Method for measuring content of oxide in yttrium-containing glass microsphere and application of melting agent in measuring content of oxide in yttrium-containing glass microsphere

By using a mixture of anhydrous sodium carbonate and boric acid for high-temperature melting treatment and acidic aqueous solution dissolution, the problem of difficulty in digestion and inaccurate measurement of yttrium-containing glass microspheres was solved, and accurate measurement and efficient quality control of oxide content were achieved.

CN118731003APending Publication Date: 2024-10-01BEIJING SINOTAU INT PHARMA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410858111.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing methods are difficult to accurately measure the oxide content in yttrium-containing glass microspheres, especially due to the difficulty in digesting the glass microspheres and the volatilization of silicon fluoride gas, which results in inaccurate measurement.

Method used

A mixture of anhydrous sodium carbonate and boric acid is used as the melting agent, and the yttrium-containing glass microspheres are converted into melts through high-temperature melting treatment. After being dissolved in an acidic aqueous solution, the oxide content is determined by the inductively coupled plasma method.

Benefits of technology

The accurate measurement of yttrium-containing glass microspheres is achieved, the impact of the microsphere digestion process on the test results is reduced, and the measurement accuracy and repeatability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004918579400000071
    Figure BDA0004918579400000071
  • Figure BDA0004918579400000081
    Figure BDA0004918579400000081
  • Figure BDA0004918579400000082
    Figure BDA0004918579400000082
Patent Text Reader

Abstract

The invention discloses a method for measuring the content of oxides in yttrium-containing glass microspheres and application of a melting agent in measuring the content of the oxides in the yttrium-containing glass microspheres. The method comprises the following steps: mixing the yttrium-containing glass microspheres with the melting agent, and carrying out melting treatment to obtain a melt; dissolving the melt with an acidic aqueous solution to obtain a solution to be measured, and measuring to obtain the content of oxides; the melting agent is a mixture of anhydrous sodium carbonate and boric acid, the method can accurately and efficiently determine the content of the oxide in the yttrium-containing glass microspheres, the provided method can solve the problem that the yttrium-containing glass microspheres are difficult to digest, the influence of the microsphere digestion process on a test result is greatly reduced, and the accuracy of the method is improved.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the Chinese patent application with application number 202310495804.2, application date May 5, 2023, and invention name “Method for determining the oxide content in yttrium-containing glass microspheres, and use of flux in determining the oxide content in yttrium-containing glass microspheres”. Technical Field

[0002] The present application relates to the field of detection technology, and in particular to a method for determining the oxide content in yttrium-containing glass microspheres, and use of a flux in determining the oxide content in yttrium-containing glass microspheres. Background Art

[0003] Liver cancer is a highly malignant cancer. More than 60% of patients are diagnosed at an advanced stage and have lost the chance of surgical resection. 90 Y] Glass microsphere injection is a new non-surgical treatment method that uses glass microsphere embolization and local radiotherapy. Clinical applications have shown that it has broad prospects in the treatment of internal radiation liver segment / lobe resection, transitional / downgrade treatment before liver transplantation, liver cancer recurrence after liver resection, and palliative treatment of advanced liver cancer. 89 Y] glass microspheres are yttrium[ 90 Y] glass microspheres are made of a certain proportion of yttrium oxide, aluminum oxide and silicon oxide. The determination of the content of each oxide is a key parameter for its quality control. Therefore, it is important to establish an accurate and efficient method for determining the content of oxides. 90 Y] The quality control and administration safety of glass microsphere injection are crucial.

[0004] The current technology mainly measures the content of oxides by measuring the content of characteristic elements and then calculating the content of oxides. For the determination of element content, there are mainly technologies such as ICP-OES and X-ray fluorescence spectroscopy (XRF). Among them, the ICP-OES method has good repeatability and accuracy. Summary of the invention

[0005] The premise for accurately determining the content of each component of yttrium-containing glass microspheres is that the glass microspheres can be effectively digested without introducing interference or adversely affecting the determination. For general glass, the main component is silicon dioxide, which has a simple composition. The current dissolution methods are mainly sodium-alkali melting method and acid dissolution method, which are simple to operate, efficient and fast. The sodium-alkali melting method uses sodium hydroxide and sodium carbonate as flux, which are dissolved in an acidic aqueous solution after high-temperature melting to prepare a clear solution. However, experimental results show that yttrium-containing glass microspheres cannot be digested by this method, and the high concentration of alkali metals introduced by this method will also affect the detection results of ICP-OES. When using the acid dissolution method, hydrofluoric acid is necessary, but the silicon fluoride generated by the reaction of silicon dioxide and hydrofluoric acid is a gas. Because the volatilization of the gas will cause inaccurate determination of the silicon dioxide content, this method is also not available.

[0006] In order to solve the above technical problems, the present application provides a method for determining the oxide content in yttrium-containing glass microspheres and the use of a flux in determining the oxide content in yttrium-containing glass microspheres. The method can accurately determine the oxide content in yttrium-containing glass microspheres, and the method is simple and efficient to operate.

[0007] The specific technical solutions of this application are as follows:

[0008] 1. A method for determining the oxide content in yttrium-containing glass microspheres, comprising:

[0009] Mixing yttrium-containing glass microspheres with a flux and performing a melting process to obtain a melt;

[0010] The melt is dissolved in an acidic aqueous solution to obtain a test solution, and the content of the oxide is measured;

[0011] The flux is a mixture of anhydrous sodium carbonate and boric acid.

[0012] 2. The method according to item 1, wherein the mass ratio of the yttrium-containing glass microspheres to the flux is 1:(2-12), preferably 1:(4-10).

[0013] 3. The method according to item 1 or 2, wherein the mass ratio of anhydrous sodium carbonate to boric acid is 1:(0.1-0.5), preferably 1:(0.2-0.5).

[0014] 4. The method according to any one of items 1 to 3, wherein the temperature during the melt treatment is 700-1000° C., preferably 800-950° C.;

[0015] Preferably, the melting treatment time is 30-120 min.

[0016] 5. The method according to any one of items 1 to 4, wherein the acidic aqueous solution is an aqueous solution of an inorganic acid, preferably an aqueous solution of nitric acid;

[0017] Preferably, the concentration of the nitric acid aqueous solution is 0.1-5M.

[0018] 6. The method according to any one of items 1 to 5, wherein the determination is performed using an inductively coupled plasma method.

[0019] 7. A method according to any one of items 1 to 6, wherein the oxide comprises yttrium oxide, aluminum oxide and silicon oxide.

[0020] 8. Use of a flux in determining the oxide content in yttrium-containing glass microspheres, wherein the flux is a mixture of anhydrous sodium carbonate and boric acid.

[0021] 9. The use according to item 8, wherein the mass ratio of anhydrous sodium carbonate to boric acid is 1:(0.1-0.5), preferably 1:(0.2-0.5).

[0022] 10. The use according to item 8 or 9, wherein the mass ratio of the yttrium-containing glass microspheres to the flux is 1:(2-12), preferably 1:(4-10).

[0023] Effects of the Invention

[0024] The method described in the present application can accurately and efficiently determine the content of oxides in yttrium-containing glass microspheres. The provided method can solve the problem that yttrium-containing glass microspheres are difficult to digest, and greatly reduces the impact of the microsphere digestion process on the test results, thereby improving the accuracy of the method. DETAILED DESCRIPTION

[0025] The embodiments described below are described in detail for the present application. Although specific embodiments of the present application are shown, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present application and to fully convey the scope of the present application to those skilled in the art.

[0026] It should be noted that certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that technicians may use different nouns to refer to the same component. This specification and claims do not use the difference in nouns as a way to distinguish components, but use the functional differences of components as the criterion for distinction. As mentioned throughout the specification and claims, "including" or "comprising" are open-ended terms and should be interpreted as "including but not limited to". The subsequent description of the specification is a preferred embodiment of the present application, but the description is based on the general principles of the specification and is not intended to limit the scope of the present application. The scope of protection of the present application shall be determined by the attached claims.

[0027] The present application provides a method for determining the oxide content in yttrium-containing glass microspheres, comprising:

[0028] Mixing yttrium-containing glass microspheres with a flux and performing a melting process to obtain a melt;

[0029] The melt is dissolved in an acidic aqueous solution to obtain a test solution, and the content of the oxide is measured;

[0030] The flux is a mixture of anhydrous sodium carbonate and boric acid.

[0031] The present application adopts a melting method to dissolve the glass microspheres, thereby avoiding the influence of silicon fluoride gas generated when using hydrofluoric acid to dissolve the glass on the test results, and the operation is relatively simple.

[0032] The method described in the present application uses a mixture of anhydrous sodium carbonate and boric acid as a flux, which solves the problem that yttrium-containing glass microspheres are difficult to digest, and greatly reduces the impact of the microsphere digestion process on the test results, thereby improving the accuracy of the method.

[0033] The yttrium-containing glass microspheres described in the present application are microspheres prepared using conventional methods in the art, that is, yttrium-containing glass microspheres prepared using yttrium oxide, aluminum oxide, and silicon oxide.

[0034] In the present application, the yttrium-containing glass microspheres refer to glass microspheres containing yttrium elements, for example, yttrium [ 89 Y] glass microspheres or yttrium[ 90 Y] Glass microspheres, yttrium-containing glass microspheres containing oxides such as yttrium oxide, aluminum oxide and silicon oxide.

[0035] The yttrium-containing glass microspheres have special properties and cannot be digested by conventional methods. The method described in the present application can digest the yttrium-containing glass microspheres and accurately determine the content of oxides in the glass microspheres.

[0036] The method described in the present application is to perform quality control on the obtained microspheres, that is, to determine the content of oxides such as yttrium oxide, aluminum oxide and silicon oxide in the glass microspheres to obtain glass microspheres that meet the standards in the art.

[0037] For yttrium-containing glass microspheres, according to the standards in this field, the yttrium oxide content is 10%-75%, the aluminum oxide content is 10%-60%, and the silicon dioxide content is 10-70%. That is, the contents of yttrium oxide, aluminum oxide and silicon oxide need to be controlled within this range to meet the standards in this field.

[0038] For example, for yttrium-containing glass microspheres, the content of yttrium oxide can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, etc.;

[0039] The content of aluminum oxide can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc.;

[0040] The content of silicon dioxide can be 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70%, etc., indicating that the glass microspheres containing yttrium oxide, aluminum oxide and silicon dioxide can be digested using the method described in this application, and the contents of yttrium oxide, aluminum oxide and silicon dioxide in the yttrium-containing glass microspheres can be accurately determined.

[0041] The contents of yttrium oxide, aluminum oxide and silicon oxide in the yttrium-containing glass microspheres measured by the method described in this application are within the range of the above standards and have good repeatability, indicating that the method described in this application is highly accurate and further verifies that the obtained yttrium-containing glass microspheres meet the standards.

[0042] In some embodiments, the mass ratio of the yttrium-containing glass microspheres to the flux is 1:(2-12), preferably 1:(4-10).

[0043] For example, the mass ratio of the yttrium-containing glass microspheres to the flux (m 含钇玻璃微球 :m 熔融剂 ) can be 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, etc.

[0044] In some embodiments, the mass ratio of anhydrous sodium carbonate to boric acid is 1:(0.1-0.5), preferably 1:(0.2-0.5).

[0045] For example, the mass ratio of anhydrous sodium carbonate to boric acid (m 无水碳酸钠 :m 硼酸 ) can be 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, etc.

[0046] In some embodiments, the temperature during melt processing is 700-1000°C, preferably 800-950°C;

[0047] Preferably, the melting treatment time is 30-120 min.

[0048] For example, the temperature during the melt treatment may be 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, etc.;

[0049] The time for melt treatment is 30min, 35min, 40min, 45min, 50min, 55min, 60min, 65min, 70min, 75min, 80min, 85min, 90min, 95min, 100min, 105min, 110min, 115min, 120min and the like.

[0050] In some embodiments, the acidic aqueous solution is an inorganic acid aqueous solution, preferably a nitric acid aqueous solution; preferably, the concentration of the nitric acid aqueous solution is 0.1-5M.

[0051] For example, the concentration of the nitric acid aqueous solution is 0.1M, 0.5M, 1M, 2M, 3M, 4M, 5M, etc.

[0052] In the present application, there is no limitation on the amount of the acidic aqueous solution added, which can be conventionally selected according to needs, as long as the melt is completely dissolved.

[0053] In some embodiments, the measuring is performed using an inductively coupled plasma method. In some embodiments, the oxide comprises yttrium oxide, aluminum oxide and silicon oxide.

[0054] The inductively coupled plasma method is a method for atomic emission spectrometry using a light source that generates plasma discharge through high-frequency inductive coupling. It is a flame technology with a flame temperature range of 6000 to 10000K. The emission intensity represents the concentration of elements in the sample. It is a new type of excitation light source with excellent performance and wide application.

[0055] The method described in the present application uses an inductively coupled plasma method to determine the contents of yttrium, aluminum and silicon in the test solution, thereby obtaining the contents of yttrium oxide, aluminum oxide and silicon oxide, and then further performing quality control on the yttrium-containing glass microspheres.

[0056] The present application does not impose any limitation on the parameters of the inductively coupled plasma method, which are measured using conventional parameters in the art.

[0057] In some embodiments, the method for determining the oxide content in yttrium-containing glass microspheres comprises: mixing yttrium-containing glass microspheres with a flux and performing a melting treatment to obtain a melt; dissolving the melt with an acidic aqueous solution to obtain a test solution, and performing a measurement to obtain the oxide content; the flux is a mixture of anhydrous sodium carbonate and boric acid. In some embodiments, the mass ratio of the yttrium-containing glass microspheres to the flux is 1:(2-12), preferably 1:(4-10). For example, the mass ratio of the yttrium-containing glass microspheres to the flux (m 含钇玻璃微球 :m 熔融剂 ) can be 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, etc. In some embodiments, the mass ratio of anhydrous sodium carbonate to boric acid is 1:(0.1-0.5), preferably 1:(0.2-0.5). For example, the mass ratio of anhydrous sodium carbonate to boric acid (m 无水碳酸钠 :m 硼酸 ) can be 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, etc. In some embodiments, the temperature during the melt treatment is 700-1000°C, preferably 800-950°C; preferably, the time during the melt treatment is 30-120min. For example, the temperature during the melt treatment can be 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, etc.; the time during the melt treatment is 30min, 35min, 40min, 45min, 50min, 55min, 60min, 65min, 70min, 75min, 80min, 85min, 90min, 95min, 100min, 105min, 110min, 115min, 120min, etc. In some embodiments, the acidic aqueous solution is an inorganic acid aqueous solution, preferably a nitric acid aqueous solution; preferably, the concentration of the nitric acid aqueous solution is 0.1-5M. For example, the concentration of the nitric acid aqueous solution is 0.1 M, 0.5 M, 1 M, 2 M, 3 M, 4 M, 5 M, etc. In some embodiments, the determination is performed using an inductively coupled plasma method In some embodiments, the oxide includes yttrium oxide, aluminum oxide, and silicon oxide.

[0058] The method described in the present application is highly accurate in determining the oxide content in yttrium-containing glass microspheres. The obtained oxide content is within the conventional standards in the field, and the method described has good repeatability.

[0059] The present application provides the use of a flux in determining the oxide content in yttrium-containing glass microspheres, wherein the flux is a mixture of anhydrous sodium carbonate and boric acid. In some embodiments, the mass ratio of the anhydrous sodium carbonate to the boric acid is 1:(0.1-0.5), preferably 1:(0.2-0.5).

[0060] For example, the mass ratio of anhydrous sodium carbonate to boric acid (m 无水碳酸钠 :m 硼酸 ) can be 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, etc.

[0061] In some embodiments, the mass ratio of the yttrium-containing glass microspheres to the flux is 1:(2-12), preferably 1:(4-10).

[0062] For example, the mass ratio of the yttrium-containing glass microspheres to the flux (m 含钇玻璃微球 :m 熔融剂 ) can be 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, etc.

[0063] The content control of oxides in yttrium-containing glass microspheres is a very critical quality control project. It not only has an important impact on the later hot medicine process, but also is related to the safety of clinical medication. Whether the glass microspheres can be completely dissolved and not affect subsequent detection is the key to content quality control. There are two commonly used methods for dissolving glass in this field, namely sodium alkali melting method and acid dissolution method. However, experiments have found that the sodium alkali melting method cannot dissolve yttrium-containing glass microspheres, and the use of hydrofluoric acid dissolution method not only cannot completely dissolve yttrium-containing glass microspheres, but also will cause the silicon oxide content to be low due to the production of silicon fluoride gas, and the test results are inaccurate. After a large number of experimental processes, the present application uses anhydrous sodium carbonate and boric acid as mixed fluxes to make the glass microspheres melt under high temperature conditions so that they can be dissolved in an acidic aqueous solution for direct detection. The operation is simple, the results are accurate, and the method is efficient.

[0064] Example

[0065] The present application provides a general and / or specific description of the materials and test methods used in the experiments. In the following examples, unless otherwise specified, % means wt%, i.e., weight percentage. The reagents or instruments used without indicating the manufacturer are all conventional reagent products that can be obtained commercially.

[0066] Example 1

[0067] Take yttrium 89Y] 6 portions of glass microspheres (about 25 mg each, accurately weighed) were placed in platinum crucibles, and 50 mg, 100 mg, 150 mg, 200 mg, 250 mg, and 300 mg of flux were added in sequence (the ratio of glass microspheres to flux was 1:2, 1:4, 1:6, 1:8, 1:10, and 1:12, and the mass ratio of anhydrous sodium carbonate and boric acid in the flux was 2:1), mixed, placed in a muffle furnace, melted at 800°C for 60 minutes, naturally cooled, added 15 mL of 1 M nitric acid solution, heated and stirred to completely dissolve, transferred to a 100 mL volumetric flask, cleaned the crucible with 1 M nitric acid solution in small amounts and multiple times, the washings were combined in the volumetric flask, and diluted to volume with 1 M nitric acid solution.

[0068] Then use ICP-OES to test the above test solution, the instrument parameters are as follows:

[0069] Read time (s): 5 RF power (kW): 1.2 Stabilization time (s): 15

[0070] Viewing mode: Radial Viewing height (mm): 8 Nebulizer flow (L / min): 0.7

[0071] Plasma flow (L / min): 12Aux flow (L / min): 1Sample Uptake Time (s): 18

[0072] Pump Speed ​​(rpm): 12, the contents of yttrium, aluminum and silicon in the solution to be tested were obtained, and the contents of oxides were calculated. The results are shown in Table 1.

[0073] Table 1 Content of oxides in Example 1

[0074]

[0075]

[0076] The results show that the use of the above-mentioned flux ratio can achieve a good microsphere melting effect, and the test results meet the standards (the yttrium oxide content standard is 30% ± 2%, the aluminum oxide content standard is 40% ± 2%, and the silicon dioxide content standard is 30% ± 2%). However, when the ratio of microspheres to flux is 1:2, the melting state of the sample is uneven. At the same time, considering that a too high flux ratio may affect the ICP-OES detection, the 1: (4-10) condition is the best.

[0077] Example 2

[0078] Take yttrium 89 Y] 6 portions of glass microspheres (about 25 mg of sample per portion, accurately weighed) were placed in platinum crucibles respectively, and about 200 mg of flux were added in sequence (the ratio of glass microspheres to flux was 1:8, and the mass ratio of anhydrous sodium carbonate and boric acid in the flux was 2:1), mixed, placed in a muffle furnace, and melted at 700°C, 750°C, 850°C, 900°C, 950°C, and 1000°C for 60 minutes respectively. After natural cooling, 15 mL of 1 M nitric acid solution was added, heated and stirred to completely dissolve, and transferred to a 100 mL volumetric flask. The crucible was cleaned with 1 M nitric acid solution in small amounts and multiple times. The washings were combined in the volumetric flask and diluted to volume with 1 M nitric acid solution.

[0079] Then use ICP-OES to test the above test solution, the instrument parameters are as follows:

[0080] Read time (s): 5 RF power (kW): 1.2 Stabilization time (s): 15

[0081] Viewing mode: Radial Viewing height (mm): 8 Nebulizer flow (L / min): 0.7

[0082] Plasma flow (L / min): 12Aux flow (L / min): 1Sample Uptake Time (s): 18

[0083] Pump Speed ​​(rpm): 12, the contents of yttrium, aluminum and silicon in the solution to be tested were obtained, and the contents of oxides were calculated. The results are shown in Table 2.

[0084] Table 2 Content of oxides in Example 2

[0085]

[0086]

[0087] The results show that the above-mentioned melting temperatures can achieve good microsphere melting effects, and the test results meet the standards (the yttrium oxide content standard is 30% ± 2%, the aluminum oxide content standard is 40% ± 2%, and the silicon dioxide content standard is 30% ± 2%). However, when the melting temperature is 700°C and 750°C, the melting state of the sample is uneven. Considering that too high a melting temperature may affect the performance and operation of the equipment, the 800°C-950°C condition is the best.

[0088] It can be seen from Table 2 that when the melting time is constant, a melting temperature of 700°C-1000°C can achieve a better microsphere melting effect.

[0089] Example 3

[0090] Take yttrium 89 Y] 5 portions of glass microspheres (about 25 mg of sample each, accurately weighed) were placed in platinum crucibles respectively, and about 200 mg of flux were added in sequence (the ratio of glass microspheres to flux was 1:8, and the mass ratios of anhydrous sodium carbonate and boric acid in the flux were 1:0.1, 1:0.2, 1:0.3, 1:0.5, and 1:1), mixed, placed in a muffle furnace, melted at 800°C for 60 minutes, and after natural cooling, 15 mL of 1 M nitric acid solution was added, heated and stirred to completely dissolve, and transferred to a 100 mL volumetric flask, the crucible was cleaned with 1 M nitric acid solution in small amounts and multiple times, the washings were combined in the volumetric flask, and diluted to volume with 1 M nitric acid solution.

[0091] Then use ICP-OES to test the above test solution, the instrument parameters are as follows:

[0092] Read time (s): 5 RF power (kW): 1.2 Stabilization time (s): 15

[0093] Viewing mode: Radial Viewing height (mm): 8 Nebulizer flow (L / min): 0.7

[0094] Plasma flow (L / min): 12Aux flow (L / min): 1Sample Uptake Time (s): 18

[0095] Pump Speed ​​(rpm): 12, the contents of yttrium, aluminum and silicon in the solution to be tested were obtained, and the contents of oxides were calculated. The results are shown in Table 3.

[0096] Table 3 Content of oxides in Example 3

[0097]

[0098]

[0099] The results show that a flux ratio of 1:0.1-1:0.5 can achieve a good microsphere melting effect, and the test results meet the standards (the yttrium oxide content standard is 30%±2%, the aluminum oxide content standard is 40%±2%, and the silicon dioxide content standard is 30%±2%), but when the melting ratio is 1:0.1, the melting state of the sample is uneven, so the flux ratio of 1: (0.2-0.5) is the best condition.

[0100] Example 4

[0101] Take yttrium 89 Y] 6 portions of glass microspheres (about 25 mg each, accurately weighed) were placed in platinum crucibles, and about 200 mg of flux were added in sequence (the ratio of glass microspheres to flux was 1:8, and the mass ratio of anhydrous sodium carbonate and boric acid in the flux was 2:1), mixed, placed in a muffle furnace, melted at 800°C for 60 minutes, and after natural cooling, 15 mL of 1 M nitric acid solution was added, heated and stirred to completely dissolve, and transferred to a 100 mL volumetric flask, and the crucible was cleaned with 1 M nitric acid solution in small amounts and multiple times. The washings were combined in the volumetric flask and diluted to volume with 1 M nitric acid solution.

[0102] Then use ICP-OES to test the above test solution, the instrument parameters are as follows:

[0103] Read time (s): 5 RF power (kW): 1.2 Stabilization time (s): 15

[0104] Viewing mode: Radial Viewing height (mm): 8 Nebulizer flow (L / min): 0.7

[0105] Plasma flow (L / min): 12Aux flow (L / min): 1Sample Uptake Time (s): 18

[0106] Pump Speed ​​(rpm): 12, the contents of yttrium, aluminum and silicon in the solution to be tested were obtained, and the contents of oxides were calculated. The results are shown in Table 4.

[0107] Table 4 Content of oxides in Example 4

[0108] <![CDATA[Y2O3(%)]]> <![CDATA[Al2O3(%)]]> <![CDATA[SiO2(%)]]> Appearance Description Sample 1 29.8 40.6 30.5 Completely melted Sample 2 29.8 39.8 30.4 Completely melted Sample 3 30.0 40.4 30.5 Completely melted Sample 4 30.1 40.5 30.3 Completely melted Sample 5 29.8 40.6 30.4 Completely melted Sample 6 30.3 39.9 31.1 Completely melted RSD% 0.7 0.9 0.9 -

[0109] It can be seen from Table 4 that the RSD of each oxide content result is less than 2%, and the repeatability is good.

[0110] Example 5

[0111] Take 1 portion of each of the four yttrium-containing glass microspheres (about 25 mg each, accurately weighed) and place them in platinum crucibles respectively, add about 200 mg of flux in sequence (the ratio of glass microspheres to flux is 1:8, and the mass ratio of anhydrous sodium carbonate and boric acid in the flux is 2:1), mix well, place in a muffle furnace, melt at 800°C for 60 minutes, add 15 mL of 1 M nitric acid solution after natural cooling, heat and stir to completely dissolve it, transfer to a 100 mL volumetric flask, wash the crucible with 1 M nitric acid solution in small amounts and multiple times, combine the washings into the volumetric flask, and dilute to volume with 1 M nitric acid solution.

[0112] The theoretical compositions of the four yttrium-containing glass microspheres are shown in Table 5.

[0113] Table 5 Theoretical compositions of four yttrium-containing glass microspheres

[0114] <![CDATA[Y2O3(%)]]> <![CDATA[Al2O3(%)]]> <![CDATA[SiO2(%)]]> Microsphere 1 10 20 70 Microsphere 2 15 60 25 Microsphere 3 40 50 10 Microsphere 4 75 10 15

[0115] Then use ICP-OES to test the above test solution, the instrument parameters are as follows:

[0116] Read time (s): 5 RF power (kW): 1.2 Stabilization time (s): 15

[0117] Viewing mode: Radial Viewing height (mm): 8 Nebulizer flow (L / min): 0.7

[0118] Plasma flow (L / min): 12Aux flow (L / min): 1Sample Uptake Time (s): 18

[0119] Pump Speed ​​(rpm): 12, the contents of yttrium, aluminum and silicon in the test solution were obtained, and the content of oxides was calculated. The results are shown in Table 6.

[0120] Table 6 Content of oxides in Example 6

[0121] Appearance Description <![CDATA[Y2O3(%)]]> Relative error (%) <![CDATA[Al2O3(%)]]> Relative error (%) <![CDATA[SiO2(%)]]> Relative error (%) Microsphere 1 Completely melted 10.2 1.9 19.8 1.0 70.2 0.3 Microsphere 2 Completely melted 14.8 1.3 60.5 0.8 25.3 1.2 Microsphere 3 Completely melted 40.5 1.3 49.5 1.0 10.0 0 Microsphere 4 Completely melted 75.4 0.5 9.8 1.9 15.1 0.7

[0122] It can be seen from Table 6 that the relative errors between the measured values ​​and the theoretical values ​​of the oxide content in each yttrium-containing microsphere are no more than 2%, indicating that the method described in this application has a high accuracy for various yttrium-containing glass microspheres.

[0123] In summary, the yttrium-containing glass microspheres in the present application are composed of yttrium oxide, aluminum oxide and silicon dioxide, wherein the proportion of yttrium oxide is 10%-75%, the proportion of aluminum oxide is 10%-60%, and the proportion of silicon dioxide is 10%-70%.

[0124] Comparative Example 1

[0125] The difference between Comparative Example 1 and Example 1 lies in the difference in the flux. Sodium hydroxide is selected as the flux. Unmelted glass microspheres are visible in the solid material obtained after melting under the same high temperature conditions. The melt cannot be completely dissolved by the acidic aqueous solution and cannot be detected by ICP-OES.

[0126] The above is only the preferred embodiment of the present application, and does not limit the present application in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present application without departing from the technical solution of the present application still falls within the protection scope of the technical solution of the present application.

Claims

1. A method for determining the oxide content in yttrium-containing glass microspheres, comprising: Mixing yttrium-containing glass microspheres with a flux and performing a melting process to obtain a melt; The melt is dissolved in an acidic aqueous solution to obtain a test solution, and the content of the oxide is measured; The flux is a mixture of anhydrous sodium carbonate and boric acid; The mass ratio of the yttrium-containing glass microspheres to the flux is 1:(4-8); The mass ratio of anhydrous sodium carbonate to boric acid is 1:(0.3-0.5); The temperature during the melt treatment is 850-950°C; The acidic aqueous solution is a nitric acid aqueous solution, and the concentration of the nitric acid aqueous solution is 0.1-5M; The measurement is carried out using an inductively coupled plasma method.

2. The method according to claim 1, wherein: The melting time is 30-120 minutes.

3. The method according to any one of claims 1 to 2, wherein: The oxides include yttrium oxide, aluminum oxide, and silicon oxide.

4. Use of a flux in determining the oxide content in yttrium-containing glass microspheres, wherein: The flux is a mixture of anhydrous sodium carbonate and boric acid; The mass ratio of anhydrous sodium carbonate to boric acid is 1:(0.3-0.5); The mass ratio of the yttrium-containing glass microspheres to the flux is 1:(4-8); The measurement methods include: Mixing yttrium-containing glass microspheres with a flux and performing a melting process to obtain a melt; The melt is dissolved in an acidic aqueous solution to obtain a test solution, and the content of the oxide is measured; The temperature during the melt treatment is 850-950°C; The acidic aqueous solution is a nitric acid aqueous solution, and the concentration of the nitric acid aqueous solution is 0.1-5M; The measurement is carried out using an inductively coupled plasma method.