluorine silicon monomer is one or more of octamethylcyclotetrasiloxane and trifluoropropylmethylcyclotrisiloxane, and the mass ratio is 1:0-0:1; The cationic ring-opener is dodecylbenzenesulfonic acid; The crosslinking agent is vinyl trimethoxy silane, one of vinyl trimethoxy silane.

7. The preparation method according to claim 1, It is characterized in that In step (3), the organic fluorine silicon monomer, soft monomer, initiator, crosslinking agent, water, emulsifier and cationic ring-opening agent are mixed and added to the reaction kettle by injection at 70-80° C. for reaction for 4-12 hours, and the injection speed is 10-30 ml / h.

8. The preparation method according to claim 1, It is characterized in that In step (4), the surface tension regulator is a nonionic defoaming wetting agent; The pH regulator is any one of sodium carbonate, sodium bicarbonate, sodium hydroxide and potassium carbonate; The moisturizing agent is stearyl alcohol polyoxyethylene ether.

9. The preparation method according to claim 1, It is characterized in that In step (4), the micro-nano fluorosilicone polymer coated color hard ball digital inkjet ink is made of the following raw materials in percentage by weight: Moisturizer 3wt%-5wt%; Surface tension regulator 0.05wt%-1wt%; The residual amount of the latex of colored hard balls coated with micro-nano fluorosilicone polymer; The pH value of the digital inkjet ink of micro-nano fluorosilicone polymer coated color hard ball is adjusted to 7-9 by using a pH regulator.

10. Use of digital inkjet ink of micro-nano fluorosilicone polymer coated color hard balls prepared by the preparation method according to any one of claims 1 to 9 in digital inkjet printing.

Citation Information

Cited By

  • Preparation method for and use of digital inkjet ink having micron / nano-sized fluoro-silicon polymer-coated colored hard spheres

    WO2026051343A1