Brightness enhancement film with anti-electromagnetic wave effect and preparation method thereof
By integrating reflection and absorption loss-type materials in the brightness enhancement film, combined with graphene and modified ferrite nanowires, dual protection against electromagnetic waves is achieved, solving the problem of limited performance of existing brightness enhancement films in anti-electromagnetic wave environments. , improving the performance of the LCD display.
Patent Information
- Application Number
- CN202411006185.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-01
AI Technical Summary
Existing brightness-enhancing films have limited performance in environments that require resistance to electromagnetic waves, and cannot take into account both light-gathering performance and electromagnetic wave shielding performance.
Design a brightness-enhancing film, including a prism structure layer, a functional layer and a base material layer from top to bottom. The functional layer is composed of a shielding group and an absorbing group. The shielding group uses a reflection loss type material, and the absorbing group uses an absorption loss type. material, achieving double protection against electromagnetic waves by integrating two materials. The absorbing unit of the absorbing group is composed of modified ferrite and iron nanowires, and the shielding group uses graphene combined with ultraviolet curing resin to prepare a prism structural layer.
It achieves effective shielding and absorption of electromagnetic waves, improves the performance of the LCD display in specific environments, while maintaining the light-gathering performance.
Smart Images

Figure CN118732103A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical protective films, and in particular to a brightness enhancement film with an anti-electromagnetic wave effect and a preparation method thereof. Background Art
[0002] With the development of electronic display and other related technologies, new requirements have been put forward for the functions of brightness enhancement films. The main function of brightness enhancement films is to focus light and improve the utilization rate of light; however, this single-function brightness enhancement film limits the performance of LCD screens in some specific environments, such as occasions that require electromagnetic wave resistance.
[0003] In order to meet the diverse market demands, how to prepare a brightness enhancement film with anti-electromagnetic wave effect, while ensuring the light focusing performance and taking into account its anti-electromagnetic wave performance is the technical problem that the present invention aims to solve. Summary of the invention
[0004] In order to solve at least one of the above problems, the present invention provides a brightness enhancement film with anti-electromagnetic wave effect, which includes a prism structure layer, a functional layer and a substrate layer from top to bottom; wherein the functional layer is composed of a shielding group and an absorbing group; the absorbing group is a plurality of absorbing units arranged at intervals.
[0005] When electromagnetic waves reach the surface of a material, they can be divided into reflection loss type materials and absorption loss type materials according to the interaction mechanism between the electromagnetic waves and the material; reflection loss type materials achieve the shielding function by reflecting electromagnetic waves, while absorption loss type materials create special boundary conditions so that the incident electromagnetic waves are not reflected on the surface of the material and enter the interior of the material as much as possible; absorbing materials can convert the electromagnetic waves entering the interior of the material into heat energy, so that they are quickly absorbed and attenuated. In the technical solution provided by the present invention, the functional layer includes a shielding group and an absorbing group. The shielding group uses reflection loss type materials, and the absorbing group uses absorption loss type materials. By integrating the two materials into an integral functional group, dual protection of shielding and absorption of electromagnetic waves is achieved.
[0006] Furthermore, the width of the wave absorbing unit is 40-60 μm; the height of the wave absorbing unit is 60-80 μm; and the distance between any two adjacent wave absorbing units does not exceed the width of the wave absorbing unit.
[0007] Furthermore, the raw materials of the absorbing unit include, by mass, 20-30 parts of acrylic resin and 60-80 parts of absorbing resin particles; wherein the average particle size of the absorbing resin particles is 5-10 μm.
[0008] Furthermore, the absorbing resin particles are prepared by the following method: A: using a silane coupling agent to activate the surface of ferrite microspheres to obtain modified ferrite; B: mixing and stirring isocyanate and a catalyst, adding a diol to react to obtain a prepolymer; C: adding modified ferrite and iron nanowires to the prepolymer, applying magnetic stirring at the same time, and reacting to obtain an absorbing resin; D: adding a foaming agent to the absorbing resin, and then sequentially performing a curing treatment and a crushing treatment to obtain absorbing resin particles.
[0009] Furthermore, according to the mass ratio, the raw materials of the absorbing resin particles meet the following requirements: isocyanate: diol: catalyst: blowing agent: modified ferrite: iron nanowire = (45-60): (45-60): (0.1-1): (0.1-1): (20-30): (20-30).
[0010] Furthermore, the raw materials of the shielding group include, by mass, 80-120 parts of acrylic resin, 20-30 parts of cross-linking agent, 50-65 parts of shielding material, and 5-10 parts of dispersant.
[0011] Furthermore, the shielding material is graphene.
[0012] Furthermore, the material of the substrate layer is one of PET, PC or PMMA; the thickness of the substrate layer is 200-250 μm.
[0013] Furthermore, the prism structure layer includes a plurality of prism monomers, each of which has a height of 30-40 μm; the raw material of the prism structure layer includes ultraviolet curing resin; the ultraviolet curing resin is selected from at least one of isocyanate, polyurethane, epoxy resin and acrylate.
[0014] The present invention also provides a method for preparing the above-mentioned brightness enhancement film, comprising the following steps: obtaining a substrate layer; applying a shielding slurry on the surface of the substrate layer, baking it at a temperature of 200-220°C for 15-30s, and then using an embossing roller to transfer the shape of the absorbing unit on the surface of the shielding slurry, and curing it with an ultraviolet light source at a temperature of 120-150°C for 5-10min; then applying the absorbing slurry, and curing it with an ultraviolet light source for 5-10min to obtain a functional layer; applying a brightening slurry on the surface of the functional layer, transferring it with an embossing roller to obtain a prism structure, and curing it with an ultraviolet light source for 30-45min to obtain a prism structure layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0016] Figure 1 A schematic structural diagram of a brightness enhancement film provided in an embodiment of the present invention.
[0017] Figure 2 for Figure 1 Sectional view along line A-A'.
[0018] Explanation of reference numerals: 10 - prism structure layer; 20 - functional layer; 21 - wave absorbing unit; 22 - shielding group; 30 - substrate layer. DETAILED DESCRIPTION
[0019] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] In the related art, the brightness enhancement film generally includes a substrate, a functional layer 20 and a prism structure; the substrate is the base of the brightness enhancement film, and generally a material with high light transmittance is selected; the functional layer 20 can be set according to actual needs, such as anti-peep function, wide-angle function, wave absorption function, etc.; the prism structure is mainly used for centralized brightness enhancement. With the development of technology, improving the anti-electromagnetic wave performance of the brightness enhancement film is also a focus of current research and development.
[0021] Based on the above reasons, the present application provides a brightness enhancement film with anti-electromagnetic wave effect, which includes a prism structure layer 10, a functional layer 20 and a substrate layer 30 from top to bottom; wherein the functional layer 20 is composed of a shielding group 22 and an absorbing group; the absorbing group is a plurality of absorbing units 21 arranged at intervals; see Figure 1 and Figure 2 .
[0022] When electromagnetic waves reach the surface of a material, they can be divided into reflection loss type materials and absorption loss type materials according to the interaction mechanism between the electromagnetic waves and the material; reflection loss type materials achieve the shielding function by reflecting electromagnetic waves, while absorption loss type materials create special boundary conditions so that the incident electromagnetic waves are not reflected on the surface of the material and enter the interior of the material as much as possible; absorbing materials can convert the electromagnetic waves entering the interior of the material into heat energy, so that they are quickly absorbed and attenuated. In the technical solution provided by the present invention, the functional layer 20 includes a shielding group 22 and an absorbing group. The shielding group 22 uses a reflection loss type material, and the absorbing group uses an absorption loss type material. By integrating the two materials into an integral functional group, dual protection of shielding and absorption of electromagnetic waves is achieved.
[0023] Furthermore, the microwave absorbing resin particles are prepared by the following method:
[0024] A: Use silane coupling agent to activate the surface of ferrite microspheres to obtain modified ferrite;
[0025] B: Mix and stir isocyanate and catalyst, add diol to react to obtain prepolymer;
[0026] C: adding modified ferrite and iron nanowires to the prepolymer to react and obtain a microwave absorbing resin;
[0027] D: Add a foaming agent to the absorbing resin, and then perform curing treatment and crushing treatment in sequence to obtain absorbing resin particles.
[0028] Furthermore, according to the mass ratio, the raw materials of the absorbing resin particles meet the following requirements: isocyanate: diol: catalyst: blowing agent: modified ferrite: iron nanowire = (45-60): (45-60): (0.1-1): (0.1-1): (20-30): (20-30).
[0029] Preferably, the microwave absorbing resin particles are prepared by the following method:
[0030] A: Soak the ferrite microspheres in silane coupling agent, disperse them ultrasonically for 2-3 hours at 40-45°C, filter and dry to obtain modified ferrite.
[0031] B: At 10-30°C, mix isocyanate and catalyst and stir for 30-45 minutes; add diol and stir for 1-2 hours to obtain a prepolymer.
[0032] C: Adding modified ferrite and iron nanowires to the prepolymer, applying magnetic stirring at the same time, controlling the reaction temperature to 50-60°C, and reacting for 6-8 hours to obtain the microwave absorbing resin;
[0033] D: Add a foaming agent to the absorbing resin, and then perform curing treatment and crushing treatment in sequence to obtain absorbing resin particles.
[0034] In the above process, there is no special requirement for the content of ferrite microspheres and silane coupling agent, and those skilled in the art can set them according to the needs of the reagents. The modified ferrite after activation is more easily cross-linked with the polyurethane resin. Furthermore, the ferrite microspheres are microspheres with Fe3O4 as the matrix, and can also be compounded with other metal materials. The average particle size of the ferrite microspheres is 10-100nm; preferably, the ferrite microspheres are hollow microspheres, which can increase the attenuation rate of electromagnetic waves inside the material.
[0035] Preferably, the isocyanate is selected from at least one of xylene diisocyanate, toluene diisocyanate, diisocyanate polyethylene glycol, diphenylmethane diisocyanate, lysine diisocyanate, o-xylene diisocyanate, hexamethylene diisocyanate, TDI trimer, and diisocyanate ditoluene; the diol is selected from at least one of triethylene glycol, polypropylene glycol, tetraethylene glycol, and diethylene glycol. The length of the iron nanowire is preferably no more than 5 μm.
[0036] In this embodiment, modified ferrite and iron nanowires are added to the prepolymer. As the polymerization reaction proceeds, the modified ferrite is cross-linked to the interior of the polyurethane resin. In order to improve the dispersion of the modified ferrite, magnetic stirring is applied during the reaction to obtain a polyurethane resin with ferrite microspheres uniformly embedded inside. Ferrite microspheres, as wave-absorbing components, can convert electromagnetic waves into thermal energy to achieve the absorption function, so heat dissipation performance is also an important indicator. In the above preparation method, since the modified ferrite is wrapped by polyurethane, its heat dissipation performance will also be affected to a certain extent; further, iron nanowires are added as bridges to overlap the ferrite microspheres, thereby forming a highly connected three-dimensional network structure; so that after the ferrite microspheres absorb electromagnetic waves, they can better transfer heat energy. Preferably, the iron nanowires are α-Fe nanowires.
[0037] In step D, a foaming agent is added to generate a large number of bubbles inside the absorbing resin, which is beneficial to the subsequent crushing process. Among them, the foaming agent can be selected, for example, cyclopentane. Generally speaking, the crushing process is to grind the cured absorbing resin to obtain absorbing resin particles with an average particle size of 5-10 μm. In this embodiment, the absorbing resin particles use polyurethane as a matrix and have good light transmittance. On the other hand, because they are added to the absorbing unit 21 in the form of particles, they have a certain brightening effect.
[0038] Furthermore, in terms of mass, the raw materials of the absorbing unit 21 include: 20-30 parts of acrylic resin and 60-80 parts of absorbing resin particles; wherein the average particle size of the absorbing resin particles is 5-10 μm.
[0039] In this embodiment, acrylic resin is used as the base material for dispersing the absorbing resin particles. To ensure the absorbing and heat dissipating effects, its usage is relatively small. The mass of acrylic resin needs to be controlled to be less than 50% of the mass of the absorbing resin particles.
[0040] Further, by weight, the raw materials of the shielding group 22 include: 80-120 parts of acrylic resin, 20-30 parts of cross-linking agent, 50-65 parts of shielding material, and 5-10 parts of dispersant. Preferably, the shielding material is graphene.
[0041] In this embodiment, the shielding material is mainly used to reflect electromagnetic waves, and generally carbon-based materials are selected, such as carbon nanotubes, graphene, carbon fibers, etc. Graphene is preferred in this embodiment. The cross-linking agent is preferably glycidyl ether, and the dispersant is preferably nano nickel powder.
[0042] Furthermore, the width of the absorbing unit 21 is 40-60 μm; the height of the absorbing unit 21 is 60-80 μm; and the distance between any two adjacent absorbing units 21 does not exceed the width of the absorbing unit 21 .
[0043] In a specific embodiment, since the shielding material uses graphene, it may have a certain influence on the light transmission performance of the film material. Therefore, from the cross-section of the functional layer 20, preferably, the area of the shielding group 22 is smaller than the area of the absorbing group. In this embodiment, the size and spacing of the absorbing units 21 are set. Since the absorbing units 21 have a certain light focusing effect in addition to the absorbing function, the spacing between any two adjacent absorbing units 21 should not be too large, preferably not more than twice its width.
[0044] Due to the requirement of light transmittance, generally speaking, the material of the substrate layer 30 is one of PET, PC or PMMA; the thickness of the substrate layer 30 is 200-250 μm.
[0045] Furthermore, the prism structure layer 10 includes a plurality of prism monomers, each of which has a height of 30-40 μm; the raw material of the prism structure layer 10 includes a UV curable resin; the UV curable resin is selected from at least one of isocyanate, polyurethane, epoxy resin, and acrylate. In this embodiment, the prism structure layer 10 is mainly used for centralized brightness enhancement. Generally speaking, the prism monomer is a multi-faceted pyramid structure, or a prism structure. This embodiment does not specifically limit its specific structure and shape, and those skilled in the art can adjust it according to actual production needs.
[0046] The present invention also provides a method for preparing the brightness enhancement film, comprising the following steps:
[0047] S10: Obtaining a substrate layer 30;
[0048] S20: coating the shielding slurry on the surface of the substrate layer 30, baking at a temperature of 200-220°C for 15-30s, then using an embossing roller to transfer the shape of the absorbing unit 21 on the surface of the shielding slurry, and curing it at a temperature of 120-150°C with a UV light source for 5-10min; then coating the absorbing slurry, and curing it with a UV light source for 5-10min to obtain a functional layer 20;
[0049] S30: coating the surface of the functional layer 20 with a brightening slurry, transferring the prism structure using an embossing roller, and curing the prism structure layer 10 with an ultraviolet light source for 30-45 minutes.
[0050] The brightening slurry, i.e. the slurry of the prism structure layer 10, includes ultraviolet curing resin, and those skilled in the art can add other additives according to the needs of the reagent, which is not particularly limited here. The absorbing slurry includes 20-30 parts of acrylic resin and 60-80 parts of absorbing resin particles.
[0051] The shielding slurry comprises 80-120 parts of acrylic resin, 20-30 parts of cross-linking agent, 50-65 parts of shielding material and 5-10 parts of dispersant.
[0052] Further, taking graphene, glycidyl ether, nano nickel powder and acrylic resin as an example, the preparation process of the shielding slurry is as follows:
[0053] Under protective atmosphere, nano nickel powder and graphene are mixed and ball-milled at a speed of 25-30 r / min for 1-3 hours, and then heat-treated at a temperature of 600-800°C for 8-10 hours; after the heat treatment, the temperature is rapidly cooled to room temperature at a cooling rate of 60-70°C / min and a second ball-milling is performed; the speed of the second ball-milling is set to 10-15 r / min, and the ball-milling time is 5-8 hours; a composite powder is obtained. The composite powder, glycidyl ether and acrylic resin are mixed and stirred for 1-2 hours to obtain a shielding slurry.
[0054] In this embodiment, the nano nickel powder and graphene are firstly dry-milled at a relatively fast speed to make the two evenly mixed, and the collision generated by the ball milling is used to achieve mechanical bonding between the nano nickel powder and the graphene. Further, the bonding strength between the two is further strengthened by the process of heat preservation and rapid cooling, and then the composite powder of the nano nickel powder and the graphene is obtained by slow and long-term ball milling, and the nickel powder is attached to the surface of the graphene.
[0055] Furthermore, in step S20, before baking, a 2T magnetic field is applied to the substrate layer 30 coated with the shielding slurry for 5-10 minutes, so that the nano nickel powder can be evenly distributed in the coating under the effect of the magnetic field, and further, the distribution of graphene in the coating is more uniform. As a shielding material, graphene can realize the function of electromagnetic shielding on the one hand, and on the other hand, due to its excellent heat dissipation performance, it is also conducive to the discharge of heat energy generated by the absorbing group.
[0056] Example 1
[0057] The present invention also provides a method for preparing the brightness enhancement film, comprising the following steps:
[0058] S10: Obtain a substrate layer; the substrate layer is made of PET and has a thickness of 200 μm.
[0059] S20: Shielding slurry is coated on the surface of the substrate layer, treated with a 2T magnetic field for 5 minutes, baked at 200°C for 15 seconds, and then the shape of the absorbing unit is transferred to the surface of the shielding slurry using an embossing roller, and cured at 120°C with a UV light source for 5 minutes; then the absorbing slurry is coated and cured with a UV light source for 5 minutes to obtain a functional layer.
[0060] The width of the absorbing unit is 40 μm; the height of the absorbing unit is 60 μm; and the spacing between any two adjacent absorbing units is 40 μm.
[0061] S30: coating a brightening slurry on the surface of the functional layer, transferring the prism structure using an embossing roller, and curing the prism structure layer using an ultraviolet light source for 30 minutes.
[0062] The preparation method of the shielding slurry is as follows: in a protective atmosphere, the nano nickel powder and graphene are mixed and ball-milled at a speed of 25 r / min for 1 hour, and then heat-treated at a temperature of 600°C for 8 hours; after the heat treatment, the temperature is quickly cooled to room temperature at a cooling rate of 60°C / min and a second ball-milling is performed; the speed of the second ball-milling is set to 10 r / min, and the ball-milling time is 5 hours; a composite powder is obtained. The composite powder, glycidyl ether and acrylic resin are mixed and stirred for 1 hour to obtain a shielding slurry.
[0063] The shielding slurry includes 80 parts of acrylic resin, 20 parts of glycidyl ether, 50 parts of graphene and 5 parts of nano nickel powder.
[0064] The microwave absorbing slurry comprises 20 parts of acrylic resin and 60 parts of microwave absorbing resin particles.
[0065] The preparation process of the microwave absorbing resin particles is as follows:
[0066] A: Soak the ferrite microspheres in silane coupling agent, disperse them ultrasonically at 40°C for 2 hours, and filter and dry to obtain modified ferrite.
[0067] B: At 10°C, mix isocyanate and catalyst and stir for 30 minutes; add diol and stir for 1 hour to obtain a prepolymer.
[0068] C: Add modified ferrite and iron nanowires to the prepolymer, apply magnetic stirring, control the reaction temperature to 50°C, and react for 6 hours to obtain the absorbing resin;
[0069] D: Add a foaming agent to the absorbing resin, and then perform curing treatment and crushing treatment in sequence to obtain absorbing resin particles with an average particle size of 5 μm.
[0070] The raw materials of the wave-absorbing resin particles meet the following conditions: isocyanate: diol: catalyst: foaming agent: modified ferrite: iron nanowire = 45:45:0.1:0.1:20:20.
[0071] Example 2
[0072] The present invention also provides a method for preparing the brightness enhancement film, comprising the following steps:
[0073] S10: Obtain a substrate layer; the substrate layer is made of PMMA and has a thickness of 250 μm.
[0074] S20: coating the shielding slurry on the surface of the substrate layer, baking at 220°C for 30s, then using an embossing roller to transfer the shape of the absorbing unit on the surface of the shielding slurry, and curing it at 150°C for 10min with a UV light source; then coating the absorbing slurry, and curing it with a UV light source for 10min to obtain a functional layer.
[0075] The width of the wave absorbing unit is 60 μm; the height of the wave absorbing unit is 80 μm; and the spacing between any two adjacent wave absorbing units is 60 μm.
[0076] S30: coating a brightening slurry on the surface of the functional layer, transferring the prism structure using an embossing roller, and curing the prism structure layer using an ultraviolet light source for 45 minutes.
[0077] The preparation method of the shielding slurry is as follows: in a protective atmosphere, the nano nickel powder and graphene are mixed and ball milled at a speed of 30r / min for 3h, and then heat treated at a temperature of 800℃ for 10h; after the heat treatment, the temperature is quickly cooled to room temperature at a cooling rate of 70℃ / min and a second ball milling is performed; the speed of the second ball milling is set to 15r / min, and the ball milling time is 8h; a composite powder is obtained. The composite powder, glycidyl ether and acrylic resin are mixed and stirred for 2h to obtain a shielding slurry. In the shielding slurry, there are 120 parts of acrylic resin, 30 parts of glycidyl ether, 65 parts of graphene and 10 parts of nano nickel powder.
[0078] The microwave absorbing slurry comprises 30 parts of acrylic resin and 80 parts of microwave absorbing resin particles.
[0079] The preparation process of the microwave absorbing resin particles is as follows:
[0080] A: Soak the ferrite microspheres in silane coupling agent, disperse them ultrasonically at 45°C for 3 hours, and filter and dry to obtain modified ferrite.
[0081] B: At 30°C, mix isocyanate and catalyst and stir for 45 minutes; add diol and stir for 2 hours to obtain a prepolymer.
[0082] C: Add modified ferrite and iron nanowires to the prepolymer, apply magnetic stirring, control the reaction temperature to 60°C, and react for 8 hours to obtain the absorbing resin;
[0083] D: Add a foaming agent to the absorbing resin, and then perform curing treatment and crushing treatment in sequence to obtain absorbing resin particles with an average particle size of 10 μm.
[0084] The raw materials of the wave-absorbing resin particles meet the following conditions: isocyanate: diol: catalyst: foaming agent: modified ferrite: iron nanowire = 60:60:1:1:30:30.
[0085] Example 3
[0086] The present invention also provides a method for preparing the brightness enhancement film, comprising the following steps:
[0087] S10: Obtain a substrate layer; the substrate layer is made of PET and has a thickness of 220 μm.
[0088] S20: Apply shielding slurry on the surface of the substrate layer, bake at 210°C for 20s, then use an embossing roller to transfer the shape of the absorbing unit on the surface of the shielding slurry, and cure it at 130°C with a UV light source for 8min; then apply the absorbing slurry and cure it with a UV light source for 8min to obtain a functional layer.
[0089] The width of the wave absorbing unit is 50 μm; the height of the wave absorbing unit is 70 μm; and the interval between any two adjacent wave absorbing units is 30 μm.
[0090] S30: coating a brightening slurry on the surface of the functional layer, transferring the prism structure using an embossing roller, and curing the prism structure layer using an ultraviolet light source for 40 minutes.
[0091] The preparation method of the shielding slurry is as follows: in a protective atmosphere, the nano nickel powder and graphene are mixed and ball milled at a speed of 25r / min for 2h, and then heat treated at a temperature of 700°C for 9h; after the heat treatment, the temperature is quickly cooled to room temperature at a cooling rate of 65°C / min and a second ball milling is performed; the speed of the second ball milling is set to 12r / min, and the ball milling time is 7h; a composite powder is obtained. The composite powder, glycidyl ether and acrylic resin are mixed and stirred for 2h to obtain a shielding slurry. In the shielding slurry, there are 9 parts of acrylic resin, 25 parts of glycidyl ether, 55 parts of graphene and 5 parts of nano nickel powder.
[0092] The microwave absorbing slurry comprises 25 parts of acrylic resin and 70 parts of microwave absorbing resin particles.
[0093] The preparation process of the microwave absorbing resin particles is as follows:
[0094] A: Soak the ferrite microspheres in silane coupling agent, disperse them ultrasonically at 40°C for 3 hours, and filter and dry to obtain modified ferrite.
[0095] B: At 20°C, mix isocyanate and catalyst and stir for 30 minutes; add diol and stir for 1 hour to obtain a prepolymer.
[0096] C: Add modified ferrite and iron nanowires to the prepolymer, apply magnetic stirring, control the reaction temperature to 55°C, and react for 7 hours to obtain the absorbing resin;
[0097] D: Add a foaming agent to the absorbing resin, and then perform curing treatment and crushing treatment in sequence to obtain absorbing resin particles with an average particle size of 8 μm.
[0098] The raw materials of the wave-absorbing resin particles meet the following conditions: isocyanate: diol: catalyst: foaming agent: modified ferrite: iron nanowire = 50:60:0.4:0.6:25:20.
[0099] Comparative Example 1
[0100] A brightness enhancement film is provided, and its preparation process is similar to that of Example 1, except that no wave absorbing group is provided.
[0101] Comparative Example 2
[0102] A brightness enhancement film is provided, and its preparation process is similar to that of Example 1, except that no shielding group is provided.
[0103] The brightness enhancement films provided in Examples 1-3 and Comparative Examples 1-2 were subjected to performance tests, as shown in Table 1. Electromagnetic waves within the frequency band of 2 GHZ-4 GHZ were used for the tests to detect the shielding / absorption rate of the electromagnetic waves.
[0104] Table 1
[0105] Transmittance % Electromagnetic wave shielding / absorption rate % Example 1 93.2 94.5 Example 2 92.8 93.7 Example 3 92.0 93.4 Comparative Example 1 89.1 88.0 Comparative Example 2 92.3 87.5
[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A brightness enhancement film with anti-electromagnetic wave effect, characterized in that: It includes a prism structure layer, a functional layer and a substrate layer from top to bottom; Wherein, the functional layer is composed of a shielding group and a wave absorbing group; the wave absorbing group is a plurality of wave absorbing units arranged at intervals.
2. The brightness enhancement film according to claim 1, characterized in that: The width of the wave absorbing unit is 40-60 μm; the height of the wave absorbing unit is 60-80 μm; and the distance between any two adjacent wave absorbing units does not exceed the width of the wave absorbing unit.
3. The brightness enhancement film according to claim 1, characterized in that: According to the mass, the raw materials of the wave absorbing unit include: 60-80 parts of acrylic resin and 15-25 parts of wave absorbing resin particles; Wherein, the average particle size of the absorbing resin particles is 5-10 μm.
4. The brightness enhancement film according to claim 3, characterized in that: The wave absorbing resin particles are prepared by the following method: A: Use silane coupling agent to activate the surface of ferrite microspheres to obtain modified ferrite; B: Mix and stir isocyanate and catalyst, add diol to react to obtain prepolymer; C: adding the modified ferrite and the iron nanowires to the prepolymer, applying magnetic stirring at the same time, and reacting to obtain a microwave absorbing resin; D: adding a foaming agent to the absorbing resin, and then sequentially performing a curing treatment and a crushing treatment to obtain the absorbing resin particles.
5. The brightness enhancement film according to claim 4, characterized in that: According to the mass ratio, the raw materials of the absorbing resin particles meet the following requirements: Isocyanate: diol: catalyst: blowing agent: modified ferrite: iron nanowire = (45-60): (45-60): (0.1-1): (0.1-1): (20-30): (20-30).
6. The brightness enhancement film according to claim 1, characterized in that: According to mass, the raw materials of the shielding group include: 80-120 parts of acrylic resin, 20-30 parts of cross-linking agent, 50-65 parts of shielding material, and 5-10 parts of dispersant.
7. The brightness enhancement film according to claim 6, characterized in that: The shielding material is graphene.
8. The brightness enhancement film according to claim 1, characterized in that: The material of the substrate layer is one of PET, PC or PMMA; the thickness of the substrate layer is 200-250 μm.
9. The brightness enhancement film according to claim 1, characterized in that: The prism junction structure layer includes a plurality of prism monomers, and the height of each prism monomer is 30-40 μm; The raw material of the prism structure layer includes ultraviolet curing resin; the ultraviolet curing resin is selected from at least one of isocyanate, polyurethane, epoxy resin and acrylate.
10. The method for preparing a brightness enhancement film according to any one of claims 1 to 9, characterized in that: The following steps are involved: obtaining a substrate layer; Apply shielding slurry on the surface of the substrate layer, bake at 200-220°C for 15-30s, then use an embossing roller to transfer the shape of the absorbing unit on the surface of the shielding slurry, and cure it at 120-150°C with a UV light source for 5-10min; then apply absorbing slurry, and cure it with a UV light source for 5-10min to obtain a functional layer; The brightening slurry is coated on the surface of the functional layer, and a prism structure is obtained by transfer printing using an embossing roller. The prism structure layer is obtained by curing with an ultraviolet light source for 30-45 minutes.