Method for extracting and detecting plastic microbeads in cosmetics
Through sample pretreatment and microscopic infrared spectroscopy detection combined with laser Raman spectroscopy detection, the problems of low detection efficiency and false negative results in the existing technology are solved, and efficient and accurate detection of plastic microbeads in cosmetics is achieved.
Patent Information
- Application Number
- CN202411002098.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-01
AI Technical Summary
Existing detection methods for plastic microbeads in cosmetics cannot effectively detect smaller secondary plastic microbeads and plastic microbeads in complex matrices, and suffer from low detection rates and false negative results.
Using sample pretreatment method selection and microscopic infrared spectroscopy detection combined with laser Raman spectroscopy detection, matrix interference is removed through silver film interception and dispersion purification steps to improve detection efficiency and sensitivity.
It improves the detection efficiency and accuracy of plastic microbeads in cosmetics, can effectively detect smaller plastic microbeads and plastic microbeads in complex matrices, and reduces false negative results.
Smart Images

Figure CN118730684A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of cosmetics, and in particular to a method for extracting and detecting plastic microbeads in cosmetics. Background Art
[0002] Plastic microbeads or microplastics can be expressed in English as microplastics, plastic microbeads. Science magazine defines microplastics as plastic particles, fragments or fibers smaller than 5 mm. The United Nations Environment Programme pointed out that plastic microbeads in cosmetics have the following characteristics: solid matter, particle size less than 5 mm, insoluble in water, difficult to degrade, and composed of plastic. Daily chemical products containing plastic microbeads refer to "rinse-off cosmetics (such as shower gels, facial cleansers, scrubs, shampoos, etc.) and toothpastes and tooth powders that intentionally add solid plastic particles with a particle size of less than 5 mm for the purpose of scrubbing, exfoliating, and cleaning." Depending on the source, plastic microbeads in cosmetics can be divided into primary and secondary. Primary plastic microbeads are tiny plastic particles directly generated in the production process, such as particles in body scrubs that have a scrubbing and cleaning effect or are used as fillers in products. Secondary plastic microbeads are particles formed when large pieces of plastic are worn, decomposed, and broken over time in the environment.
[0003] Plastic microbeads pose a serious threat to the environment and are the main source of plastic pollution in the ocean and other water bodies. The harm to human health has also attracted great attention in the industry. Due to the small size and non-degradable nature of plastic microbeads, they will enter the ocean and water circulation system with domestic wastewater, accumulate in marine organisms such as fish, and then enter the human body through the food chain. Microplastics can be retained in human organs such as the lungs and liver, causing organ damage. At the same time, the plasticizers and bisphenol A they carry can cause endocrine disruption, reproductive development and other risks. Currently, the global "plastic ban" is being gradually implemented.
[0004] The testing standard GB / T 40146-2021 "Determination of Plastic Microbeads in Cosmetics" issued and implemented in 2021 uses Fourier infrared and microscopic infrared to determine plastic microbeads in cosmetics, toothpaste, soap, and laundry detergent, but this method has the following two defects: 1) It is not suitable for the detection of smaller plastic particles, such as secondary plastic microbeads smaller than 100μm. When this method is used for spectral testing, whether it is the potassium bromide tablet method, ATR method in the infrared method, or the direct test method and diamond pressure cell method in the microscopic infrared method, the plastic microbeads in the sample must be visible to the naked eye and have a high purity. However, in actual testing, no large-sized particles visible to the naked eye were found in the product. Therefore, it is difficult to collect solid particles for testing after the sample is pre-treated. 2) It is not suitable for complex matrix cosmetics such as sunscreen, toothpaste, and makeup. When complex matrix cosmetics are treated according to this method, the sample cannot be well dispersed in solutions such as water and ethanol, the interference of the complex matrix cannot be eliminated, and the sample pretreatment efficiency is low, which seriously interferes with subsequent infrared determination. 3) Infrared and micro-infrared tests on plastic microbeads wrapped in cosmetic matrices may result in false negative results.
[0005] Therefore, it is extremely necessary to establish sample processing and testing methods for cosmetics in order to monitor the risks of plastic microbeads in cosmetics and provide support for protecting the cosmetic environment and human health. Summary of the invention
[0006] The purpose of the present invention is to provide a method for extracting and detecting plastic microbeads in cosmetics.
[0007] The first aspect of the present invention provides a method for detecting plastic microbeads in cosmetics, comprising the steps of:
[0008] Step 1: Selection of sample pretreatment method:
[0009] Disperse the cosmetic sample to be tested with water and observe the dispersion state of the sample in water:
[0010] If the sample is completely dispersed, pre-treat according to Scheme A in step 2;
[0011] If floccules precipitate out after the sample is dispersed in water, perform pretreatment according to Scheme B in Step 2;
[0012] If a large amount of foam is produced after the sample is dispersed in water, add isopropanol to defoam and perform pretreatment according to Scheme C in Step 2;
[0013] If the sample does not disperse in water, pretreat according to Scheme D in Step 2;
[0014] Step 2: Sample pretreatment:
[0015] Solution A: Weigh the sample, add water to disperse it, add potassium ferrocyanide solution and zinc acetate solution, vortex disperse it and centrifuge it, take the supernatant, heat it to 50-80℃ and maintain it for 5-20min, filter the supernatant with a silver film and dry it to obtain a silver film covered with the sample;
[0016] Solution B: Weigh the sample, add saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add the first portion of ethanol aqueous solution and hydrochloric acid, fully vortex disperse the sample, add the second portion of ethanol aqueous solution, heat to 50-80°C and maintain for 5-20 minutes, centrifuge and take the supernatant, filter the supernatant with a silver film and dry it to obtain a silver film covered with the sample;
[0017] Scheme C: Weigh the sample and add saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add the first portion of anhydrous ethanol and hydrochloric acid, vortex disperse the sample thoroughly, add the second portion of anhydrous ethanol, heat to 50-80°C and maintain for 5-20 minutes, filter the solution with a silver film and dry it to obtain a silver film covered with the sample;
[0018] Solution D: Weigh the sample and add the first portion of n-hexane, vortex to disperse the sample, then add the second portion of n-hexane, stir evenly, heat to 50-80°C and maintain for 5-20 minutes, filter the solution with a silver membrane, rinse the container with n-hexane, filter the rinse solution with the same silver membrane, and then dry to obtain a silver membrane covered with the sample.
[0019] In another preferred embodiment, the method further comprises:
[0020] Step 3: Microscopic infrared spectrum detection:
[0021] The silver film covered with the sample is detected by infrared spectroscopy, an infrared spectrum of the sample is collected, and the infrared spectrum is compared with a standard spectrum to identify the type of plastic microbeads in the sample.
[0022] In another preferred embodiment, the method further comprises:
[0023] Step 4: Laser Raman spectroscopy detection:
[0024] Laser Raman spectroscopy is used to detect the silver film covered with the sample, a Raman spectrum of the sample is collected, and the Raman spectrum is compared with a standard spectrum to identify the type of plastic microbeads in the sample.
[0025] In another preferred embodiment, the method further comprises:
[0026] Step 5: Result determination:
[0027] Use a computer to compare the infrared spectrum of the sample and the standard infrared spectrum. When the matching score is greater than 90 points, compare the infrared spectrum of the sample with the standard infrared spectrum. If the characteristic peaks of the infrared spectrum of the sample and the standard infrared spectrum are consistent, it is judged as positive;
[0028] When the matching score is 80 to 90 points, the infrared spectrum of the sample is compared with the standard infrared spectrum. If the characteristic peaks of the infrared spectrum of the sample and the standard infrared spectrum are significantly different, it is determined to be negative; if the characteristic peaks of the infrared spectrum of the sample and the standard infrared spectrum are similar but not completely consistent, it is determined to be a suspicious sample and further confirmed by laser Raman spectroscopy; preferably, a computer is used to compare the Raman spectrum of the sample and the standard Raman spectrum. If the laser Raman spectrum matching score is greater than 90 points and the characteristic peaks of the Raman spectrum of the sample are consistent with those of the standard Raman spectrum, it is determined to be positive.
[0029] In another preferred embodiment, in step 1, weigh 5 g of sample, add 5 mL of water and stir evenly, heat the water (preferably 60° C. hot water) to 100 mL and stir continuously with a glass rod, and observe the dispersion state of the sample in water.
[0030] In another preferred embodiment, scheme A is as follows: weigh 0.2 g of sample and add 1 mL of water, vortex disperse the sample, add 9 mL of water, and stir evenly; add 50 μL of potassium ferrocyanide solution and zinc acetate solution, vortex disperse and centrifuge, take the supernatant, heat in a 60°C water bath for 10 min, filter the supernatant with a silver film, dry in an oven at 60°C, place in a dryer and let it reach room temperature to obtain a silver film covered with the sample to be tested.
[0031] In another preferred embodiment, Scheme B is as follows: weigh 0.2 g of sample, add 2 mL of saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add 2 mL of ethanol aqueous solution and 0.6 mL of hydrochloric acid, fully vortex disperse the sample, add ethanol aqueous solution to 10 mL, heat in a 60°C water bath for 10 min, centrifuge at 4000 rpm, take the supernatant, filter the supernatant with a silver film, dry in an oven at 60°C, place in a desiccator and let it reach room temperature to obtain a silver film covered with the sample to be tested.
[0032] In another preferred embodiment, Scheme C is as follows: weigh 0.2 g of sample, add 2 mL of saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add 2 mL of anhydrous ethanol and 0.6 mL of hydrochloric acid, fully vortex disperse the sample, add anhydrous ethanol to 10 mL, heat in a 60°C water bath for 10 min, filter the solution with a silver film, dry in a 60°C oven, place in a desiccator and let it reach room temperature to obtain a silver film covered with the sample to be tested.
[0033] In another preferred embodiment, Scheme D is as follows: weigh 0.2 g of sample and add 1 mL of n-hexane, vortex disperse the sample, add 9 mL of n-hexane, stir evenly, heat in a 60° C. water bath for 10 min, and filter the solution with a silver film; rinse the glass centrifuge tube with 5 mL of n-hexane, filter the solution with the same silver film, dry it in an oven at 60° C., place it in a dryer and let it reach room temperature to obtain a silver film covered with the sample to be tested.
[0034] In another preferred embodiment, the steps of microscopic infrared spectrum detection in step 3 are as follows:
[0035] Place the prepared silver film covered with the sample on the microscope infrared sample stage, focus on the sample surface, determine the scanning area and scanning parameters, and collect the infrared spectrum of the sample; after obtaining the infrared spectrum, use software to compare and analyze the obtained infrared spectrum with the standard infrared spectrum in the spectrum library.
[0036] In another preferred embodiment, the steps of laser Raman spectroscopy detection in step 4 are as follows:
[0037] Place the prepared silver film covered with the sample on the laser Raman sample stage, inspect the suspicious solid particles through the objective lens, focus on the surface of the particles and collect the Raman spectrum of the sample; compare the Raman spectrum of the sample with the standard Raman spectrum to identify the type of plastic microbeads in the sample.
[0038] In another preferred embodiment, in step 2, the potassium ferrocyanide solution is an aqueous solution with a mass fraction of 5-15%; the zinc acetate solution is an aqueous solution with a mass fraction of 10-30%; and the ethanol aqueous solution is a solution with a volume fraction of 40-60%.
[0039] In another preferred embodiment, the silver film used in step 2 is circular, and the pore size is less than 0.45 μm.
[0040] In another preferred embodiment, in step three, the infrared spectrum acquisition mode is the reflection mode; the objective lens is 100 times; the resolution is 8; and the number of scans is 1.
[0041] In another preferred embodiment, in step three, the scanning area is selected to be 10000 μm×10000 μm or 20000 μm×20000 μm according to the area of the silver film.
[0042] In another preferred embodiment, in step 4, the laser light source wavelength of laser Raman spectroscopy detection is 523 nm, the laser power is 5 mW, the grating aperture is 50 μm, and the exposure time is 0.04 s.
[0043] In another preferred embodiment, in step five, the standard spectrum library includes standard spectra of polyethylene (PE), polypropylene (PP), polystyrene (PS), nylon (PA), polycarbonate (PC), polymethyl methacrylate (PMMA), polytetrafluoroethylene (PTFE), polyvinyl chloride (PVC), and polylactic acid (PLA).
[0044] It should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described below (such as embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The infrared spectrum and matching results of polymethyl methacrylate (PMMA) particles in the sample.
[0046] Figure 2 This is the Raman spectrum and matching results of polymethyl methacrylate (PMMA) particles in the sample.
[0047] Figure 3 The infrared spectrum and matching results of polyethylene (PE) particles in the sample.
[0048] Figure 4 The Raman spectrum and matching results of polyethylene (PE) particles in the sample. DETAILED DESCRIPTION
[0049] The inventors found in their research that the existing methods for determining plastic microbeads in cosmetics have problems such as low detection rate, low method efficiency, and false negative results. For this reason, the present invention uses coprecipitation, saturated sodium chloride flotation, hydrochloric acid micro-digestion, n-hexane dispersion purification and other steps to remove matrix interference; silver film can be used to intercept plastic microbeads of smaller size, and the silver film can be directly placed on a microscopic infrared instrument to observe the particles. Compared with the existing methods, the operation is simple, the filtration time is short, and the work efficiency is greatly improved. The silver film can be directly observed, reducing the loss caused by steps such as transfer, and the method has a higher sensitivity. The present invention was completed on this basis.
[0050] Before describing the present invention, it should be understood that the present invention is not limited to the specific methods and experimental conditions described, because such methods and conditions can be changed. It should also be understood that the terminology used herein is intended only to describe specific embodiments, and is not intended to be restrictive, and the scope of the present invention will be limited only by the appended claims.
[0051] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. As used herein, the term "about" when used in reference to a specific recited value means that the value may vary by no more than 1% from the recited value. For example, as used herein, the expression "about 100" includes 99 and 101 and all values therebetween (e.g., 99.1, 99.2, 99.3, 99.4, etc.).
[0052] Although any methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, the preferred methods and materials are now described.
[0053] The present invention provides a method for extracting and detecting plastic microbeads in cosmetics, which specifically comprises the following steps:
[0054] Step 1: Sample pretreatment method selection:
[0055] Weigh 5g of sample into a 250mL beaker, add 5mL of water, heat the water to 100mL and stir continuously with a glass rod, and observe the dispersion state of the sample in the water. If the sample is completely dispersed, treat it according to Scheme A in Step 2; if floccules are precipitated when dispersed in water, treat it according to Scheme B in Step 2; if a large amount of foam is generated when dispersed in water, add a small amount of isopropanol to defoam and treat it according to Scheme C in Step 2; if it does not disperse in water, treat it according to Scheme D in Step 2.
[0056] Step 2: Sample pretreatment method:
[0057] Solution A: Weigh 0.2g of sample into a 10mL round-bottom glass centrifuge tube, add 1mL of water, vortex to disperse the sample, then add 9mL of water and stir evenly. Add 50μL each of potassium ferrocyanide solution and zinc acetate solution, vortex to disperse and centrifuge, take the supernatant, heat in a 60℃ water bath for 10min, filter the supernatant with a silver membrane, dry in a 60℃ oven, place in a desiccator to room temperature, and wait for testing.
[0058] Solution B: Weigh 0.2 g of sample into a 10 mL round-bottom glass centrifuge tube, add 2 mL of saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add 2 mL of ethanol aqueous solution and 0.6 mL of hydrochloric acid, vortex disperse the sample thoroughly, add ethanol aqueous solution to 10 mL, heat in a 60 ° C water bath for 10 min, centrifuge at 4000 rpm, take the supernatant, filter the supernatant with a silver membrane, dry in a 60 ° C oven, place in a desiccator and let it reach room temperature for testing.
[0059] Scheme C: Weigh 0.2 g of sample into a 10 mL round-bottom glass centrifuge tube, add 2 mL of saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add 2 mL of anhydrous ethanol and 0.6 mL of hydrochloric acid, vortex disperse the sample thoroughly, add anhydrous ethanol to 10 mL, heat in a 60 ° C water bath for 10 min, filter the solution with a silver membrane, dry in a 60 ° C oven, place in a desiccator and let it reach room temperature for testing.
[0060] Solution D: Weigh 0.2g of sample into a 10mL round-bottom glass centrifuge tube, add 1mL of n-hexane, vortex to disperse the sample, add 9mL of n-hexane, stir evenly, heat in a 60℃ water bath for 10min, and filter the solution with a silver membrane. Rinse the glass centrifuge tube with 5mL of n-hexane, filter the solution with the same silver membrane, dry it in a 60℃ oven, place it in a desiccator and let it reach room temperature before testing.
[0061] Step 3: Microscopic infrared spectrum test:
[0062] Place the prepared silver film covered with the sample on the microscope infrared sample stage, focus on the sample surface, determine the scanning area and scanning parameters, and then collect the infrared spectrum of the sample. After obtaining the particle spectrum, the software will automatically perform qualitative analysis with the standard spectrum in the spectrum library.
[0063] Step 4: Laser Raman spectroscopy test:
[0064] Place the prepared silver film covered with the sample on the laser Raman sample stage, examine the suspicious solid particles through the objective lens, and collect the Raman spectrum of the particles after focusing on the surface of the particles. Compare the Raman spectrum of the sample with the Raman spectrum of the plastic microbeads to identify the type of plastic microbeads in the sample.
[0065] Step 5: Result determination:
[0066] When the system's automatic matching score is higher than 90 points, the particle infrared spectrum is compared with the standard spectrum. If the characteristic peaks of the particle spectrum and the standard spectrum are consistent, it is judged as positive. When the system score is between 80-90 points, the particle infrared spectrum is compared with the standard spectrum. If the characteristic peaks of the sample spectrum and the standard spectrum are greatly different, it is judged as negative; if the characteristic peaks of the sample spectrum and the standard spectrum are similar but not completely consistent, it is judged as a suspicious sample and further confirmed by laser Raman spectroscopy. If the laser Raman spectrum matching score is higher than 90 and the particle spectrum is consistent with the characteristic peaks of the standard spectrum, it is judged as positive.
[0067] Furthermore, in step 1, the temperature of the hot water is 60°C.
[0068] Furthermore, in step 2, the potassium ferrocyanide solution is a 10% aqueous solution; the zinc acetate solution is a 20% aqueous solution; and the ethanol aqueous solution is a 50% aqueous solution.
[0069] Furthermore, in step 2, the centrifugal speed is 4000 rpm.
[0070] Furthermore, in step 2, the silver film is circular and has a pore size of 0.45 μm.
[0071] Furthermore, in step three, the acquisition mode is a reflection mode; the objective lens is 100 times; the resolution is 8; and the number of scans is 1.
[0072] Furthermore, in step three, the scanning area can be selected to be 10000 μm×10000 μm or 20000 μm×20000 μm according to the area of the silver film.
[0073] Furthermore, in step 4, the wavelength of the laser light source is 523 nm, the laser power is 5 mW, the grating aperture is 50 μm, and the exposure time is 0.04 s.
[0074] Further, in step 5, the plastic particles in the library are polyethylene (PE), polypropylene (PP), polystyrene (PS), nylon (PA), polycarbonate (PC), polymethyl methacrylate (PMMA), polytetrafluoroethylene (PTFE), polyvinyl chloride (PVC), polylactic acid (PLA)
[0075] The main advantages of the present invention are:
[0076] The present invention provides an extraction method and a detection method for plastic microbeads in cosmetics, which use coprecipitation, saturated sodium chloride flotation, hydrochloric acid microdigestion, n-hexane dispersion purification and other steps to remove matrix interference; a silver film can be used to intercept plastic microbeads of smaller size, and the silver film can be directly placed on a microscopic infrared instrument to observe the particles. Compared with the existing method, the operation is simple, the filtration time is short, and the work efficiency is greatly improved. The silver film can be directly observed, reducing the loss caused by the transfer and other steps. The method has high sensitivity and has broad application prospects and market potential.
[0077] The present invention will be further described in detail below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify detailed conditions are usually carried out under conventional conditions such as, or according to the conditions recommended by the manufacturer. Unless otherwise specified, percentages and parts are calculated by weight. The experimental materials and reagents used in the following examples can be obtained from commercial channels unless otherwise specified.
[0078] Test drugs and instruments:
[0079] Isopropanol and ethanol were of chromatographic grade and purchased from Merck, Germany; potassium ferrocyanide, zinc acetate, saturated sodium chloride, hydrochloric acid, n-hexane, and dichloromethane were of analytical grade and purchased from Sinopharm Chemical Reagent Co., Ltd.; water was high-purity water.
[0080] Silver membrane (silver metal filter membrane) was purchased from Merck Millipore, with a circular diameter of 25 mm, a thickness of 50 μm, and a pore size of 0.45 μm.
[0081] Thermo Scientific NICOLET iN10 Fourier transform infrared microscope (Thermo Corporation, USA); Thermo Scientific DXR3xi laser Raman spectrometer (Thermo Corporation, USA); electronic analytical balance (Beijing Sartorius Scientific Instrument Co., Ltd.); Vortex4 vortex oscillator (IKA, Germany); 5810R centrifuge (Eppendorf, Germany); Mil li-Q ultrapure water device (Mill iQ, USA).
[0082] Example 1
[0083] This embodiment provides a method for detecting plastic microbeads in sunscreen cosmetics, comprising the following steps:
[0084] Step 1: Selection of sample pretreatment method:
[0085] Weigh 5g of sample into a 250mL beaker, add 5mL of water, heat the water to 100mL and stir with a glass rod to observe the dispersion of the sample in the water. If the sample is completely dissolved in water, treat it according to Scheme A in Step 2.
[0086] Step 2: Sample pretreatment method:
[0087] Weigh 0.2g of sample into a 10mL round-bottom glass centrifuge tube, add 1mL of water, vortex to disperse the sample, then add 9mL of water and stir evenly. Add 50μL each of potassium ferrocyanide solution and zinc acetate solution, vortex to disperse and centrifuge, take the supernatant, heat in a 60℃ water bath for 10min, filter the supernatant with a silver membrane, dry in a 60℃ oven, place in a desiccator to room temperature, and wait for testing. Step 3: Microscopic infrared spectroscopy test:
[0088] Place the prepared silver film covered with the sample on the sample stage of the micro-infrared spectrometer, focus on the sample surface and collect the infrared spectrum of the sample. After obtaining the particle spectrum, the software will automatically perform qualitative analysis with the standard spectrum in the spectrum library.
[0089] Step 4: Laser Raman spectroscopy test:
[0090] Place the prepared silver film covered with the sample on the laser Raman sample stage, examine the suspicious solid particles through the objective lens, and collect the Raman spectrum of the particles after focusing on the surface of the particles. Compare the Raman spectrum of the sample with the Raman spectrum of the plastic microbeads to identify the type of plastic microbeads in the sample.
[0091] Step 5: Result determination:
[0092] The infrared spectrum of the particles to be tested in the sample is consistent with the characteristic peaks of the standard spectrum of polymethyl methacrylate, with a matching score of 94.42, and the result shows that polymethyl methacrylate is detected in the sample; laser Raman spectroscopy is further used for confirmation, and the Raman spectrum of the particles to be tested in the sample is consistent with the characteristic peaks of the standard spectrum of polymethyl methacrylate, with a matching score of 94.26, and the result shows that polymethyl methacrylate is detected in the sample. Comprehensively judged, polymethyl methacrylate plastic microbeads were detected in the sample.
[0093] Regarding the determination of the sample sampling amount, the sample weight was determined to be 0.2g-0.5g according to the area of the silver film. Sunscreen samples and toothpaste samples with relatively complex matrices were selected for the investigation of the sample weight.
[0094] Weigh 0.2g and 0.5g of sunscreen sample and toothpaste sample respectively. The sunscreen sample is treated by solution A in step 2, and the toothpaste sample is treated by solution B in step 2. The results are shown in the following table. According to the filtering situation, the final sample weight is 0.2g.
[0095] Table 1 Determination of sample weight
[0096]
[0097] Regarding the choice of sample purification method in Scheme A, the purification effects of potassium ferrocyanide-zinc sulfate precipitation reagent and petroleum ether were compared.
[0098] Three sunscreen products were selected for purification using the above two methods. Most impurities were precipitated after treatment with potassium ferrocyanide and zinc sulfate precipitation reagents. Although there were occasional suspended solids in the upper layer and the initial filtration speed was slow, the subsequent filtration speed was accelerated and the filtration could be completed quickly. After extraction with petroleum ether, the water layers of the three samples were all milky white, uniformly dispersed, opaque liquids that could not be filtered by the silver membrane. Finally, the precipitation reagent was selected to purify the samples.
[0099] Example 2
[0100] This embodiment provides a method for detecting plastic microbeads in color cosmetics, comprising the following steps:
[0101] Step 1: Sample pretreatment method selection:
[0102] Weigh 5g of sample into a 250mL beaker, add 5mL of water, heat the water to 100mL and stir with a glass rod to observe the dispersion of the sample in water. If the sample does not disperse in water, proceed with solution D in step 2.
[0103] Step 2: Sample pretreatment method:
[0104] Weigh 0.2g of sample into a 10mL round-bottom glass centrifuge tube, add 1mL of n-hexane, vortex to disperse the sample, add 9mL of n-hexane, stir evenly, heat in a 60℃ water bath for 10min, and filter the solution with a silver membrane. Rinse the glass centrifuge tube with 5mL of n-hexane, filter the solution with the same silver membrane, dry it in a 60℃ oven, place it in a desiccator and let it reach room temperature before testing.
[0105] Step 3: Microscopic infrared spectrum test:
[0106] Place the prepared silver film covered with the sample on the sample stage of the micro-infrared spectrometer, focus on the sample surface and collect the infrared spectrum of the sample. After obtaining the particle spectrum, the software will automatically perform qualitative analysis with the standard spectrum in the spectrum library.
[0107] Step 4: Laser Raman spectroscopy test:
[0108] Place the prepared silver film covered with the sample on the laser Raman sample stage, examine the suspicious solid particles through the objective lens, and collect the Raman spectrum of the particles after focusing on the surface of the particles. Compare the Raman spectrum of the sample with the Raman spectrum of the plastic microbeads to identify the type of plastic microbeads in the sample.
[0109] Step 5: Result determination:
[0110] The infrared spectrum of the particles to be tested in the sample is consistent with the characteristic peaks of the polyethylene (PE) standard spectrum, with a matching score of 94.14, and the result shows that polyethylene (PE) is detected in the sample; laser Raman spectroscopy is further used for confirmation, and the Raman spectrum of the particles to be tested in the sample is consistent with the characteristic peaks of the polyethylene (PE) standard spectrum, with a matching score of 94.67, and the result shows that polyethylene (PE) is detected in the sample. Comprehensively judged, polyethylene (PE) plastic microbeads were detected in the sample.
[0111] Regarding the selection of the dispersing solution in Scheme D, the extraction and purification effects of n-hexane and petroleum ether on the sample matrix were compared.
[0112] Three cosmetic products, lipstick, liquid foundation, and blush, were selected and extracted and dispersed using the above two solvents. The pretreatment method of adding petroleum ether was to first disperse the sample with water, then add a certain amount of petroleum ether and heat to help disperse the sample. After extraction, the water layer was filtered. The results are shown in the following table. After extraction with petroleum ether, part of the sample matrix co-precipitated with plastic microbeads in the lower solution, which may cause the loss of plastic particles due to incomplete absorption. Finally, n-hexane was selected as the solvent.
[0113] Table 2 Selection of solvents in Scheme D
[0114]
[0115] Example 3
[0116] This embodiment provides a method for detecting plastic microbeads in scrub cosmetics, comprising the following steps:
[0117] Step 1: Sample pretreatment method selection:
[0118] Weigh 5g of sample into a 250mL beaker, add 5mL of water, heat the water to 100mL and stir continuously with a glass rod to observe the dispersion state of the sample in water. The sample dispersed in water produces a lot of foam. After adding a small amount of isopropanol to defoam, treat it according to Scheme C in Step 2.
[0119] Step 2: Sample pretreatment method:
[0120] Weigh 0.2 g of sample into a 10 mL round-bottom glass centrifuge tube, add 2 mL of saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add 2 mL of anhydrous ethanol and 0.6 mL of hydrochloric acid, vortex disperse the sample thoroughly, add anhydrous ethanol to 10 mL, heat in a 60 ° C water bath for 10 min, filter the solution with a silver membrane, dry in a 60 ° C oven, place in a desiccator and let it reach room temperature for testing.
[0121] Step 3: Microscopic infrared spectrum test:
[0122] Place the prepared silver film covered with the sample on the sample stage of the micro-infrared spectrometer, focus on the sample surface and collect the infrared spectrum of the sample. After obtaining the particle spectrum, the software will automatically perform qualitative analysis with the standard spectrum in the spectrum library.
[0123] Step 4: Laser Raman spectroscopy test:
[0124] Place the prepared silver film covered with the sample on the laser Raman sample stage, examine the suspicious solid particles through the objective lens, and collect the Raman spectrum of the particles after focusing on the surface of the particles. Compare the Raman spectrum of the sample with the Raman spectrum of the plastic microbeads to identify the type of plastic microbeads in the sample.
[0125] Step 5: Result determination:
[0126] The infrared spectrum of the particles to be tested in the sample is similar to the characteristic peaks of the standard spectrum of polymethyl methacrylate (PMMA), with a matching score of 84.91, and it is determined to be a suspicious sample; laser Raman spectroscopy is further used for confirmation, and the Raman spectrum of the particles to be tested in the sample is consistent with the characteristic peaks of the standard spectrum of methyl methacrylate (PMMA), with a matching score of 92.45. The results show that methyl methacrylate (PMMA) is detected in the sample. Comprehensively judged, methyl methacrylate (PMMA) plastic microbeads were detected in the sample.
[0127] Comparative Example 1
[0128] This comparative example provides a method for extracting and detecting plastic microbeads in a toothpaste sample, the steps comprising:
[0129] Take a toothpaste sample, and judge the sample pretreatment type. Use solution B in step 2 for sample pretreatment. The results show that no plastic microbeads are detected in the sample. Take the sample and make a toothpaste sample with polyethylene plastic microbeads added, with the addition amount of 1%. Use solution B in step 2 for pretreatment and instrument detection.
[0130] Microscopic infrared spectroscopy results showed that polyethylene plastic microbeads were detected in the homemade samples. Laser Raman spectroscopy was used to confirm the results and polyethylene plastic microbeads were detected, which was consistent with the actual results.
[0131] The role of the saturated sodium chloride solution in Scheme B is to float the plastic microbeads based on the principle that the density of the plastic microbeads is lower than the density of the saturated sodium chloride solution.
[0132] Among them, regarding the investigation of the volume of hydrochloric acid in Scheme B, the role of hydrochloric acid is to micro-digest the sample matrix and reduce the influence of the matrix on filtration, instrumental measurement and other steps. Compare the digestion effects of hydrochloric acid volumes of 0.3mL, 0.6mL, and 1.5mL on the sample. When the volume of hydrochloric acid is 0.3mL, it cannot effectively digest the organic matter in the matrix, and the filtration speed is slow. During filtration, the filtrate drips in the form of droplets at a speed of about 0.5 drops / second, and can barely be filtered; when the volume of hydrochloric acid is 0.6mL and 1.5mL, it can be filtered quickly. Finally, the hydrochloric acid volume of 0.6mL was selected.
[0133] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as reference individually. In addition, it should be understood that after reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
Claims
1. A method for detecting plastic microbeads in cosmetics, characterized in that: Includes steps: Step 1: Selection of sample pretreatment method: Disperse the cosmetic sample to be tested with water and observe the dispersion state of the sample in water: If the sample is completely dispersed, pre-treat according to Scheme A in step 2; If floccules precipitate out after the sample is dispersed in water, perform pretreatment according to Scheme B in Step 2; If a large amount of foam is produced after the sample is dispersed in water, add a small amount of isopropanol to defoam and then perform pretreatment according to Scheme C in Step 2; If the sample does not disperse in water, pretreat according to Scheme D in Step 2; Step 2: Sample pretreatment: Solution A: Weigh the sample, add water to disperse it, add potassium ferrocyanide solution and zinc acetate solution, vortex disperse it and centrifuge it, take the supernatant, heat it to 50-80℃ and maintain it for 5-20min, filter the supernatant with a silver film and dry it to obtain a silver film covered with the sample; Solution B: Weigh the sample, add saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add the first portion of ethanol aqueous solution and hydrochloric acid, fully vortex disperse the sample, add the second portion of ethanol aqueous solution, heat to 50-80°C and maintain for 5-20 minutes, centrifuge and take the supernatant, filter the supernatant with a silver film and dry it to obtain a silver film covered with the sample; Scheme C: Weigh the sample and add saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add the first portion of anhydrous ethanol and hydrochloric acid, vortex disperse the sample thoroughly, add the second portion of anhydrous ethanol, heat to 50-80°C and maintain for 5-20 minutes, filter the solution with a silver film and dry it to obtain a silver film covered with the sample; Solution D: Weigh the sample and add the first portion of n-hexane, vortex to disperse the sample, then add the second portion of n-hexane, stir evenly, heat to 50-80°C and maintain for 5-20 minutes, filter the solution with a silver membrane, rinse the container with n-hexane, filter the rinse solution with the same silver membrane, and then dry to obtain a silver membrane covered with the sample.
2. The method according to claim 1, characterized in that The method further comprises: Step 3: Microscopic infrared spectrum detection: The silver film covered with the sample is detected by infrared spectroscopy, an infrared spectrum of the sample is collected, and the infrared spectrum is compared with a standard spectrum to identify the type of plastic microbeads in the sample.
3. The method according to claim 2, characterized in that The method further comprises: Step 4: Laser Raman spectroscopy detection: Laser Raman spectroscopy is used to detect the silver film covered with the sample, a Raman spectrum of the sample is collected, and the Raman spectrum is compared with a standard spectrum to identify the type of plastic microbeads in the sample.
4. The method according to claim 3, characterized in that The method further comprises: Step 5: Result determination: Use a computer to compare the infrared spectrum of the sample and the standard infrared spectrum. When the matching score is greater than 90 points, compare the infrared spectrum of the sample with the standard infrared spectrum. If the characteristic peaks of the infrared spectrum of the sample and the standard infrared spectrum are consistent, it is judged as positive; When the matching score is 80 to 90 points, the infrared spectrum of the sample is compared with the standard infrared spectrum. If the characteristic peaks of the infrared spectrum of the sample and the standard infrared spectrum are significantly different, it is determined to be negative; if the characteristic peaks of the infrared spectrum of the sample and the standard infrared spectrum are similar but not completely consistent, it is determined to be a suspicious sample and further confirmed by laser Raman spectroscopy; preferably, a computer is used to compare the Raman spectrum of the sample and the standard Raman spectrum. If the laser Raman spectrum matching score is greater than 90 points and the characteristic peaks of the Raman spectrum of the sample are consistent with those of the standard Raman spectrum, it is determined to be positive.
5. The method according to claim 1, characterized in that In step 1, weigh 5 g of sample, add 5 mL of water and stir evenly, heat the water (preferably 60° C. hot water) to 100 mL and stir continuously with a glass rod, and observe the dispersion state of the sample in water.
6. The method according to claim 1, characterized in that Scheme A in step 2 is as follows: weigh 0.2 g of sample and add 1 mL of water, vortex disperse the sample, add 9 mL of water, and stir evenly; add 50 μL of potassium ferrocyanide solution and zinc acetate solution, vortex disperse and centrifuge, take the supernatant, heat in a 60°C water bath for 10 min, filter the supernatant with a silver film, dry in a 60°C oven, place in a desiccator and let it reach room temperature to obtain a silver film covered with the sample to be tested.
7. The method according to claim 1, characterized in that Scheme B in step 2 is as follows: weigh 0.2 g of sample, add 2 mL of saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add 2 mL of ethanol aqueous solution and 0.6 mL of hydrochloric acid, fully vortex disperse the sample, add ethanol aqueous solution to 10 mL, heat in a 60°C water bath for 10 min, centrifuge at 4000 rpm, take the supernatant, filter the supernatant with a silver film, dry in a 60°C oven, place in a desiccator and let it reach room temperature to obtain a silver film covered with the sample to be tested.
8. The method according to claim 1, characterized in that Scheme C in step 2 is as follows: weigh 0.2 g of sample, add 2 mL of saturated sodium chloride solution, vortex disperse and centrifuge, take the supernatant, add 2 mL of anhydrous ethanol and 0.6 mL of hydrochloric acid, fully vortex disperse the sample, add anhydrous ethanol to 10 mL, heat in a 60°C water bath for 10 min, filter the solution with a silver film, dry in a 60°C oven, place in a desiccator and let it reach room temperature to obtain a silver film covered with the sample to be tested.
9. The method according to claim 1, characterized in that Scheme D in step 2 is as follows: weigh 0.2 g of sample and add 1 mL of n-hexane, vortex disperse the sample, add 9 mL of n-hexane, stir evenly, heat in a 60°C water bath for 10 min, and filter the solution with a silver film; rinse the glass centrifuge tube with 5 mL of n-hexane, filter the solution with the same silver film, dry it in an oven at 60°C, place it in a desiccator and let it reach room temperature to obtain a silver film covered with the sample to be tested.
10. The method according to claim 1, characterized in that The potassium ferrocyanide solution is an aqueous solution with a mass fraction of 5-15%; the zinc acetate solution is an aqueous solution with a mass fraction of 10-30%; and the ethanol aqueous solution is a solution with a volume fraction of 40-60%.