Optical laminate

By adjusting the relationship between refractive index and thickness in the optical laminate, the unevenness of the liquid crystal phase retardation film optical laminate in the tilt direction was solved, achieving a more uniform optical performance.

CN118732137APending Publication Date: 2024-10-01SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410378103.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-02-29
Filing Date
2024-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing optical laminates with multiple liquid crystal phase retardation films are prone to unevenness in the tilt direction.

Method used

By adjusting the refractive index and thickness relationship of each layer in the optical laminate, especially controlling the refractive index difference between the second protective film and the first adhesive layer within a certain range and satisfying a specific refractive index relationship nx>ny≥nz or nx

Benefits of technology

It effectively reduces interference inhomogeneity of optical laminates when viewed from an oblique direction, and improves the overall performance of optical laminates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118732137A_ABST
    Figure CN118732137A_ABST
Patent Text Reader

Abstract

The present invention provides an optical laminate which is provided with a retardation plate having a plurality of liquid crystal retardation films, and which has reduced unevenness when viewed from an inclined direction. The optical laminate is obtained by laminating a first protective film, an adhesive layer, a polarizer, an adhesive layer, a second protective film, a first adhesive layer, a first liquid crystal phase difference film, a second adhesive layer, and a second liquid crystal phase difference film adjacent to each other in this order. When the refractive index of the second protective film with respect to light having a wavelength of 589 nm is defined as NaII and the refractive index of the first adhesive layer with respect to light having a wavelength of 589 nm is defined as NbI, the second protective film and the first adhesive layer satisfy the following formula (1): NaII-NbI < 0.1 (1), and the first liquid crystal phase difference film and the second liquid crystal phase difference film each independently satisfy the following formula (2) or formula (3): nx > ny > = nz (2) nx < ny < = nz (3). The thickness of the second adhesive layer is 2.8 [mu] m to 20 [mu] m.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to optical stacks. Background Art

[0002] Conventionally, in image display devices, a method of disposing a circular polarizing plate on the visible side of an image display panel to suppress a decrease in visibility due to reflection of external light has been adopted.

[0003] The circular polarizing plate is an optical laminate in which a linear polarizing plate and a phase difference plate are stacked. In the circular polarizing plate, the external light toward the image display panel is converted into linear polarized light by the linear polarizing plate, and then converted into circular polarized light by the subsequent phase difference plate. Although the external light as circular polarized light is reflected on the surface of the image display panel, the rotation direction of the polarization plane is reversed during the reflection, and after being converted into linear polarized light by the phase difference plate, it is shielded by the subsequent linear polarizing plate. As a result, the emission of external light to the outside is significantly suppressed.

[0004] Among retardation plates, a structure having a liquid crystal retardation film (Japanese: phase difference film) containing a cured product of a liquid crystal compound is known (for example, Patent Documents 1 and 2). With this structure, the retardation plate can be made thinner.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-163935

[0008] Patent Document 2: Japanese Patent Application Publication No. 2019-91030 Summary of the invention

[0009] Problems to be solved by the invention

[0010] An optical laminate including a retardation plate having a plurality of liquid crystal retardation films may be uneven when viewed from an oblique direction.

[0011] A first object of the present invention is to provide an optical laminate including a retardation plate having a plurality of liquid crystal retardation films, wherein unevenness when viewed from an oblique direction is reduced.

[0012] Means for solving problems

[0013] A first aspect of the present invention provides the following optical layered body.

[0014] [1-1] An optical laminate, wherein a first protective film, an adhesive layer, a polarizing plate, an adhesive layer, a second protective film, a first adhesive bonding layer, a first liquid crystal retardation film, a second adhesive bonding layer, and a second liquid crystal retardation film are laminated adjacent to each other in this order,

[0015] When the refractive index of the second protective film with respect to light of wavelength 589 nm is N aII The refractive index of the first adhesive layer with respect to light of wavelength 589 nm is N bI When the second protective film and the first adhesive layer satisfy the following formula (1):

[0016] |N aII -N bI |<0.1···(1),

[0017] The first liquid crystal retardation film and the second liquid crystal retardation film each independently satisfy the following formula (2) or formula (3):

[0018] nx>ny≥nz···(2)

[0019] nx<ny≤nz···(3),

[0020] The thickness of the second adhesive layer is 2.8 μm to 20 μm.

[0021] (In formula (2) and formula (3), nx represents the principal refractive index in the direction parallel to the plane of the first liquid crystal retardation film or the second liquid crystal retardation film in the refractive index ellipsoid formed by the first liquid crystal retardation film or the second liquid crystal retardation film, ny represents the refractive index in the direction parallel to the plane and orthogonal to the direction of nx in the refractive index ellipsoid, and nz represents the refractive index in the direction perpendicular to the plane in the refractive index ellipsoid.)

[0022] [1-2] The optical layered body according to [1-1], wherein the thickness of the first tackiness adhesive layer is in the range of 1 μm to 3 μm.

[0023] [1-3] The optical laminate according to [1-1] or [1-2], wherein the refractive index N of the first adhesive layer is bI It is 1.48~1.54.

[0024] [1-4] The optical layered body according to any one of [1-1] to [1-3], wherein the refractive index of the second tackiness adhesive layer with respect to light of a wavelength of 589 nm is 1.50 to 1.57.

[0025] [1-5] The optical layered body according to any one of [1-1] to [1-4], wherein the storage modulus of the second adhesive layer at a temperature of 80° C. is 0.04 MPa or more.

[0026] [1-6] The optical layered body according to any one of [1-1] to [1-5], wherein the storage modulus of the first tackiness adhesive layer at a temperature of 80° C. is 0.02 GPa or more and 5 GPa or less.

[0027] A second aspect of the present invention provides the following optical layered body.

[0028] [2-1] An optical laminate, wherein a first protective film, an adhesive layer, a polarizing plate, an adhesive layer, a second protective film, a first adhesive bonding layer, a first liquid crystal retardation film, a second adhesive bonding layer, and a second liquid crystal retardation film are laminated adjacent to each other in this order,

[0029] The storage modulus of the first adhesive layer at a temperature of 80° C. is 0.4 GPa or more.

[0030] The first liquid crystal retardation film and the second liquid crystal retardation film satisfy the following formula (2) or formula (3):

[0031] nx>ny≥nz···(2)

[0032] nx<ny≤nz···(3),

[0033] The thickness of the second adhesive layer is 2.8 μm to 20 μm.

[0034] (In formula (2) and formula (3), nx represents the principal refractive index in the direction parallel to the plane of the first liquid crystal retardation film or the second liquid crystal retardation film in the refractive index ellipsoid formed by the first liquid crystal retardation film or the second liquid crystal retardation film, ny represents the refractive index in the direction parallel to the plane and orthogonal to the direction of nx in the refractive index ellipsoid, and nz represents the refractive index in the direction perpendicular to the plane in the refractive index ellipsoid.)

[0035] [2-2] The optical layered body according to [2-1], wherein the thickness of the first tackiness adhesive layer is in the range of 1 μm to 3 μm.

[0036] [2-3] The optical laminate according to [2-1] or [2-2], wherein the refractive index N of the first tackiness adhesive layer with respect to light of a wavelength of 589 nm is bI It is 1.48~1.54.

[0037] [2-4] The optical layered body according to any one of [2-1] to [2-3], wherein the refractive index of the second tackiness adhesive layer with respect to light of a wavelength of 589 nm is 1.50 to 1.57.

[0038] [2-5] The optical layered body according to any one of [2-1] to [2-4], wherein the storage modulus of the second adhesive layer at a temperature of 80° C. is 0.04 MPa or more.

[0039] Effects of the Invention

[0040] According to the first and second aspects of the present invention, there can be provided an optical laminate including a retardation plate having a plurality of liquid crystal retardation films, wherein unevenness when viewed from an oblique direction is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a schematic cross-sectional view schematically showing an example of the optical layered body according to the present embodiment.

[0042] Figure 2 It is a schematic cross-sectional view schematically showing a specific example of a phase difference plate.

[0043] Figure 3 This is a schematic diagram schematically showing a method of polishing the end surface of the optical layered body according to the present embodiment.

[0044] Figure 4 This is a schematic cross-sectional view schematically showing an example of the image display device according to this embodiment. DETAILED DESCRIPTION

[0045] The following describes the embodiments of the present invention with reference to the accompanying drawings, but the present invention is not limited to the following embodiments. In all the following drawings, the scales are appropriately adjusted to facilitate understanding of each component, and the scales of each component shown in the drawings are not necessarily consistent with the scales of the actual components.

[0046] [Optical laminate]

[0047] Figure 1 Schematic cross-sectional view schematically showing an example of the optical laminate of this embodiment. Figure 1 As shown, the optical laminate 1 is stacked with a first protective film 11, an adhesive layer 12, a polarizer 13, an adhesive layer 14, a second protective film 15, a first adhesive bonding layer 21, a first liquid crystal phase difference film 31, a second adhesive bonding layer 34, and a second liquid crystal phase difference film 32 in order from the front side. In this specification, the linear polarizing plate 10 is set as a laminate composed of the first protective film 11, the adhesive layer 12, the polarizer 13, the adhesive layer 14, and the second protective film 15. In this specification, the phase difference plate 30 is set as a laminate composed of the first liquid crystal phase difference film 31, the second adhesive bonding layer 34, and the second liquid crystal phase difference film 32. The optical laminate 1 may be a circular polarizing plate.

[0048] In the optical laminate 1, the refractive index of the second protective film with respect to light of a wavelength of 589 nm is N aII The refractive index of the first adhesive layer with respect to light of wavelength 589 nm is N bI When , the second protective film 15 and the first adhesive bonding layer 21 preferably satisfy the following formula (1).

[0049] |N aII -N bI |<0.1···(1)

[0050] In the optical layered body 1, by satisfying the above-mentioned formula (1), interference unevenness (Japanese: interference unevenness) viewed from an oblique direction can be reduced.

[0051] In the phase difference plate 30, the first liquid crystal phase difference film and the second liquid crystal phase difference film each independently satisfy the following formula (2) or formula (3):

[0052] nx>ny≥nz···(2)

[0053] nx<ny≤nz···(3).

[0054] (In formula (2) and formula (3), nx represents the principal refractive index in the direction parallel to the plane of the first liquid crystal retardation film or the second liquid crystal retardation film in the refractive index ellipsoid formed by the first liquid crystal retardation film or the second liquid crystal retardation film, ny represents the refractive index in the direction parallel to the plane and orthogonal to the direction of nx in the refractive index ellipsoid, and nz represents the refractive index in the direction perpendicular to the plane in the refractive index ellipsoid.)

[0055] That is, it is preferred that the first liquid crystal retardation film satisfies the formula (2), and the second liquid crystal retardation film satisfies the formula (3).

[0056] The first liquid crystal retardation film may satisfy the formula (3), and the second liquid crystal retardation film may satisfy the formula (2).

[0057] The first liquid crystal retardation film may satisfy the formula (2), and the second liquid crystal retardation film may satisfy the formula (2).

[0058] The first liquid crystal retardation film may satisfy the formula (3), and the second liquid crystal retardation film may satisfy the formula (3).

[0059] [First adhesive layer]

[0060] The first adhesive layer 21 is a bonding layer for bonding the phase difference plate 30 and the linear polarization plate 10 together.

[0061] The first adhesive bonding layer 21 is an adhesive layer formed using an adhesive composition or an adhesive layer formed using an adhesive composition. From the viewpoint of processability of the end surface of the optical laminate, an adhesive layer formed using an adhesive composition is preferred.

[0062] In the case where the first adhesive bonding layer 21 is an adhesive layer, from the viewpoint of handling in the laminating process, its thickness is preferably 2 μm or more, more preferably 3 μm or more, and more preferably 4 μm or more. In addition, it is preferably 30 μm or less, more preferably 20 μm or less, and more preferably 10 μm or less. In the case where the first adhesive bonding layer 21 is an adhesive layer, from the viewpoint of adhesion and curability, its thickness is preferably 0.1 μm or more, more preferably 0.4 μm or more, and more preferably 1 μm or more. In addition, for the same reason, it is preferably 5 μm or less, more preferably 4 μm or less, and more preferably 3 μm or less.

[0063] When the first adhesive bonding layer 21 is formed of an adhesive layer, the storage elastic modulus at a temperature of 80° C. may be 0.01 MPa or more and 0.8 MPa or less.

[0064] It is preferably 0.02 MPa or more and 0.4 MPa or less.

[0065] More preferably, it is 0.03 MPa or more and 0.2 MPa or less.

[0066] More preferably, it is 0.04 MPa or more and 0.1 MPa or less.

[0067] When the first adhesive layer 21 is formed of an adhesive layer, the storage elastic modulus at a temperature of 80° C. may be 0.01 GPa or more and 10 GPa or less.

[0068] Preferably, it is 0.02 GPa or more and 5 GPa or less.

[0069] More preferably, it is 0.1 GPa or more and 3 GPa or less.

[0070] More preferably, it is 0.5 GPa or more and 2 GPa or less. By making the storage modulus of the first adhesive layer 21 at a temperature of 80° C. be within the above range, it is easy to grind the end face of the optical laminate 1, and it is possible to reduce contamination when grinding the end face of the optical laminate 1. In this specification, the storage modulus of the first adhesive layer 21 can be measured by the method described in the examples described later.

[0071] When the first adhesive layer 21 is formed of an adhesive layer, the storage modulus at a temperature of 23° C. may be 0.01 MPa or more and 1 MPa or less.

[0072] It is preferably 0.02 MPa or more and 0.5 MPa or less.

[0073] More preferably, it is 0.03 MPa or more and 0.3 MPa or less.

[0074] More preferably, it is 0.05 MPa or more and 0.15 MPa or less.

[0075] When the first adhesive layer 21 is formed of an adhesive layer, the storage elastic modulus at a temperature of 23° C. may be 0.01 GPa or more and 10 GPa or less.

[0076] Preferably, it is 0.1 GPa or more and 5 GPa or less,

[0077] More preferably, it is 0.3 GPa or more and 4 GPa or less.

[0078] More preferably, it is 0.5 GPa or more and 3 GPa or less. By making the storage modulus of the first adhesive layer 21 at a temperature of 23° C. be within the above range, it is easy to grind the end face of the optical laminate 1, and it is possible to reduce contamination when grinding the end face of the optical laminate 1. In this specification, the storage modulus of the first adhesive layer 21 can be measured by the method described in the examples described later.

[0079] The refractive index N of the first adhesive layer 21 with respect to light of a wavelength of 589 nm is bI The refractive index N with respect to light of wavelength 589 nm is preferably 1.46 or more, more preferably 1.48 or more, and still more preferably 1.50 or more. bI By making the refractive index of the first adhesive layer 21 within the above range, the interference unevenness generated between the interface of the first liquid crystal phase difference film 31 and the first adhesive layer 21 and the interface of the second protective film 15 and the first adhesive layer 21 can be suppressed, and the interference unevenness observed from the tilt direction of the optical laminate 1 can be further reduced.

[0080] The first adhesive layer 21 is a bonding layer for bonding the phase difference plate 30 to the linear polarizing plate 10. It is believed that if the storage modulus of the first adhesive layer 21 at a temperature of 80°C is 0.4 GPa or more, or even 0.6 GPa or more, when bonding the phase difference plate 30 to the linear polarizing plate 10, the slight deformation of the first adhesive layer 21 is suppressed, thereby the distance between the phase difference plate 30 and the linear polarizing plate 10 becomes uniform, and the unevenness observed from the oblique direction can be suppressed. The storage modulus of the first adhesive layer 21 at a temperature of 80°C is usually 1.2 GPa or less, preferably 1.0 GPa or less.

[0081] [Second adhesive layer]

[0082] The second adhesive bonding layer 34 is a layer responsible for the lamination of the first liquid crystal phase difference film 31 and the second liquid crystal phase difference film 32. The second adhesive bonding layer 34 is an adhesive layer formed using an adhesive composition or an adhesive layer formed using an adhesive composition. From the viewpoint of the processability of the end face of the optical laminate, it is preferably an adhesive layer formed using an adhesive composition. From the viewpoint of reducing the interference unevenness observed from the oblique direction, the thickness of the second adhesive bonding layer 34 is 2.8 μm or more, preferably 3.0 μm or more, and more preferably 3.2 μm or more. From the viewpoint of the processability and bending of the optical laminate, the thickness of the second adhesive bonding layer 34 is 20 μm or less, preferably 15 μm or less, more preferably 10 μm or less, and further preferably 7 μm or less. By making the thickness of the second adhesive bonding layer 34 the above range, the interference unevenness observed from the oblique direction of the optical laminate 1 can be reduced.

[0083] When the second adhesive bonding layer 34 is formed of an adhesive layer, the storage elastic modulus at a temperature of 80° C. may be 0.01 MPa or more and 0.8 MPa or less.

[0084] It is preferably 0.02 MPa or more and 0.4 MPa or less.

[0085] More preferably, it is 0.03 MPa or more and 0.2 MPa or less.

[0086] More preferably, it is 0.04 MPa or more and 0.1 MPa or less.

[0087] The second adhesive layer 34 may be formed of an adhesive layer and the storage elastic modulus at a temperature of 80° C. may be 0.001 GPa or more and 5 GPa or less.

[0088] Preferably, it is 0.005 GPa or more and 3 GPa or less.

[0089] More preferably, it is 0.1 GPa or more and 1 GPa or less.

[0090] More preferably, it is 0.02 GPa or more and 0.5 GPa or less. By making the storage modulus of the second adhesive layer 34 at a temperature of 80° C. be within the above range, it is easy to grind the end face of the optical laminate 1, and it is possible to reduce contamination when grinding the end face of the optical laminate 1. In this specification, the storage modulus of the second adhesive layer 34 can be measured by the method described in the examples described later.

[0091] When the second adhesive bonding layer 34 is formed of an adhesive layer, the storage elastic modulus at a temperature of 23° C. may be 0.01 MPa or more and 1 MPa or less.

[0092] It is preferably 0.02 MPa or more and 0.5 MPa or less.

[0093] More preferably, it is 0.03 MPa or more and 0.3 MPa or less.

[0094] More preferably, it is 0.05 MPa or more and 0.15 MPa or less.

[0095] The second adhesive layer 34 may be formed of an adhesive layer and have a storage elastic modulus of 0.01 GPa or more and 10 GPa or less at a temperature of 23° C.

[0096] Preferably, it is 0.1 GPa or more and 5 GPa or less,

[0097] More preferably, it is 0.3 GPa or more and 4 GPa or less.

[0098] It is further preferably above 0.5 GPa and below 3 GPa. By making the storage modulus of the second adhesive layer 34 at a temperature of 23°C within the above range, it is easy to grind the end face of the optical laminate 1. In addition, the contamination when the end face of the optical laminate 1 is grinded can be reduced. In this specification, the storage modulus of the second adhesive layer 34 can be measured by the method described in the embodiments described later. The method for measuring the storage modulus of the second adhesive layer 34 is different on the adhesive layer and the adhesive layer as shown in the embodiments described later.

[0099] The refractive index of the second adhesive bonding layer 34 relative to the light of wavelength 589nm is preferably 1.48 or more, more preferably 1.50 or more, and further preferably 1.52 or more. The refractive index relative to the light of wavelength 589nm is preferably 1.59 or less, more preferably 1.57 or less, and further preferably 1.55 or less. By making the refractive index of the second adhesive bonding layer 34 be the above range, the interference unevenness generated between the interface of the first liquid crystal phase difference film 31 and the second adhesive bonding layer 34 and the interface of the second liquid crystal phase difference film 32 and the second adhesive bonding layer 34 can be suppressed, and the interference unevenness observed from the tilt direction of the optical stack 1 can be further reduced. In addition, the reflectivity of the optical stack 1 can be reduced.

[0100] The second adhesive bonding layer 34 is preferably an adhesive layer from the viewpoint of easily forming an adhesive composition that satisfies the above-mentioned numerical range of the storage elastic modulus more than an adhesive composition.

[0101] <Adhesive composition>

[0102] In the optical laminate 1, the adhesive composition can be used as a material for forming the adhesive layer 12, the adhesive layer 14, the first adhesive bonding layer 21, and the second adhesive bonding layer 34. As the adhesive composition, for example, there can be mentioned: an aqueous adhesive composition, a curable adhesive composition cured by heating or irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, etc. As the aqueous adhesive composition, for example, there can be mentioned: a composition formed by dissolving a polyvinyl alcohol resin or a carbamate resin as a main component in water, and a composition formed by dispersing a polyvinyl alcohol resin or a carbamate resin as a main component in water. The aqueous adhesive composition may further contain curable components such as polyaldehydes, melamine compounds, zirconium oxide compounds, zinc compounds, glyoxal compounds, and water-soluble epoxy resins, and crosslinking agents. Examples of the water-based adhesive composition include the adhesive composition described in JP-A-2010-191389, the adhesive composition described in JP-A-2011-107686, the composition described in JP-A-2020-172088, and the composition described in JP-A-2005-208456.

[0103] The curable adhesive composition is preferably an active energy ray-curable adhesive composition that contains a curable (polymerizable) compound as a main component and is cured by irradiation with active energy rays. Examples of the active energy ray-curable adhesive composition include a cationic polymerizable adhesive composition containing a cationic polymerizable compound as a curable compound, a free radical polymerizable adhesive composition containing a free radical polymerizable compound as a curable compound, and a mixed adhesive composition containing both a cationic polymerizable compound and a free radical polymerizable compound as curable compounds.

[0104] The cationically polymerizable compound is a compound or oligomer that is cured by cation polymerization reaction when irradiated with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays or heated, and specific examples thereof include epoxy compounds, oxetane compounds, and vinyl compounds.

[0105] Examples of epoxy compounds include alicyclic epoxy compounds (compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule) such as 3,4-epoxycyclohexylmethyl 3',4'-epoxycyclohexylcarboxylate; aromatic epoxy compounds (compounds having an aromatic ring and an epoxy group in the molecule) such as diglycidyl ether of bisphenol A; and aliphatic epoxy compounds (compounds having at least one oxirane ring bonded to an aliphatic carbon atom in the molecule) such as 2-ethylhexyl glycidyl ether and 1,4-butanediol diglycidyl ether.

[0106] Examples of the oxetane compound include compounds having one or more oxetane rings in the molecule, such as 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane.

[0107] The cationic polymerization adhesive composition preferably contains a cationic polymerization initiator. The cationic polymerization initiator may be a thermal cationic polymerization initiator or a photocationic polymerization initiator. Examples of cationic polymerization initiators include aromatic diazonium salts such as benzene diazonium hexafluoroantimonate; aromatic iodonium salts such as diphenyl iodonium tetrakis (pentafluorophenyl) borate; aromatic sulfonium salts such as triphenyl sulfonium hexafluorophosphate; iron-aromatic complexes such as ditoluene-cyclopentadienyl iron (II) hexafluoroantimonate, etc. The content of the cationic polymerization initiator is generally 0.1 to 10 parts by mass relative to 100 parts by mass of the cationic polymerization compound. Two or more cationic polymerization initiators may be included.

[0108] Examples of the cationic polymerizable adhesive composition include cationic polymerizable compositions described in JP-A-2016-126345, WO-2019 / 10315, and JP-A-2021-113969.

[0109] The free radical polymerizable compound is a compound or oligomer that is cured by free radical polymerization reaction by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, or heating, and specifically, a compound having an ethylenically unsaturated bond can be cited. As the compound having an ethylenically unsaturated bond, a (meth)acrylic compound having one or more (meth)acryloyl groups in the molecule, a vinyl compound having one or more vinyl groups in the molecule, etc. can be cited.

[0110] Examples of the (meth)acrylic compound include (meth)acrylic oligomers having at least two (meth)acrylic groups in a molecule obtained by reacting two or more (meth)acrylic acid ester monomers, (meth)acrylamide monomers, and functional group-containing compounds. In the present specification, the (meth)acrylic group may be either an acryloyl group or a methacryloyl group.

[0111] The radical polymerization adhesive composition preferably contains a radical polymerization initiator. The radical polymerization initiator may be a thermal radical polymerization initiator or a photoradical polymerization initiator. Examples of the radical polymerization initiator include: acetophenone-based initiators such as acetophenone and 3-methylacetophenone; benzophenone-based initiators such as benzophenone, 4-chlorobenzophenone, and 4,4'-diaminobenzophenone; benzoin ether-based initiators such as benzoin propyl ether and benzoin ethyl ether; thioxanthone-based initiators such as 4-isopropylthioxanthone; xanthone, fluorenone, etc. The content of the radical polymerization initiator is generally 0.1 to 10 parts by mass relative to 100 parts by mass of the radical polymerizable compound. Two or more radical polymerization initiators may be included.

[0112] Examples of the radical polymerizable adhesive composition include radical polymerizable compositions described in JP-A-2016-126345, JP-A-2016-153474, and International Publication No. 2017 / 183335.

[0113] The active energy ray-curable adhesive composition may contain additives such as ion trapping agents, antioxidants, chain transfer agents, tackifiers, thermoplastic resins, fillers, flow regulators, plasticizers, defoamers, antistatic agents, leveling agents, and solvents as necessary.

[0114] The bonding of the first liquid crystal retardation film 31 and the second liquid crystal retardation film 32 using an adhesive layer can be performed as follows: an adhesive composition is applied on at least one bonding surface selected from each of the two layers, the two are overlapped with the aid of the coated layer of the adhesive composition, and after being bonded together by pressing from top and bottom using a bonding roller, they are irradiated with active energy rays to cure, or heated to cure.

[0115] Before forming the coating layer of the adhesive layer, at least one of the bonding surfaces of the two layers may be subjected to an adhesion-facilitating treatment such as saponification treatment, corona treatment, plasma treatment, primer treatment, anchor coating treatment, etc.

[0116] The coating layer of the adhesive composition can be formed by various coating methods such as a die coater, a comma coater, a gravure coater, a wire bar coater, and a knife coater.

[0117] The light irradiation intensity during irradiation with active energy rays is determined according to the composition of the active energy ray-curable adhesive composition and is not particularly limited, but is preferably 10 mW / cm 2 Above and 1000mW / cm 2 It should be noted that the irradiation intensity is preferably an intensity in the wavelength region effective for the activation of the photocationic polymerization initiator or the photoradical polymerization initiator. The irradiation is performed once or multiple times with such a light irradiation intensity, and the accumulated light amount is preferably set to 10 mJ / cm2 More preferably, 100 mJ / cm 2 Above and 1000mJ / cm 2 the following.

[0118] The light source used for polymerizing and curing the active energy ray-curable adhesive composition is not particularly limited, and examples thereof include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, halogen lamps, chemical lamps, black light lamps, microwave-excited mercury lamps, and metal halide lamps.

[0119] <Adhesive composition>

[0120] In the optical laminate 1, the adhesive composition can be used as a material for forming the first adhesive bonding layer 21 and the second adhesive bonding layer 34. As the adhesive composition, there can be used any adhesive composition with excellent optical transparency known in the past without particular limitation, for example, an adhesive composition with base polymers such as acrylic resin, urethane resin, silicone resin, polyvinyl ether resin, etc. can be used. In addition, it can also be an active energy ray-curable adhesive composition, a thermosetting adhesive composition, etc. Among them, an adhesive composition with an acrylic resin having excellent transparency, adhesion, re-peelability, weather resistance, heat resistance, etc. as a base polymer is suitable.

[0121] The adhesive composition may further include a cross-linking agent, a silane compound, an antistatic agent, and the like.

[0122] ((Meth)acrylic resin)

[0123] The (meth)acrylic resin contained in the adhesive composition is preferably a polymer (hereinafter also referred to as a "(meth)acrylate polymer") having a structural unit derived from an alkyl (meth)acrylate represented by the following formula (I) (hereinafter also referred to as "structural unit (I)") as a main component (for example, containing 50 parts by mass or more relative to 100 parts by mass of the structural unit of the (meth)acrylic resin).

[0124] In addition, in this specification, a (meth)acrylic resin may be either an acrylic resin or a methacrylic resin, and "(meth)" of (meth)acrylate etc. has the same meaning.

[0125]

[0126] [Where R 10 represents a hydrogen atom or a methyl group, R 20 It represents an alkyl group having 1 to 20 carbon atoms, the alkyl group may have any structure of linear, branched or cyclic, and the hydrogen atoms of the alkyl group may be substituted by an alkoxy group having 1 to 10 carbon atoms.]

[0127] Examples of the (meth)acrylate represented by formula (X) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, stearyl (meth)acrylate, and tert-butyl (meth)acrylate. Specific examples of the alkyl acrylate containing an alkoxy group include 2-methoxyethyl (meth)acrylate and ethoxymethyl (meth)acrylate. Among them, it is preferable to contain n-butyl (meth)acrylate or 2-ethylhexyl (meth)acrylate, and it is particularly preferable to contain n-butyl (meth)acrylate.

[0128] The (meth)acrylate polymer may contain structural units derived from other monomers in addition to the structural unit (I). The structural units derived from other monomers may be one or more. Other monomers that may be contained in the (meth)acrylate polymer include monomers having polar functional groups, monomers having aromatic groups, and acrylamide monomers.

[0129] Examples of the monomer having a polar functional group include (meth)acrylates having a polar functional group. Examples of the polar functional group include: hydroxyl groups; carboxyl groups; substituted or unsubstituted amino groups substituted with alkyl groups having 1 to 6 carbon atoms; heterocyclic groups such as epoxy groups, and the like.

[0130] The content of the structural unit derived from the monomer having a polar functional group in the (meth)acrylate polymer is preferably 10 parts by mass or less, more preferably 0.5 parts by mass or more and 10 parts by mass or less, further preferably 0.5 parts by mass or more and 5 parts by mass or less, particularly preferably 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of all structural units of the (meth)acrylate polymer.

[0131] Examples of monomers having an aromatic group include (meth)acrylates having one (meth)acryloyl group and one or more aromatic rings (e.g., benzene ring, naphthalene ring, etc.) in the molecule and having a phenyl group, a phenoxyethyl group, or a benzyl group. By including these structural units, the whitening phenomenon of the optical laminate produced under high temperature and high humidity environments can be suppressed.

[0132] The content of the structural unit derived from the monomer having an aromatic group in the (meth)acrylate polymer is preferably 20 parts by mass or less, more preferably 4 parts by mass or more and 20 parts by mass or less, and further preferably 4 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of all structural units of the (meth)acrylate polymer.

[0133] Examples of acrylamide monomers include N-(methoxymethyl)acrylamide, N-(ethoxymethyl)acrylamide, N-(propoxymethyl)acrylamide, N-(butoxymethyl)acrylamide, and N-(2-methylpropoxymethyl)acrylamide. By including these structural units, the bleeding of additives such as antistatic agents described below can be suppressed.

[0134] Furthermore, as structural units derived from other monomers other than the structural unit (I), structural units derived from styrene-based monomers, structural units derived from vinyl-based monomers, and structural units derived from monomers having a plurality of (meth)acryloyl groups in the molecule may be included.

[0135] The weight average molecular weight (hereinafter, also referred to as "Mw") of the (meth)acrylic resin (1) is preferably 500,000 to 2.5 million. If the weight average molecular weight is 500,000 or more, the durability of the first adhesive layer in a high temperature and high humidity environment can be improved. If the weight average molecular weight is 2.5 million or less, the operability when applying a coating liquid containing an adhesive composition becomes good. The molecular weight distribution (Mw / Mn) represented by the ratio of the weight average molecular weight (Mw) to the number average molecular weight (hereinafter, also referred to as "Mn") is generally 2 to 10. In this specification, "weight average molecular weight" and "number average molecular weight" are polystyrene conversion values ​​measured by gel permeation chromatography (GPC).

[0136] When the (meth)acrylic resin is dissolved in ethyl acetate to prepare a solution having a concentration of 20% by mass, the viscosity at 25° C. is preferably 20 Pa·s or less, and more preferably 0.1 to 15 Pa·s. If the viscosity at 25° C. of the (meth)acrylic resin is within the above range, it helps to improve the durability and reworkability of the optical laminate including the adhesive layer formed using the resin. The above viscosity can be measured by a Brookfield viscometer.

[0137] The glass transition temperature (Tg) of the (meth)acrylic resin is, for example, -60 to 20° C., preferably -50 to 15° C., more preferably -45 to 10° C., and further preferably -40 to 0° C. The glass transition temperature can be measured by a differential scanning calorimeter (DSC).

[0138] The (meth)acrylic resin may contain two or more (meth)acrylate polymers. Examples of such (meth)acrylate polymers include (meth)acrylate polymers having a relatively low molecular weight, such as a structural unit (I) derived from the above (meth)acrylate as a main component and a weight average molecular weight in the range of 50,000 to 300,000.

[0139] (Meth) acrylic resins can be generally produced by known polymerization methods such as solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization. In the production of (meth) acrylic resins, polymerization is generally carried out in the presence of a polymerization initiator. The amount of the polymerization initiator used is generally 0.001 to 5 parts by mass relative to a total of 100 parts by mass of all monomers constituting the (meth) acrylic resin. (Meth) acrylic resins can also be produced by a method of polymerization using active energy rays such as ultraviolet rays.

[0140] (Crosslinking agent)

[0141] The adhesive composition preferably contains a crosslinking agent. As the crosslinking agent, conventional crosslinking agents (such as isocyanate compounds, epoxy compounds, aziridine compounds, metal chelate compounds, peroxides, etc.) can be cited, and isocyanate compounds are preferred from the viewpoints of the application period of the adhesive composition, the crosslinking speed, and the durability of the polarizing plate.

[0142] Isocyanate compounds are compounds having at least two isocyanate groups (-NCO) in the molecule. Specifically, toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, naphthalene diisocyanate, triphenylmethane triisocyanate, etc. can be mentioned. In addition, adducts obtained by reacting these isocyanate compounds with polyols such as glycerol and trimethylolpropane, dimers and trimers of these isocyanate compounds can also be mentioned. Two or more isocyanate compounds can be combined.

[0143] The ratio of the cross-linking agent relative to 100 parts by mass of the (meth)acrylic resin is, for example, 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 1 part by mass.

[0144] (Silane compound)

[0145] The adhesive composition may further contain a silane compound.

[0146] Examples of the silane compound include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylethoxydimethylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane.

[0147] In addition, the silane compound may contain an oligomer derived from the above-mentioned silane compound.

[0148] The content of the silane compound in the adhesive composition is usually 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the (meth)acrylic resin. If the content of the silane compound is 0.01 parts by mass or more, there is a tendency for the adhesion between the adhesive layer and the adherend to be improved, and if the content is 10 parts by mass or less, there is a tendency for the oozing out of the silane compound from the adhesive layer to be suppressed.

[0149] (Antistatic Agent)

[0150] The adhesive composition may further include an antistatic agent. As the antistatic agent, known antistatic agents can be mentioned, and ionic antistatic agents are suitable. As cationic components constituting the ionic antistatic agent, organic cations and inorganic cations can be mentioned. As organic cations, pyridinium cations, imidazolium cations, ammonium cations, sulfonium cations, phosphonium cations, etc. can be mentioned. As inorganic cations, alkali metal cations such as lithium cations, potassium cations, sodium cations, and cesium cations, and alkaline earth metal cations such as magnesium cations and calcium cations can be mentioned. As anionic components constituting the ionic antistatic agent, any of inorganic anions and organic anions can be mentioned. From the perspective of excellent antistatic performance, anionic components containing fluorine atoms are preferred. As anionic components containing fluorine atoms, hexafluorophosphate anions (PF6 - ), bis(trifluoromethanesulfonyl)imide anion [(CF3SO2)2N - ]、bis(fluorosulfonyl)imide anion [(FSO2)2N - ] anions, etc.

[0151] From the viewpoint of excellent temporal stability of the antistatic performance of the pressure-sensitive adhesive composition, an ionic antistatic agent that is solid at room temperature is preferred.

[0152] The content of the antistatic agent is, for example, 0.01 to 20 parts by mass, preferably 0.1 to 10 parts by mass, and more preferably 1 to 7 parts by mass, relative to 100 parts by mass of the (meth)acrylic resin.

[0153] The adhesive composition may contain additives such as a UV absorber, a solvent, a crosslinking catalyst, a tackifying resin (tackifier), and a plasticizer, either alone or in combination of two or more. In addition, a method of incorporating a UV curable compound into the adhesive composition, irradiating UV rays after forming the adhesive layer to cure it, and making the adhesive layer harder is also useful.

[0154] The adhesive layer can be formed, for example, by dissolving or dispersing the above adhesive composition in a solvent to form a solvent-containing adhesive composition, and then coating the surface of the layer where the adhesive layer is to be provided and drying it.

[0155] [Linear polarizing plate]

[0156] The linear polarizing plate 10 is a film having the function of light absorption anisotropy, and is usually a film including a polarizing film (Japanese: 偏光フィルム) in which dichroic pigments are uniaxially oriented and a polarizer 13 including a polarizing film (Japanese: 偏光膜). In order to uniaxially orient the dichroic pigments, it can be made from a film formed by uniaxially stretching a polymer such as PVA impregnated with iodine or an organic dichroic dye, or a polarizing film formed by orienting a dichroic pigment and a polymerizable liquid crystal compound. That is, by utilizing the dichroic pigments contained in the polymer obtained by stretching the polymer or the polymerizable liquid crystal compound, light anisotropy absorption is performed, thereby exhibiting a polarization function.

[0157] The polarization performance of the linear polarizing plate can be measured using a spectrophotometer. For example, in the visible light range of wavelengths 380 nm to 780 nm, using a device equipped with a prism polarizer on a spectrophotometer, the transmittance (T1) in the transmission axis direction (orientation perpendicular direction) and the transmittance (T2) in the absorption axis direction (orientation direction) can be measured by the double beam method. Regarding the polarization performance in the visible light range, the monomer transmittance and degree of polarization at each wavelength are calculated using the following formulas (Formula 1) and (Formula 2), and further, the visibility (Japanese: 視感度) correction is performed using the 2-degree field of view (C light source) of JIS Z 8701, whereby the visibility-corrected monomer transmittance (Ty) and visibility-corrected degree of polarization (Py) can be calculated. In addition, based on the transmittance measured in the same way, the chromaticity a * a * b * in the (CIE) color system * and b *, thereby obtaining the color tone of the linear polarizing plate alone (single color tone), the color tone of the linear polarizing plates arranged in parallel (parallel color tone), and the color tone of the linear polarizing plates arranged orthogonally (orthogonal color tone). * and b * The closer the value is to 0, the more neutral the color tone can be judged to be.

[0158] Single body transmittance (%) = (T1 + T2) / 2 (Formula 1)

[0159] Polarization degree (%) = (T1-T2) / (T1+T2)×100 (Formula 2)

[0160] The visibility correction polarization degree Py of the linear polarizing plate is usually 80% or more, preferably 90% or more, more preferably 95% or more, further preferably 98% or more, particularly preferably 99% or more, and if it is 99.9% or more, it can be suitably used in a liquid crystal display. Increasing the visibility correction polarization degree Py of the linear polarizing plate is advantageous in improving the anti-reflection function of the optical laminate. If the visibility correction polarization degree Py is less than 80%, the anti-reflection function when used as an anti-reflection film may not be exerted.

[0161] The higher the visibility correction single transmittance Ty of the linear polarizing plate, the higher the clarity of the white display. However, from the relationship between (Formula 1) and (Formula 2), if the single transmittance is excessively increased, there is a problem of reduced polarization degree. Therefore, it is preferably 30% or more and 60% or less, more preferably 35% or more and 55% or less, further preferably 38% or more and 50% or less, and further preferably 40% or more and 45% or less. If the visibility correction single transmittance Ty is too high, the visibility correction polarization degree Py becomes too low, and sometimes the anti-reflection function when used as an anti-reflection film becomes insufficient.

[0162] The linear polarizing plate includes a first protective film 11 and a second protective film 15 on both sides of a polarizer 13. As the protective films 11 and 15, thermoplastic resin films can be used. The polarizer 13 and the protective films 11 and 15 are laminated with the aid of an adhesive layer. In order to improve the adhesion with the polarizer 13, the film formed of the thermoplastic resin may be subjected to a surface treatment (e.g., a corona treatment, etc.), or a thin layer such as a primer layer (also referred to as an undercoat layer) may be formed.

[0163] Thermoplastic resins constituting the thermoplastic resin film are preferably transparent films, and examples thereof include: cellulose resins such as triacetyl cellulose; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polyethersulfone resins; polysulfone resins; polycarbonate resins; polyamide resins such as nylon and aromatic polyamide; polyimide resins; polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers; cyclic polyolefin resins having a ring system and a norbornene structure (also referred to as norbornene resins); (meth)acrylic resins; polyarylate resins; polystyrene resins; polyvinyl alcohol resins, etc. Among them, the thermoplastic resin film is preferably a cyclic polyolefin resin film, a cellulose ester resin film, a polyester resin film, or a (meth)acrylic resin film. Among them, as the protective films 11, 15, from the viewpoint of the balance between optical properties, processability and economy, preferably, a resin film comprising a cellulose resin such as triacetyl cellulose and a cyclic polyolefin resin having a ring system and norbornene structure is used. In particular, as the second protective film 15, from the viewpoint of the refractive index, a triacetyl cellulose (TAC) film is preferably used.

[0164] The thickness of the protective films 11 and 15 is preferably 3 μm to 60 μm, more preferably 5 μm to 40 μm, and even more preferably 10 μm to 30 μm.

[0165] The protective films 11 and 15 may be formed with a hard coating on the thermoplastic resin film. The hard coating may be formed on one side of the thermoplastic resin film or on both sides. By providing a hard coating, a thermoplastic resin film with improved hardness and scratch resistance can be made. The hard coating is, for example, an active energy ray-curable resin, preferably a cured layer of an ultraviolet-curable resin. As ultraviolet-curable resins, for example: (meth) acrylic resins, silicone resins, polyester resins, urethane resins, amide resins, epoxy resins, etc. can be cited. In order to increase the strength, the hard coating may contain additives. The additives are not particularly limited, and inorganic particles, organic particles or mixtures thereof can be cited.

[0166] The adhesive layer used for laminating the polarizer 13 with the protective films 11 and 15 is formed using the above-mentioned adhesive composition. As the adhesive composition, for example, a water-based adhesive composition, a curable adhesive composition cured by heating or irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, etc., can be cited. In the case of using a water-based adhesive composition, from the viewpoint of adhesion and processability, the film thickness is preferably in the range of 0.01 μm to 1.0 μm, more preferably in the range of 0.02 μm to 0.5 μm, and further preferably in the range of 0.03 μm to 0.3 μm.

[0167] Regarding the second protective film 15, when its refractive index with respect to light of a wavelength of 589 nm is N aIIWhen the refractive index N of the first adhesive layer with respect to light of wavelength 589 nm is bI The absolute value of the difference preferably satisfies the following formula (1):

[0168] |N aII -N bI |<0.1···(1).

[0169] From the perspective of further reducing the interference unevenness observed from an oblique direction, N aII With N bI The absolute value of the difference is preferably 0.08 or less, more preferably 0.06 or less, and further preferably 0.04 or less.

[0170] The refractive index N of the second protective film 15 is aII The refractive index N with respect to light of wavelength 589 nm is preferably 1.46 or more, more preferably 1.47 or more, and still more preferably 1.48 or more. aII By setting the refractive index of the protective film 15 to the above range, the interference unevenness generated between the interface of the second protective film 15 and the first adhesive layer 21 can be suppressed, and the interference unevenness observed from the tilt direction of the optical laminate 1 can be further reduced.

[0171] <Polarizing film>

[0172] Polarizing films, i.e. films uniaxially stretched in a state where iodine and an organic dichroic dye are impregnated in a polymer such as a polyvinyl alcohol resin film (PVA), can generally be manufactured through the following steps: a step of uniaxially stretching the polyvinyl alcohol resin film; a step of dyeing the polyvinyl alcohol resin film with a dichroic dye such as iodine to adsorb the dichroic dye; a step of treating the polyvinyl alcohol resin film adsorbed with the dichroic dye with a crosslinking agent such as an aqueous boric acid solution; and a step of washing with water after the treatment with a crosslinking agent such as an aqueous boric acid solution. The polarizing film may contain a crosslinking agent.

[0173] The thickness of the polarizing film is usually 30 μm or less, preferably 18 μm or less, more preferably 15 μm or less, and further preferably 10 μm or less. The thickness is usually 1 μm or more, for example 5 μm or more.

[0174] The uniaxial stretching of the polyvinyl alcohol resin film can be performed before dyeing with a dichroic dye, simultaneously with dyeing, or after dyeing. When the uniaxial stretching is performed after dyeing, the uniaxial stretching can be performed before the boric acid treatment or during the boric acid treatment. Of course, the uniaxial stretching can also be performed in multiple stages as shown here. The uniaxial stretching can be performed by: a method of uniaxially stretching along the film conveying direction between rollers with different peripheral speeds; a method of uniaxially stretching along the film conveying direction using a hot roller; a method of stretching along the width direction using a tenter, etc. In addition, the uniaxial stretching can be performed by dry stretching in the atmosphere, or by wet stretching in a state where the polyvinyl alcohol resin film is swollen using a solvent such as water. The stretching ratio is generally about 3 to 8 times. In addition, a coating containing The solution is then dried and stretched together with the thermoplastic resin film by the above-mentioned method.

[0175] The polyvinyl alcohol-based resin film can be dyed with a dichroic dye by, for example, immersing the polyvinyl alcohol-based resin film in an aqueous solution containing the dichroic dye. Specifically, iodine and a dichroic organic dye can be used as the dichroic dye.

[0176] <Polarizing film>

[0177] Polarizing films, i.e., optically anisotropic layers comprising polymers of polymerizable liquid crystal compounds containing dichroic dyes, can be suitably used, for example, for flexible displays, from the viewpoints of being able to arbitrarily control color tones, being able to be significantly thinned, and being non-contractile due to the absence of stretching and relaxation caused by heat.

[0178] The polarizing film is formed by coating a polarizing film-forming composition on an oriented film formed on a substrate as needed, and orienting the dichroic pigment contained in the above-mentioned polarizing film-forming composition. The polarizing film is a film having a thickness of 0.1 μm or more and 5 μm or less, more preferably 0.3 μm or more and 4 μm or less, and further preferably 0.5 μm or more and 3 μm or less. If the film thickness is thinner than this range, the desired light absorption may not be obtained sometimes, and if the film thickness is thicker than this range, there is a tendency that the orientation restriction force based on the oriented film is reduced and orientation defects are easily generated. In addition, the polarizing film-forming composition may further include a solvent, a photopolymerization initiator, a photosensitizer, an inhibitor, a leveling agent, and an adhesion improver.

[0179] In the case of an optically anisotropic layer in which the dichroic dye and the polymerizable liquid crystal compound are horizontally oriented relative to the substrate surface, the ratio of the absorbance A1(λ) in the orientation direction of light of wavelength λnm to the absorbance A2(λ) in the vertical direction in the orientation plane (dichroic ratio) is preferably 7 or more, more preferably 20 or more, and further preferably 40 or more. The higher the value, the more excellent the absorption selectivity of the polarizing plate. Although it also depends on the type of dichroic dye, in the case of a liquid crystal cured film cured in a nematic liquid crystal phase, it is about 5 to 10.

[0180] By mixing two or more dichroic pigments with different absorption wavelengths, polarizing films of various hues can be produced, and polarizing films with absorption in the entire visible light region can be produced. By producing polarizing films with such absorption characteristics, they can be used in various applications.

[0181] <Polarizing film; polymerizable liquid crystal compound>

[0182] A polymerizable liquid crystal compound refers to a compound having a polymerizable group and having liquid crystal properties (hereinafter, also referred to as a polymerizable liquid crystal). A polymerizable group refers to a group participating in a polymerization reaction, preferably a photopolymerizable group. Here, a photopolymerizable group refers to a group that can participate in a polymerization reaction by an active free radical, an acid, etc. generated by a photopolymerization initiator described later. As a polymerizable group, there can be cited: vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, oxetane, etc. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxirane and oxetane are preferred, and methacryloyloxy or acryloyloxy are more preferred. Liquid crystal properties can be thermotropic liquid crystals or lyotropic liquid crystals. When mixed with a dichroic pigment described later, thermotropic liquid crystals are preferred. A polymerizable liquid crystal compound can be a monomer or a polymer polymerized above a dimer.

[0183] In the case where the polymerizable liquid crystal compound is a thermotropic liquid crystal, it may be a thermotropic liquid crystal compound showing a nematic liquid crystal phase, or it may be a thermotropic liquid crystal compound showing a smectic liquid crystal phase. From the viewpoint of being able to present high dichroism, the liquid crystal state displayed by the polymerizable liquid crystal compound is preferably a smectic phase, and if it is a high-order smectic phase, it is more preferred from the viewpoint of high performance. Among them, it is more preferred to form a high-order smectic liquid crystal compound of smectic B phase, smectic D phase, smectic E phase, smectic F phase, smectic G phase, smectic H phase, smectic I phase, smectic J phase, smectic K phase or smectic L phase, and it is further preferred to form a high-order smectic liquid crystal compound of smectic B phase, smectic F phase or smectic I phase. If the liquid crystal phase formed by the polymerizable liquid crystal is these high-order smectic phases, a polarizing film with higher polarization performance can be manufactured. In addition, in the X-ray diffraction measurement, a polarizing film with high polarization performance can obtain Bragg peaks of high-order structures such as hexagonal phases (Japanese: hexagonal phases) and crystalline phases. The Bragg peak is a peak of a periodic structure derived from molecular orientation, and its periodic interval can be obtained as From the viewpoint of obtaining higher polarization characteristics, the polarizing film of the present invention preferably includes a polymer of a polymerizable liquid crystal in which the polymerizable liquid crystal is oriented in a smectic phase.

[0184] As a polymerizable liquid crystal compound, one may be used alone or in combination with two or more. As long as the effect of the present invention is not impaired, the polymerizable liquid crystal composition comprising other compounds described later may also include other polymerizable liquid crystal compounds other than the polymerizable liquid crystal compound, and from the viewpoint of obtaining a polarizing film with a high degree of orientation order, the polymerizable liquid crystal compound is preferably 51% by mass or more relative to the total mass of all polymerizable liquid crystal compounds contained in the polymerizable liquid crystal composition, more preferably 70% by mass or more, and further preferably 80% by mass or more.

[0185] Relative to the solid content of the polymerizable liquid crystal composition, the content of the polymerizable liquid crystal compound in the polarizing film forming composition of the present invention is preferably 40 to 99.9% by mass, more preferably 60 to 99% by mass, and further preferably 70 to 99% by mass. If the content of the polymerizable liquid crystal compound is within the above range, there is a tendency for the orientation of the polymerizable liquid crystal compound to become higher. It should be noted that in this specification, the solid content refers to the total amount of the components after removing the solvent from the polymerizable liquid crystal composition.

[0186] <Polarizing film; Dichroic pigment>

[0187] A dichroic pigment refers to a pigment having a property that the absorbance in the long axis direction of the molecule is different from the absorbance in the short axis direction. As a dichroic pigment, it is preferred to have the characteristic of absorbing visible light, and more preferably to have an absorption maximum wavelength (λMAX) in the range of 380 to 680 nm. As such a dichroic pigment, for example, acridine pigments, oxazine pigments, cyanine pigments, naphthalene pigments, azo pigments and anthraquinone pigments, etc., among which azo pigments are preferred. As azo pigments, monoazo pigments, disazo pigments, triazo pigments, tetrazo pigments and stilbene azo pigments, etc., are preferred, disazo pigments and triazo pigments. The dichroic pigment can be used alone or in combination. In order to be absorbed in the entire visible light region, it is preferred to combine two or more dichroic pigments, and it is more preferred to combine three or more dichroic pigments.

[0188] Examples of the azo dye include compounds represented by formula (I) (hereinafter, sometimes referred to as “compound (I)”).

[0189] T 1 -A 1 (-N=NA 2 ) p -N=NA 3 -T 2 (I)

[0190] [In formula (I), A 1 and A 2 and A 3 each independently represents a 1,4-phenylene group which may have a substituent, a naphthalene-1,4-diyl group which may have a substituent, a benzoic acid phenyl ester group which may have a substituent, a 4,4'-diphenylvinylene group which may have a substituent, or a divalent heterocyclic group which may have a substituent, 1 and T 2 is an electron withdrawing group or an electron donating group, and is substantially located at 180° relative to the azo bond plane. p represents an integer of 0 to 4. When p is 2 or more, each A 2 They may be the same or different from each other. In the range showing absorption in the visible region, the -N=N- bond may be replaced by -C=C-, -COO-, -NHCO-, or -N=CH- bonds.]

[0191] From the viewpoint of obtaining good light absorption characteristics, the content of the dichroic pigment (the total amount when multiple types are included) is usually 1 to 60 parts by mass, preferably 1 to 40 parts by mass, and more preferably 1 to 20 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. If the content of the dichroic pigment is less than this range, light absorption becomes insufficient and sufficient polarization performance cannot be obtained. If it is more than this range, the orientation of the liquid crystal molecules is sometimes hindered.

[0192] <Front layer>

[0193] The linear polarizing plate 10 may be provided with an antireflection layer at the front. The antireflection layer has a function of preventing the reflected light of the external light on the surface of the linear polarizing plate 10 from being observed, and can be formed by a conventional method of forming an antireflection layer, such as a coating method, a sputtering method, a vacuum evaporation method, etc. The antireflection layer may be formed in advance on the front side of a protective film provided on the front side of the linear polarizing plate 10, thereby constituting a linear polarizing plate with an antireflection layer using the protective film, or may be provided separately from the protective film.

[0194] The linear polarizing plate 10 may have a surface treatment layer other than the antireflection layer at the front. Examples of such a surface treatment layer include a hard coat layer, an anti-sticking layer, an anti-glare layer, and a diffusion layer.

[0195] [Phase difference plate]

[0196] The phase difference plate 30 has a first liquid crystal phase difference film 31 and a second liquid crystal phase difference film 32, and the first liquid crystal phase difference film 31 and the second liquid crystal phase difference film 32 contain a solidified material of a liquid crystal compound. The phase difference plate 30 may have a third liquid crystal phase difference film. The first liquid crystal phase difference film, the second liquid crystal phase difference film, and the third liquid crystal phase difference film may each be composed of two or more layers. In the following, the description applicable to any one of the first liquid crystal phase difference film 31, the second liquid crystal phase difference film 32, and the third liquid crystal phase difference film is sometimes referred to as a "liquid crystal phase difference film".

[0197] <Liquid crystal retardation film>

[0198] In this specification, the case where the optical axis of the polymerizable liquid crystal is horizontally oriented relative to the plane of the substrate is defined as horizontal orientation, and the case where the optical axis of the polymerizable liquid crystal is vertically oriented relative to the plane of the substrate is defined as vertical orientation. The optical axis refers to the direction in which the cross section cut in the direction orthogonal to the optical axis in the refractive index ellipsoid formed by the orientation of the polymerizable liquid crystal becomes a circle, that is, the direction in which the refractive indexes in the three directions are all equal.

[0199] As polymerizable liquid crystals, rod-shaped polymerizable liquid crystals and disc-shaped polymerizable liquid crystals can be cited. When the rod-shaped polymerizable liquid crystal is horizontally oriented or vertically oriented relative to the substrate, the optical axis of the polymerizable liquid crystal is consistent with the long axis direction of the polymerizable liquid crystal. When the disc-shaped polymerizable liquid crystal is oriented, the optical axis of the polymerizable liquid crystal exists in a direction orthogonal to the disc surface of the polymerizable liquid crystal.

[0200] In order to make the layer formed by polymerizing the polymerizable liquid crystal show an in-plane phase difference, it is sufficient to orient the polymerizable liquid crystal in a suitable direction. In the case where the polymerizable liquid crystal is rod-shaped, the in-plane phase difference is shown by orienting the optical axis of the polymerizable liquid crystal horizontally relative to the plane of the substrate, in which case the direction of the optical axis is consistent with the direction of the slow axis. In the case where the polymerizable liquid crystal is disc-shaped, the in-plane phase difference is shown by orienting the optical axis of the polymerizable liquid crystal horizontally relative to the plane of the substrate, in which case the optical axis is orthogonal to the slow axis. The orientation state of the polymerizable liquid crystal can be adjusted by a combination of an alignment film and a polymerizable liquid crystal.

[0201] The in-plane phase difference value of the liquid crystal phase difference film can be adjusted by the thickness of the phase difference film. Since the in-plane phase difference value is determined by formula (4), in order to obtain the desired in-plane phase difference value (Re(λ)), it is only necessary to adjust Δn(λ) and the film thickness d.

[0202] Re(λ)=d×Δn(λ) (4)

[0203] Where Re(λ) represents the in-plane phase difference at a wavelength of λ nm, d represents the film thickness, and Δn(λ) represents the birefringence at a wavelength of λ nm.

[0204] The birefringence Δn(λ) is obtained by measuring the in-plane phase difference value and dividing it by the thickness of the phase difference film. In a specific measurement method, the actual properties of the phase difference film can be measured by measuring the film formed on a substrate such as a glass substrate that has no in-plane phase difference.

[0205] When the optical axis of the rod-shaped polymerizable liquid crystal is aligned horizontally to the substrate plane, the refractive index relationship of the obtained retardation film is nx>ny≥nz (positive A plate), and the axis in the nx direction of the refractive index ellipsoid coincides with the slow axis.

[0206] When the optical axis of the disc-shaped polymerizable liquid crystal is aligned horizontally to the substrate plane, the refractive index relationship of the obtained retardation film becomes nx<ny≤nz (negative A plate), and the axis in the ny direction of the refractive index ellipsoid coincides with the slow axis.

[0207] In order to make the layer formed by polymerizing the polymerizable liquid crystal show a phase difference in the thickness direction, it is sufficient to align the polymerizable liquid crystal in a suitable direction. In this specification, the phase difference in the thickness direction is defined as: showing a characteristic that Rth (phase difference value in the thickness direction) in formula (20) becomes negative. Rth can be measured based on the phase difference value (Rt) measured by tilting 40 degrees with the fast axis in the plane as the tilt axis. 40), and the phase difference value (Re) within the plane. That is, Rth can be calculated as follows: 40 , d (thickness of the retardation film) and n0 (average refractive index of the retardation film), nx, ny and nz are obtained using the following equations (21) to (23), and these are substituted into equation (20) for calculation.

[0208] Rth=[(nx+ny) / 2-nz]×d (20)

[0209] Re=(nx-ny) ×d (21)

[0210] R 40 =(nx-ny') ×d / cos(φ) (22)

[0211] (nx+ny+nz) / 3=n0 (23)

[0212] Here,

[0213] φ=sin -1 [sin(40°) / n0]

[0214] ny'=ny×nz / [ny 2 ×sin 2 (φ)+nz 2 ×cos 2 (φ)] 1 / 2

[0215] In addition, nx, ny and nz are the same as defined above.

[0216] In the case where the polymerizable liquid crystal is rod-shaped, the phase difference in the thickness direction is exhibited by orienting the optical axis of the polymerizable liquid crystal perpendicularly to the plane of the substrate. In the case where the polymerizable liquid crystal is disc-shaped, the phase difference in the thickness direction is exhibited by orienting the optical axis of the polymerizable liquid crystal horizontally to the plane of the substrate. In the case of a disc-shaped polymerizable liquid crystal, since the optical axis of the polymerizable liquid crystal is parallel to the plane of the substrate, if Re is determined, the thickness is fixed, and therefore, Rth is determined without doubt, but in the case of a rod-shaped polymerizable liquid crystal, since the optical axis of the polymerizable liquid crystal is perpendicular to the plane of the substrate, by adjusting the thickness of the phase difference film, Rth can be adjusted without changing Re.

[0217] <Polymerizable liquid crystal>

[0218] Polymerizable liquid crystal refers to a compound having a polymerizable group and having liquid crystal properties. A polymerizable group refers to a group that participates in a polymerization reaction, preferably a photopolymerizable group. Here, a photopolymerizable group refers to a group that can participate in a polymerization reaction by an active free radical or acid generated by a photopolymerization initiator described later. As a polymerizable group, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, oxetane, etc. can be cited. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxirane and oxetane are preferred, and acryloyloxy is more preferred. The liquid crystal properties of the polymerizable liquid crystal can be a thermotropic liquid crystal or a lyotropic liquid crystal. If the thermotropic liquid crystal is classified by order, it can be a nematic liquid crystal or a smectic liquid crystal.

[0219] As rod-shaped polymerizable liquid crystals, for example, compounds represented by the following formula (A) and compounds containing groups represented by the following formula (X) can be cited. As rod-shaped polymerizable liquid crystals, from the viewpoint of exhibiting wavelength dispersion, liquid crystals having a mesomorphic structure in a T-shaped or H-shaped structure that is vertically oriented relative to the molecular axis and thus has birefringence are preferably used. From the viewpoint of obtaining stronger dispersion, T-shaped liquid crystals are more preferably used. As the structure of the T-shaped liquid crystal, specifically, compounds represented by the following formula (A) can be cited.

[0220] (Compound represented by formula (A))

[0221] Formula (A) is as follows: Hereinafter, the compound represented by formula (A) may be referred to as polymerizable liquid crystal (A).

[0222]

[0223] In formula (A), Ar represents a divalent aromatic group which may have a substituent. The divalent aromatic group preferably contains at least one of a nitrogen atom, an oxygen atom, and a sulfur atom. When the number of aromatic groups contained in the divalent group Ar is 2 or more, the 2 or more aromatic groups may be bonded to each other by divalent bonding groups such as a single bond, -CO-O-, or -O-.

[0224] G 1 and G 2 Each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. Here, the hydrogen atoms contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted by a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group or a nitro group, and the carbon atoms constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted by an oxygen atom, a sulfur atom or a nitrogen atom.

[0225] L 1 , L2 , B 1 and B 2 are each independently a single bond or a divalent linking group.

[0226] k and l each independently represent an integer from 0 to 3 and satisfy the relation 1 ≤ k + l. Here, when 2 ≤ k + l, B 1 and B 2 , G 1 and G 2 may be the same as or different from each other.

[0227] E 1 and E 2 each independently represent an alkanediyl group having 1 to 17 carbon atoms (in Japanese: アルカンジイル基). Here, the hydrogen atoms contained in the alkanediyl group may be substituted by halogen atoms, and the -CH2- contained in the alkanediyl group may be replaced by -O-, -S-, -COO-. When there are multiple -O-, -S-, -COO-, they are not adjacent to each other. P 1 and P 2 independently represent a polymerizable group or a hydrogen atom, and at least one is a polymerizable group.

[0228] G 1 and G 2 are each independently preferably a 1,4-phenylene diyl group that can be substituted by at least one substituent selected from halogen atoms and alkyl groups having 1 to 4 carbon atoms, a 1,4-cyclohexane diyl group that can be substituted by at least one substituent selected from halogen atoms and alkyl groups having 1 to 4 carbon atoms, more preferably a 1,4-phenylene diyl group substituted by a methyl group, an unsubstituted 1,4-phenylene diyl group, or an unsubstituted 1,4-trans-cyclohexane diyl group, and particularly preferably an unsubstituted 1,4-phenylene diyl group or an unsubstituted 1,4-trans-cyclohexane diyl group.

[0229] In addition, it is preferred that at least one of the multiple Gs 1 and G 2 is a divalent alicyclic hydrocarbon group. In addition, it is more preferably that at least one of the Gs 1 bonded to L 2 or L 1 and G 2 is a divalent alicyclic hydrocarbon group.

[0230] L 1 and L 2 are each independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a1 OR a2 -, -R a3 COOR a4 -, -R a5 OCORa6 -、R a7 OC=OOR a8 -、-N=N-、-CR c =CR d -, or C≡C-. Here, R a1 ~R a8 Each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms, and R c and R d represents an alkyl group having 1 to 4 carbon atoms or a hydrogen atom. 1 and L 2 Each independently is more preferably a single bond, -OR a2-1 -、-CH2-、-CH2CH2-、-COOR a4-1 -, or OCOR a6-1 -. Here, R a2-1 , R a4-1 , R a6-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. 1 and L 2 Each independently is further preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, or OCO-.

[0231] B 1 and B 2 Each of them is independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a9 OR a10 -、-R a11 COOR a12 -、-R a13 OCOR a14 -, or -R a15 OC(=O)OR a16 -. Here, R a9 ~R a16 Each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms. 1 and B 2 Each independently is more preferably a single bond, -OR a10-1 -、-CH2-、-CH2CH2-、-COOR a12 -1 -, or OCOR a14-1 -. Here, R a10-1 , R a12-1 , R a14-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. 1 and B 2Each independently is further preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, -OCO-, or -OCOCH2CH2-.

[0232] From the viewpoint of exhibiting reverse wavelength dispersion, k and l are preferably in the range of 2≤k+l≤6, preferably k+l=4, and more preferably k=2 and l=2. If k=2 and l=2, a symmetrical structure is obtained, which is preferred.

[0233] E 1 and E 2 Each independently is preferably an alkanediyl group having 1 to 17 carbon atoms, and more preferably an alkanediyl group having 4 to 12 carbon atoms.

[0234] As P 1 or P 2 The polymerizable group shown in the figure includes epoxy, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxiranyl and oxetanyl, etc. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxiranyl and oxetanyl are preferred, and acryloyloxy is more preferred.

[0235] Ar preferably has at least one selected from an aromatic hydrocarbon ring that may have a substituent, an aromatic heterocycle that may have a substituent, and an electron-withdrawing group. As the aromatic hydrocarbon ring, for example, benzene ring, naphthalene ring, anthracene ring, etc. can be cited, preferably benzene ring, naphthalene ring. As the aromatic heterocycle, furan ring, benzofuran ring, pyrrole ring, indole ring, thiophene ring, benzothiophene ring, pyridine ring, pyrazine ring, pyrimidine ring, triazole ring, triazine ring, pyrroline ring, imidazole ring, pyrazole ring, thiazole ring, benzothiazole ring, thienothiazole ring, oxazole ring, benzoxazole ring and phenanthroline ring etc. can be cited. Among them, preferably have thiazole ring, benzothiazole ring or benzofuran ring, further preferably have benzothiazolyl. In addition, when Ar includes nitrogen atom, the nitrogen atom preferably has π electrons.

[0236] In formula (A), the total number Nπ of π electrons contained in the divalent aromatic group represented by Ar is preferably 8 or more, more preferably 10 or more, further preferably 14 or more, and particularly preferably 16 or more. It is preferably 30 or less, more preferably 26 or less, and further preferably 24 or less.

[0237] As the aromatic group represented by Ar, for example, the following groups can be preferably mentioned.

[0238]

[0239] In the formulas (Ar-1) to (Ar-23), the * symbol represents a connecting portion, and Z 0 , Z1 and Z 2 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkylsulfinyl group having 1 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, a carboxyl group, a fluoroalkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, an N-alkylamino group having 1 to 12 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 12 carbon atoms, or an N,N-dialkylsulfamoyl group having 2 to 12 carbon atoms.

[0240] Q 1 , Q 2 and Q 3 Each independently represents -CR 2’ R 3’ -、-S-、-NH-、-NR 2’ -, -CO- or O-, R 2’ and R 3’ Each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

[0241] J 1 and J 2 Each independently represents a carbon atom or a nitrogen atom.

[0242] Y 1 , Y 2 and Y 3 Each independently represents an aromatic hydrocarbon group or an aromatic heterocyclic group which may be substituted.

[0243] W 1 and W 2 Each independently represents a hydrogen atom, a cyano group, a methyl group or a halogen atom, and m represents an integer of 0-6.

[0244] As Y 1 , Y 2 and Y 3 The aromatic hydrocarbon group in the group includes aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as phenyl, naphthyl, anthracenyl, phenanthrenyl, and biphenyl, preferably phenyl and naphthyl, and more preferably phenyl. The aromatic heterocyclic group includes aromatic heterocyclic groups having 4 to 20 carbon atoms, such as furanyl, pyrrolyl, thienyl, pyridyl, thiazolyl, and benzothiazolyl, which contain at least one hetero atom such as a nitrogen atom, an oxygen atom, or a sulfur atom, preferably furanyl, thienyl, pyridyl, thiazolyl, and benzothiazolyl.

[0245] Y 1 , Y 2 and Y 3Each independently may be a polycyclic aromatic hydrocarbon group or a polycyclic aromatic heterocyclic group which may be substituted. The polycyclic aromatic hydrocarbon group refers to a condensed polycyclic aromatic hydrocarbon group or a group derived from a collection of aromatic rings. The polycyclic aromatic heterocyclic group refers to a condensed polycyclic aromatic heterocyclic group or a group derived from a collection of aromatic rings.

[0246] Z 0 , Z 1 and Z 2 Each of Z is independently preferably a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, or an alkoxy group having 1 to 12 carbon atoms. 0 More preferably, a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a cyano group. 1 and Z 2 More preferred are a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group and a cyano group.

[0247] Q 1 , Q 2 and Q 3 Preferred are -NH-, -S-, -NR 2’ -、-O-,R 2’ A hydrogen atom is preferred, and -S-, -O-, and -NH- are particularly preferred.

[0248] Among formulae (Ar-1) to (Ar-23), formulae (Ar-6) and (Ar-7) are preferred from the viewpoint of molecular stability.

[0249] In the formulas (Ar-16) to (Ar-23), Y 1 The nitrogen atom and Z 0 Together, they form an aromatic heterocyclic group. Examples of the aromatic heterocyclic group include the aromatic heterocyclic groups described above as aromatic heterocyclic rings that Ar may have, such as a pyrrole ring, an imidazole ring, a pyrroline ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, an indole ring, a quinoline ring, an isoquinoline ring, a purine ring, and a pyrrolidine ring. The aromatic heterocyclic group may have a substituent. In addition, Y 1 The nitrogen atom and Z 0 Together, they are the above-mentioned optionally substituted polycyclic aromatic hydrocarbon groups or polycyclic aromatic heterocyclic groups, for example, benzofuran ring, benzothiazole ring, benzoxazole ring, etc.

[0250] (Compound containing a group represented by formula (X))

[0251] Formula (X) is as follows: Hereinafter, a compound including a group represented by formula (X) may be referred to as polymerizable liquid crystal (B).

[0252] P11-B11-E11-B12-A11-B13- (X)

[0253] [In formula (X), P11 represents a polymerizable group.

[0254] A11 represents a divalent alicyclic hydrocarbon group or a divalent aromatic hydrocarbon group. The hydrogen atoms contained in the divalent alicyclic hydrocarbon group and the divalent aromatic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group or a nitro group, and the hydrogen atoms contained in the alkyl group having 1 to 6 carbon atoms and the alkoxy group having 1 to 6 carbon atoms may be substituted with a fluorine atom.

[0255] B11 represents -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, -CO-NR 16 -、-NR 16 -CO-, -CO-, -CS- or a single bond. 16 It represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0256] B12 and B13 each independently represent -C≡C-, -CH=CH-, -CH2-CH2-, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -OC(=O)-O-, -CH=N-, -N=CH-, -N=N-, -C(=O)-NR 16 -、-NR 16 -C(=O)-, -OCH2-, -OCF2-, -CH2O-, -CF2O-, -CH=CH-C(=O)-O-, -OC(=O)-CH=CH- or a single bond.

[0257] E11 represents an alkanediyl group having 1 to 12 carbon atoms, wherein the hydrogen atoms contained in the alkanediyl group may be substituted by an alkoxy group having 1 to 5 carbon atoms, and the hydrogen atoms contained in the alkoxy group may be substituted by a halogen atom. In addition, -CH2- constituting the alkanediyl group may be substituted by -O- or -CO-.]

[0258] The number of carbon atoms of the aromatic hydrocarbon group and alicyclic hydrocarbon group of A11 is preferably in the range of 3 to 18, more preferably in the range of 5 to 12, and particularly preferably 5 or 6. A11 is preferably cyclohexane-1,4-diyl or 1,4-phenylene.

[0259] E11 is preferably a linear alkanediyl group having 1 to 12 carbon atoms. -CH2- constituting the alkanediyl group may be substituted with -O-.

[0260] Specifically, examples include: straight-chain alkanediyl groups having 1 to 12 carbon atoms, such as methylene, ethylene, propane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, hexane-1,6-diyl, heptane-1,7-diyl, octane-1,8-diyl, nonane-1,9-diyl, decane-1,10-diyl, undecane-1,11-diyl and dodecane-1,12-diyl; -CH2-CH2-O-CH2-CH2-, -CH2-CH2-O-CH2-CH2-O-CH2-CH2- and -CH2-CH2-O-CH2-CH2-O-CH2-CH2-O-CH2-CH2-, etc.

[0261] B11 is preferably -O-, -S-, -CO-O-, and -O-CO-, and among them, -CO-O- is more preferred.

[0262] As B12 and B13, each independently, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -OC(=O)-O-, and -O- or -OC(=O)-O- are preferred. Among them, -O- or -OC(=O)-O- is more preferred.

[0263] As the polymerizable group represented by P11, from the perspective of high polymerization reactivity, especially photopolymerization reactivity, a free radical polymerizable group or a cationic polymerizable group is preferred. From the perspective of easy operation and easy manufacture of the liquid crystal compound itself, the polymerizable group is preferably a group represented by the following formula (P-11) to (P-15).

[0264]

[0265] [In formulas (P-11) to (P-15),

[0266] R 17 ~R 21 Each independently represents an alkyl group having 1 to 6 carbon atoms or a hydrogen atom.]

[0267] Specific examples of the groups represented by formula (P-11) to formula (P-15) include groups represented by the following formula (P-16) to formula (P-20).

[0268]

[0269] P11 is preferably a group represented by formula (P-14) to formula (P-20), and more preferably a vinyl group, a p-stilbene group, an epoxy group or an oxetanyl group.

[0270] The group represented by P11-B11- is more preferably an acryloyloxy group or a methacryloyloxy group.

[0271] Examples of the polymerizable liquid crystal (B) include compounds represented by formula (I), formula (II), formula (III), formula (IV), formula (V) or formula (VI).

[0272] P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-B16-E12-B17-P12 (I)

[0273] P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-F11 (II)

[0274] P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-E12-B17-P12 (III)

[0275] P11-B11-E11-B12-A11-B13-A12-B14-A13-F11 (IV)

[0276] P11-B11-E11-B12-A11-B13-A12-B14-E12-B17-P12 (V)

[0277] P11-B11-E11-B12-A11-B13-A12-F11 (VI)

[0278] (Where,

[0279] A12 to A14 each independently have the same meaning as A11, B14 to B16 each independently have the same meaning as B12, B17 has the same meaning as B11, and E12 has the same meaning as E11.

[0280] F11 represents a hydrogen atom, an alkyl group having 1 to 13 carbon atoms, an alkoxy group having 1 to 13 carbon atoms, a cyano group, a nitro group, a trifluoromethyl group, a dimethylamino group, a hydroxyl group, a hydroxymethyl group, a formyl group, a sulfo group (-SO3H), a carboxyl group, an alkoxycarbonyl group having 1 to 10 carbon atoms, or a halogen atom, and the -CH2- constituting the alkyl group and the alkoxy group may be replaced by -O-.

[0281] Specific examples of polymerizable liquid crystals (B) include: compounds having polymerizable groups among the compounds described in "3.8.6 Network (Completely Cross-linked Type)" and "6.5.1 Liquid Crystal Materials b. Polymerizable Nematic Liquid Crystal Materials" of Liquid Crystal Handbook (edited by Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2013), and polymerizable liquid crystals described in Japanese Patent Gazette Nos. 2010-31223, 2010-270108, 2011-6360, and 2011-207765.

[0282] As specific examples of polymerizable liquid crystals (B), compounds shown in the following formulas (I-1) to (I-4), (II-1) to (II-4), (III-1) to (III-26), (IV-1) to (IV-26), (V-1) to (V-2) and (VI-1) to (VI-6) can be cited. It should be noted that in the following formula, k1 and k2 each independently represent an integer of 2 to 12. These polymerizable liquid crystals (B) are preferred from the perspective of their ease of synthesis or ease of acquisition.

[0283]

[0284]

[0285]

[0286]

[0287]

[0288]

[0289]

[0290]

[0291] Examples of the discotic polymerizable liquid crystal include compounds containing a group represented by formula (W) (hereinafter, sometimes referred to as polymerizable liquid crystal (C)).

[0292]

[0293] [In formula (W), R 40 The following formulas (W-1) to (W-5) are represented.

[0294]

[0295] X 40 and Z 40 It represents an alkyl group having 1 to 12 carbon atoms, wherein the hydrogen atoms contained in the alkyl group may be substituted by an alkoxy group having 1 to 5 carbon atoms, wherein the hydrogen atoms contained in the alkoxy group may be substituted by a halogen atom. In addition, -CH2- constituting the alkyl group may be substituted by -O- or -CO-.

[0296] Specific examples of polymerizable liquid crystals (C) include: compounds described in "6.5.1 Liquid Crystal Materials b. Polymerizable Nematic Liquid Crystal Materials Figure 6.21" of the Liquid Crystal Handbook (edited by the Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 1992), and polymerizable liquid crystals described in Japanese Patent Publication No. 7-258170, Japanese Patent Publication No. 7-30637, Japanese Patent Publication No. 7-309807, and Japanese Patent Publication No. 8-231470.

[0297] The phase difference plate 30 having the optical properties shown in formulas (11) and (12) can be obtained by combining a layer having the optical properties shown in formulas (14), (16) and (17) with a layer having the optical properties shown in formulas (15), (16) and (17) in a specific slow axis relationship.

[0298] Re(450) / Re(550) ≤1.00 (11)

[0299] 1.00≤Re(650) / Re (550) (12)

[0300] 100nm<Re (550)<150nm (14)

[0301] 150nm<Re (550)<320nm (15)

[0302] Re (450) / Re (550) ≥1.00 (16)

[0303] 1.00≥Re (650) / Re (550) (17)

[0304] The phase difference plate 30 preferably has the optical properties shown in formula (11) and formula (12). If the phase difference plate 30 has the optical properties shown in formula (11) and formula (12), the same polarization conversion properties can be obtained for light of each wavelength in the visible light region, and the coloring of reflected light during black display of a display device such as an organic EL display device can be suppressed.

[0305] As the polymerizable liquid crystal having a specific structure, for example, the polymerizable liquid crystal (A) can be cited. By aligning the polymerizable liquid crystal (A) in a manner that the optical axis is horizontal relative to the substrate plane, a phase difference film having the optical properties represented by formula (11) and formula (12) can be obtained. In addition, by adjusting the film thickness, for example, a phase difference film having a desired in-plane phase difference value such as the optical properties represented by formula (14) can be obtained.

[0306] 100nm<Re(550) <150nm (14)

[0307] As a method of combining a layer having optical characteristics shown in formula (14), (16) and (17) and a layer having optical characteristics shown in formula (15), (16) and (17) in a specific slow axis relationship, a known method can be cited. For example, Japanese Patent Publication No. 2001-4837, Japanese Patent Publication No. 2001-21720 and Japanese Patent Publication No. 2000-206331 disclose a phase difference film (Japanese: phase difference film) having at least two layers of phase difference films containing liquid crystal compounds. It should be noted that the layer having the optical characteristics shown in formula (14) is also referred to as a 1 / 4 wavelength layer, the layer having the optical characteristics shown in formula (15) is also referred to as a 1 / 2 wavelength layer, and the optical characteristics shown in formula (16) and formula (17) are also referred to as positive wavelength dispersion. In addition, from the viewpoint of being able to compensate for the anti-reflection function in the inclined direction, it is preferred to also include a layer having anisotropy in the thickness direction (positive C plate). In addition, each optically anisotropic layer may be tilted or cholesterically aligned.

[0308] The retardation film having the optical properties represented by the above formula (16) and formula (17) can be obtained by a known method. That is, the retardation film obtained by a method other than the method for obtaining the retardation film having the optical properties represented by the above formula (11) and formula (12) roughly has the optical properties represented by formula (16) and formula (17).

[0309] In a preferred embodiment of the phase difference plate 30, the first liquid crystal phase difference film 31 has the optical properties shown by formulas (15), (16) and (17), and the second liquid crystal phase difference film 32 has the optical properties shown by formulas (14), (16) and (17).

[0310] 100nm<Re(550)<150nm (14)

[0311] 150nm<Re(550)<320nm (15)

[0312] Re(450) / Re(550)≥1.00 (16)

[0313] 1.00≥Re(650) / Re(550) (17)

[0314] The second liquid crystal retardation film 32 is preferably a layer having the optical characteristics represented by formula (14-1), and the first liquid crystal retardation film 31 is preferably a layer having the optical characteristics represented by formula (15-1).

[0315] 130nm<Re(550)<150nm (14-1)

[0316] 265nm<Re(550)<285nm (15-1)

[0317] The first liquid crystal retardation film 31 is preferably a coating layer formed by polymerizing polymerizable liquid crystal (C). The second liquid crystal retardation film 32 is preferably a coating layer formed by polymerizing polymerizable liquid crystal (B).

[0318] The thickness of each of the first liquid crystal retardation film 31 and the second liquid crystal retardation film 32 is preferably 0.2 μm or more and 3.0 μm or less, and more preferably 0.4 μm or more and 2.8 μm or less. According to the present invention, even if the thickness of the first liquid crystal retardation film 31 and the second liquid crystal retardation film 32 is 3.0 μm or less, the interference unevenness observed from the oblique direction can be reduced.

[0319] The thickness of the liquid crystal retardation film can be determined by measuring with an interference film thickness meter, a laser microscope, or a stylus film thickness meter.

[0320] The first liquid crystal retardation film 31 and the second liquid crystal retardation film 32 are preferably arranged to intersect at an in-plane intersecting angle of, for example, 50° to 70°. The intersecting angle referred to here is a narrower intersecting angle among the intersecting angles of the two slow axes.

[0321] Relative to the absorption axis of the polarizer, the slow axis of the first liquid crystal retardation film 31 is, for example, 10° to 20°, preferably 12° to 18°, and more preferably about 15°, and the slow axis of the second liquid crystal retardation film 32 is, for example, greater than 70° and less than 80°, more preferably greater than 72° and less than 78°, and more preferably about 75°.

[0322] In another embodiment, relative to the absorption axis of the polarizer, the slow axis of the first liquid crystal retardation film 31 is, for example, -10° to -20°, preferably -12° to -18°, and further preferably about -15°, and the slow axis of the second liquid crystal retardation film 32 is, for example, -70° to -80°, more preferably -72° to -78°, and further preferably about -75°.

[0323] In another embodiment, relative to the absorption axis of the polarizer, the slow axis of the first liquid crystal retardation film 31 is 70° to 80°, preferably 72° to 78°, and further preferably about 75°, and the slow axis of the second liquid crystal retardation film 32 is, for example, 10° to 20°, more preferably 12° to 18°, and further preferably about 15°.

[0324] In another embodiment, relative to the absorption axis of the polarizer, the slow axis of the first liquid crystal retardation film 31 is -70° to -80°, preferably -72° to -78°, and further preferably about -75°, and the slow axis of the second liquid crystal retardation film 32 is, for example, -10° to -20°, more preferably -12° to -18°, and further preferably about -15°.

[0325] <Base material>

[0326] The phase difference plate 30 may have a substrate. The substrate is usually a transparent substrate. A transparent substrate refers to a substrate having transparency that can transmit light, especially visible light, and transparency refers to the property that the transmittance is 80% or more for light with a wavelength of 380 to 780 nm. As the substrate, a glass substrate and a film substrate can be cited, preferably a film substrate, and from the perspective of being able to be manufactured continuously, a long roll film is more preferred. As a resin constituting the film substrate, for example, there can be cited: polyolefins such as polyethylene, polypropylene, and norbornene polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylate; polyacrylate; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide and polyphenylene ether; and other plastics. Among them, from the viewpoint of transparency when used in optical film applications, a film substrate selected from triacetyl cellulose, cyclic olefin resins, polymethacrylates, and polyethylene terephthalate is more preferred.

[0327] Examples of commercially available cellulose ester substrates include "FUJITAC Film" (manufactured by Fuji Photo Film Co., Ltd.); "KC8UX2M", "KC8UY", and "KC4UY" (all manufactured by Konica Minolta Opto Co., Ltd.).

[0328] Examples of commercially available cyclic olefin resins include "Topas" (registered trademark) (manufactured by Ticona (Germany)), "ARTON" (registered trademark) (manufactured by JSR Corporation), "ZEONOR" (registered trademark), "ZEONEX" (registered trademark) (manufactured by ZEON Corporation of Japan), and "APEL" (registered trademark) (manufactured by Mitsui Chemicals, Inc.). Such cyclic olefin resins can be made into films by known methods such as solvent casting and melt extrusion to form substrates. Commercially available cyclic olefin resin substrates can also be used. Examples of commercially available cyclic olefin resin substrates include “Esushina” (registered trademark), “SCA40” (registered trademark) (all manufactured by Sekisui Chemical Co., Ltd.), “ZeonorFilm” (registered trademark) (manufactured by Optes Co., Ltd.), and “Arton Film” (registered trademark) (manufactured by JSR Corporation).

[0329] The thickness of the substrate is preferably thin enough to be handled in a practical manner, but if it is too thin, there is a tendency for reduced strength and poor processability. The thickness of the substrate is usually 5 μm to 300 μm, preferably 10 μm to 200 μm, and more preferably 10 to 50 μm. In addition, by peeling off the substrate and transferring the polarizing film or phase difference film, a further thin film effect can be obtained.

[0330] <Oriented film>

[0331] In this specification, the alignment film has an alignment regulating force for orienting the polymerizable liquid crystal compound in a desired direction.

[0332] The orientation film makes it easy to orient the liquid crystal of the polymerizable liquid crystal compound. The state of liquid crystal orientation such as horizontal orientation, vertical orientation, mixed orientation, and tilted orientation varies according to the properties of the orientation film and the polymerizable liquid crystal compound, and the combination thereof can be selected arbitrarily. For example, if the orientation film is a material that exhibits horizontal orientation as an orientation limiting force, the polymerizable liquid crystal compound can form a horizontal orientation or a mixed orientation, and if it is a material that exhibits vertical orientation, the polymerizable liquid crystal compound can form a vertical orientation or a tilted orientation. Expressions such as horizontal and vertical indicate the direction of the optical axis of the oriented polymerizable liquid crystal compound when the plane of the optical anisotropic layer is used as a reference. For example, vertical orientation refers to an optical axis of the oriented polymerizable liquid crystal compound in a direction perpendicular to the plane of the optical anisotropic layer. The vertical mentioned here refers to 90°±20° relative to the plane of the optical anisotropic layer.

[0333] Regarding the orientation restraining force, when the orientation film is formed of an orientation polymer, it can be arbitrarily adjusted according to the surface state and friction conditions, and when it is formed of a photo-orientation polymer, it can be arbitrarily adjusted according to polarized light irradiation conditions, etc. In addition, the liquid crystal orientation can also be controlled by selecting the surface tension, liquid crystal properties, etc. of the polymerizable liquid crystal compound.

[0334] As an oriented film formed between a substrate and a liquid crystal phase difference film, it is preferably an oriented film that is insoluble in the solvent used when forming a liquid crystal phase difference film on the oriented film, and has heat resistance in the heating treatment for removing the solvent and aligning the liquid crystal. As an oriented film, an oriented film comprising an oriented polymer, a photo-oriented film and a groove oriented film, a stretched film stretched along the orientation direction, etc. can be cited. In the case of a long roll film, from the viewpoint of being able to easily control the orientation direction, a photo-oriented film is preferred.

[0335] The thickness of the alignment film is usually in the range of 10 nm to 5000 nm, preferably in the range of 10 nm to 1000 nm, and more preferably in the range of 30 to 300 nm.

[0336] As the oriented polymer used in the rubbing oriented film, there can be enumerated: polyamide and gelatin with amide bonds in the molecule, polyimide with imide bonds in the molecule and polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinyl pyrrolidone, polyacrylic acid and polyacrylates etc. as their hydrolyzates. Among them, polyvinyl alcohol is preferred. These oriented polymers can be used alone or in combination of two or more.

[0337] As a method of rubbing, there is mentioned a method of bringing a film of an oriented polymer formed on the surface of a substrate by applying an oriented polymer composition to the substrate and annealing the film into contact with a rubbing roller wound with a rubbing cloth and rotating.

[0338] The photo-alignment film comprises a polymer, oligomer or monomer having a photoreactive group. The photo-alignment film obtains an alignment restraining force by irradiating polarized light. From the viewpoint that the direction of the alignment restraining force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized light, a photo-alignment film is more preferred.

[0339] A photoreactive group refers to a group that generates liquid crystal orientation capability by irradiation with light. Specifically, it is a group that generates a photoreaction that is the origin of the liquid crystal orientation capability, such as an orientation induction or isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction of a molecule generated by irradiation with light. In the photoreactive group, from the aspect of excellent orientation, a group that generates a dimerization reaction or a photocrosslinking reaction is preferred. As a photoreactive group capable of the above-mentioned reaction, a photoreactive group having an unsaturated bond, particularly a double bond, is preferably a group having at least one selected from a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond).

[0340] As photoreactive groups having C=C bonds, for example, vinyl, polyene, stilbene, stilbazolyl, stilbazolyl, chalcone and cinnamoyl groups can be cited. From the viewpoint of easy control of reactivity and the viewpoint of orientation restriction during photo-orientation, chalcone and cinnamoyl groups are preferred. As photoreactive groups having C=N bonds, groups having structures such as aromatic Schiff bases and aromatic hydrazones can be cited. As photoreactive groups having N=N bonds, groups with azobenzene as the basic structure, such as azonaphthyl, aromatic heterocyclic azo, disazo and formazan, can be cited. As photoreactive groups having C=O bonds, benzophenone, coumarin, anthraquinone and maleimide groups can be cited. These groups may have a substituent such as an alkyl group, an alkoxy group, an aryl group, an allyloxy group, a cyano group, an alkoxycarbonyl group, a hydroxyl group, a sulfonic acid group, and a halogenated alkyl group.

[0341] When irradiating polarized light, it can be a form of directly irradiating polarized light from the film surface, or it can be a form of irradiating polarized light from the substrate side and transmitting the polarized light. In addition, the polarized light is particularly preferably substantially parallel light. Regarding the wavelength of the irradiated polarized light, it is better to have a photoreactive group of a polymer or monomer with a photoreactive group. The wavelength of polarized light in the wavelength region where the photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) in the range of 250 to 400nm is particularly preferred. As the light source used in the polarized light irradiation, xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF can be cited, and high-pressure mercury lamps, ultra-high-pressure mercury lamps and metal halide lamps are more preferred. These lamps are preferred because the luminous intensity of ultraviolet light with a wavelength of 313nm is large. The light from the above-mentioned light source is irradiated through an appropriate polarizer, thereby irradiating polarized light. As the polarizer, polarizing prisms such as polarizing filters, Glan Thomson and Glan Taylor, and wire grid polarizers can be used.

[0342] <Polarizing film-forming composition, liquid crystal retardation film-forming composition>

[0343] The polarizing film-forming composition or the liquid crystal retardation film-forming composition (hereinafter also referred to as the optically anisotropic layer-forming composition) may further contain reactive additives such as solvents, leveling agents, polymerization initiators, photosensitizers, polymerization inhibitors, crosslinking agents, and adhesion agents. From the viewpoint of processability, it is preferred to contain solvents and leveling agents.

[0344] (Solvent)

[0345] The composition for forming an optically anisotropic layer may contain a solvent. Generally, the viscosity of the polymerizable liquid crystal compound is high, so by preparing the composition for forming an optically anisotropic layer that is dissolved in the solvent, coating becomes easy, and as a result, an optically anisotropic layer is easily formed in many cases. As the solvent, a solvent that can completely dissolve the polymerizable liquid crystal compound is preferred, and a solvent that is inactive to the polymerization reaction of the polymerizable liquid crystal compound is preferred.

[0346] Examples of the solvent include: alcohol solvents such as methanol, ethanol, ethylene glycol, isopropanol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone or propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene, and nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorinated solvents such as chloroform and chlorobenzene; amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone, etc. These solvents may be used alone or in combination of two or more.

[0347] The content of the solvent is preferably 50 to 98% by mass relative to the total amount of the composition for forming an optically anisotropic layer. In other words, the content of the solid component in the composition for forming an optically anisotropic layer is preferably 2 to 50% by mass, more preferably 5 to 30% by mass. If the content of the solid component is less than 50% by mass, the viscosity of the composition for forming an optically anisotropic layer decreases, so the thickness of the optically anisotropic layer becomes roughly uniform, and thus there is a tendency that the optically anisotropic layer is not easy to produce interference unevenness. In addition, the content of the solid component can be determined by considering the thickness of the optically anisotropic layer to be manufactured.

[0348] (Leveling agent)

[0349] The composition for forming anisotropic optically anisotropic layers may contain a leveling agent. A leveling agent is an additive that has the function of adjusting the fluidity of the composition and making the film obtained by coating the composition flatter, and examples thereof include organic modified silicone-based, polyacrylate-based, and perfluoroalkyl-based leveling agents. Among them, polyacrylate-based leveling agents and perfluoroalkyl-based leveling agents are preferred when the composition is horizontally oriented, and organic modified silicone-based leveling agents and perfluoroalkyl-based leveling agents are preferred when the composition is vertically oriented.

[0350] When the composition for forming an optically anisotropic layer contains a leveling agent, it is preferably 0.01 to 5 parts by mass, and more preferably 0.05 to 3 parts by mass, relative to 100 parts by mass of the content of the polymerizable liquid crystal compound. If the content of the leveling agent is within the above range, there is a tendency to easily make the polymerizable liquid crystal compound horizontally oriented and the obtained optically anisotropic layer smoother. If the content of the leveling agent exceeds the above range relative to the content of the polymerizable liquid crystal compound, there is a tendency that the obtained optically anisotropic layer is prone to interference unevenness. It should be noted that the composition for forming an optically anisotropic layer may contain two or more leveling agents.

[0351] (Polymerization initiator)

[0352] The composition for forming an optically anisotropic layer may contain a polymerization initiator. A polymerization initiator is a compound that can initiate a polymerization reaction of a polymerizable liquid crystal compound, etc. As the polymerization initiator, a photopolymerization initiator that generates active free radicals by the action of light is preferred from the viewpoint of being independent of the phase state of the thermotropic liquid crystal.

[0353] As long as the photopolymerization initiator is a compound capable of initiating a polymerization reaction of a polymerizable liquid crystal compound, a known photopolymerization initiator can be used. Specifically, a photopolymerization initiator capable of generating active free radicals or acids by the action of light can be cited, among which a photopolymerization initiator generating free radicals by the action of light is preferred. The photopolymerization initiator can be used alone or in combination of two or more.

[0354] As the photopolymerization initiator, a known photopolymerization initiator can be used. For example, as a photopolymerization initiator that generates active free radicals, self-cleaving benzoin compounds, acetophenone compounds, hydroxyacetophenone compounds, α-aminoacetophenone compounds, oxime ester compounds, acylphosphine oxide compounds, azo compounds, etc. can be used. Hydrogen-abstracting benzophenone compounds, alkylphenone compounds, benzoin ether compounds, benzyl ketal compounds, dibenzocycloheptenone compounds, anthraquinone compounds, xanthone compounds, thioxanthone compounds, halogenated acetophenone compounds, dialkoxyacetophenone compounds, halogenated bisimidazole compounds, halogenated triazine compounds, triazine compounds, etc. can be used. As a photopolymerization initiator that generates an acid, iodonium salts and sulfonium salts can be used. From the viewpoint of excellent reaction efficiency at low temperature, self-cleavage type photopolymerization initiators are preferred, and acetophenone compounds, hydroxyacetophenone compounds, α-aminoacetophenone compounds, and oxime ester compounds are particularly preferred.

[0355] The content of the polymerization initiator in the composition for forming an optically anisotropic layer can be appropriately adjusted according to the type and amount of the polymerizable liquid crystal compound, and is generally 0.1 to 30 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 8 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound. If the content of the polymerization initiator is within the above range, polymerization can be performed without disturbing the orientation of the polymerizable liquid crystal compound.

[0356] (Sensitizer)

[0357] The composition for forming an optically anisotropic layer may contain a sensitizer. As the sensitizer, a photosensitizer is preferred. Examples of the sensitizer include xanthone compounds such as xanthone and thioxanthone (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.); anthracene compounds such as anthracene and anthracene containing an alkoxy group (e.g., dibutoxyanthracene, etc.); phenothiazine and rubrene, etc.

[0358] When the composition for forming an optically anisotropic layer contains a sensitizer, the polymerization reaction of the polymerizable liquid crystal compound contained in the composition for forming an optically anisotropic layer can be further promoted. The amount of the sensitizer used is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound.

[0359] (Antioxidant)

[0360] The optically anisotropic layer-forming composition may contain an antioxidant from the viewpoint of stably advancing the polymerization reaction. The antioxidant can control the degree of progress of the polymerization reaction of the polymerizable liquid crystal compound.

[0361] The antioxidant may be, for example, a primary antioxidant selected from phenolic antioxidants, amine antioxidants, quinone antioxidants, and nitroso antioxidants, or an auxiliary antioxidant selected from phosphorus antioxidants and sulfur antioxidants.

[0362] When the composition for forming an optically anisotropic layer contains an antioxidant, the content of the antioxidant is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and further preferably 0.5 to 8 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound. The antioxidant may be used alone or in combination of two or more. If the content of the antioxidant is within the above range, polymerization can be performed without disturbing the orientation of the polymerizable liquid crystal compound.

[0363] <Optically anisotropic layer-forming composition; reactive additive>

[0364] The composition for forming an optically anisotropic layer may contain a reactive additive. As a reactive additive, it is preferred that a carbon-carbon unsaturated bond, an active hydrogen reactive group, or a mercapto group be present in the molecule. It should be noted that the "active hydrogen reactive group" referred to herein refers to a group reactive to a group having active hydrogen such as a carboxyl group (-COOH), a hydroxyl group (-OH), an amino group (-NH2), and representative examples thereof include a glycidyl group, an oxazoline group, a carbodiimide group, an aziridine group, an imide group, an isocyanate group, a thioisocyanate group, and a maleic anhydride group. The number of reactive groups possessed by the reactive additive is generally 1 to 20, and preferably 1 to 10.

[0365] <Polarizing film, liquid crystal retardation film>

[0366] (Protective layer)

[0367] The polarizing film or liquid crystal phase difference film (hereinafter also referred to as an optical anisotropic layer) may further have a protective layer. When the optical anisotropic layer is bonded to other films by using an adhesive or the like, the protective layer can prevent low molecular weight components such as unreacted polymerizable liquid crystal compounds and dichroic pigments in the optical anisotropic layer from diffusing into other layers.

[0368] The protective layer is preferably thin as long as it can prevent the unreacted polymerizable liquid crystal compound, dichroic pigment and other low molecular weight components in the optically anisotropic layer from diffusing into other layers. The preferred film thickness is 0.1 μm to 10 μm, more preferably 0.1 μm to 5 μm, and further preferably 0.1 μm to 3 μm.

[0369] Regarding the protective layer, a polymer with high crosslinking density or a water-soluble polymer with high hydrophilic interaction is preferred. For example, it contains at least one selected from acrylic resin, epoxy resin, oxetane resin, carbamate resin, melamine resin, and polyvinyl alcohol resin. Among them, from the viewpoint of high curability and easy formation, it is preferred to contain at least one selected from acrylic resin, epoxy resin, oxetane resin, carbamate resin, and melamine resin, and more preferably at least one selected from acrylic resin and carbamate resin. In addition, from the viewpoint of hydrophilicity, polyvinyl alcohol resin is preferred.

[0370] <Method for producing optically anisotropic layer>

[0371] The optically anisotropic layer can be produced by coating the composition for forming an optically anisotropic layer on the substrate and the alignment film.

[0372] <Coating of Composition for Forming Optically Anisotropic Layer>

[0373] As a method for applying the composition for forming an optically anisotropic layer on a substrate or an oriented film, extrusion coating, direct gravure coating, reverse gravure coating, CAP coating, slit coating, micro gravure, die coating, inkjet, etc. can be cited. In addition, a method for coating using a coating machine such as a dip coater, a rod coater, a spin coater, etc. can also be cited. Among them, in the case of continuous coating in the form of roll to roll (Roll to Roll), it is preferably a coating method using a micro gravure, inkjet, slit coating, die coating, and in the case of coating on a single substrate such as glass, a spin coating method with high uniformity is preferred. In the case of coating in the form of roll to roll (Roll to Roll), it is also possible to apply an oriented film forming composition on the substrate to form an oriented film, and further continuously apply an optically anisotropic layer forming composition on the resulting oriented film.

[0374] <Drying of the Composition for Forming an Optically Anisotropic Layer>

[0375] As a drying method for removing the solvent contained in the composition for forming an optically anisotropic layer, for example, natural drying, ventilation drying, heating drying, reduced pressure drying and a method combining them can be cited. Among them, natural drying or heating drying is preferred. The drying temperature is preferably in the range of 0 to 200° C., more preferably in the range of 20 to 150° C., and further preferably in the range of 50 to 130° C. The drying time is preferably 10 seconds to 10 minutes, more preferably 30 seconds to 5 minutes. The composition for forming a photo-aligned film and the oriented polymer composition can also be dried in the same manner.

[0376] <Polymerization of polymerizable liquid crystal compound>

[0377] As a method for polymerizing a polymerizable liquid crystal compound, photopolymerization is preferred. Photopolymerization is implemented by irradiating an active energy ray to a laminate coated with an optically anisotropic layer-forming composition containing a polymerizable liquid crystal compound on a substrate or an oriented film. As the active energy ray irradiated, it is appropriately selected according to the type of polymerizable liquid crystal compound contained in the dry film (especially the type of photopolymerizable functional group possessed by the polymerizable liquid crystal compound), the type of photopolymerization initiator in the case of containing a photopolymerization initiator, and their amount. Specifically, one or more lights selected from visible light, ultraviolet light, infrared light, X-rays, α rays, β rays and γ rays can be cited. Among them, from the aspect of easily controlling the progress of the polymerization reaction and the aspect of being able to use a device widely used in the art as a photopolymerization device, ultraviolet light is preferred, and the type of polymerizable liquid crystal compound is preferably selected in a manner that can be photopolymerized using ultraviolet light.

[0378] As the light source of the above-mentioned active energy rays, for example, there can be mentioned a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting a wavelength in the range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, a metal halide lamp, and the like.

[0379] The UV radiation intensity is usually 10mW / cm 2 ~3000mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a cationic polymerization initiator or a free radical polymerization initiator. The irradiation time is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and further preferably 10 seconds to 1 minute. If irradiated once or more times with such an ultraviolet irradiation intensity, the cumulative light amount is 10 mJ / cm 2 ~3000mJ / cm 2 , preferably 50 mJ / cm 2 ~2000mJ / cm 2 , more preferably 100 mJ / cm 2 ~1000mJ / cm 2 When the accumulated light amount is below this range, the curing of the polymerizable liquid crystal compound becomes insufficient, and good transferability may not be obtained. On the contrary, when the accumulated light amount is above this range, the optical film including the optical anisotropic layer may be colored.

[0380] [Method for manufacturing phase difference plate]

[0381] In the method for producing a retardation plate, the order of forming the first liquid crystal retardation film and the second liquid crystal retardation film is arbitrary.

[0382] Figure 2 It is a schematic cross-sectional view schematically showing a specific example of the phase difference plate 30 . Figure 2 (a) is a phase difference plate 30 in which a first liquid crystal phase difference film 31 and a second liquid crystal phase difference film 32 are stacked. Figure 2 (b) is a phase difference plate 30 in which a substrate 33, a first liquid crystal phase difference film 31, and a second liquid crystal phase difference film 32 are laminated in this order. Figure 2 (c) is a phase difference plate 30 in which a substrate 33, a second liquid crystal phase difference film 32, and a first liquid crystal phase difference film 31 are laminated in this order. Figure 2 (d) is a phase difference plate 30 in which a first liquid crystal phase difference film 31 , a substrate 33 , and a second liquid crystal phase difference film 32 are laminated in this order.

[0383] By removing the substrate from the phase difference plate 30 having the substrate 33, the phase difference plate 30 without the substrate can be obtained ( Figure 2 (a)).

[0384] In addition, the phase difference plate 30 can also be manufactured by bonding the substrate 33 having the first liquid crystal phase difference film 31 and the substrate 33' having the second liquid crystal phase difference film 32. As a specific example, Figure 2 (e), Figure 2 (f) and Figure 2 (g). A second adhesive bonding layer 34 may be used for lamination. Figure 2 In (a) to (g) of FIG. 1 , the second adhesive layer 34 is omitted from illustration.

[0385] [Method for producing optical layered body]

[0386] The optical laminate of the present embodiment can be obtained by bonding the above-mentioned phase difference plate to the above-mentioned linear polarizing plate using the first adhesive layer. As a method for bonding a phase difference plate without a substrate to a linear polarizing plate, there can be cited: a method of bonding the phase difference plate with the substrate removed to the linear polarizing plate using the first adhesive layer, and a method of removing the substrate after bonding the phase difference plate to the linear polarizing plate using the first adhesive layer. At this time, the first adhesive layer can be directly formed by applying an adhesive adhesive on the side of the phase difference film possessed by the phase difference plate, or it can be directly formed by applying an adhesive adhesive on the side of the linear polarizing plate, or the first adhesive layer pre-formed on other substrates can be between the linear polarizing plate and the phase difference plate. In the case where there is an alignment film between the substrate and the phase difference film, the alignment film can also be removed together with the substrate.

[0387] A substrate having a functional group on the surface that forms a chemical bond with a phase difference film or an alignment film tends to be difficult to remove due to the chemical bond with the phase difference film or the alignment film. Therefore, when removing the substrate by stripping, a substrate having fewer functional groups on the surface is preferred, and a substrate having no surface treatment for forming functional groups is preferred.

[0388] In addition, the alignment film having a functional group that forms a chemical bond with the substrate has a tendency to increase the adhesion between the substrate and the alignment film, so when the substrate is peeled off, an alignment film with fewer functional groups that form a chemical bond with the substrate is preferred. In addition, it is preferred that no reagent that crosslinks the substrate and the alignment film is included, and it is also preferred that no component such as a solvent that dissolves the substrate is included in the solution of the alignment polymer composition and the photo-alignment film-forming composition.

[0389] In addition, the oriented film having a functional group that forms a chemical bond with the phase difference film has a tendency that the adhesion between the phase difference film and the oriented film becomes larger. Therefore, when the oriented film is removed together with the substrate, an oriented film having fewer functional groups that form a chemical bond with the phase difference film is preferred. In addition, it is preferred that the phase difference film and the oriented film do not contain a reagent that crosslinks the phase difference film with the oriented film.

[0390] In addition, the phase difference film having a functional group that forms a chemical bond with the orientation film has a tendency that the adhesion between the orientation film and the phase difference film becomes larger. Therefore, in the case of removing the substrate or removing the orientation film together with the substrate, a phase difference film having a small number of functional groups that form a chemical bond with the substrate or the orientation film is preferred. In addition, the polymerizable liquid crystal composition preferably does not include a reagent that crosslinks the substrate or the orientation film with the phase difference film.

[0391] For example, by attaching the first adhesive layer 21 to the surface of the first liquid crystal phase difference film 31 of the phase difference plate 30 in which the substrate, the second liquid crystal phase difference film 32, the second adhesive layer 34 and the first liquid crystal phase difference film 31 are stacked in sequence, attaching the linear polarizing plate 10 thereto, and then removing the substrate of the phase difference plate 30, it is possible to manufacture a phase difference plate in which the linear polarizing plate 10, the first adhesive layer 21, the first liquid crystal phase difference film 31, the second adhesive layer 34 and the second liquid crystal phase difference film 32 are stacked in sequence. Figure 1 An optical laminate of the structure shown. In addition, by attaching a second adhesive layer to the surface of the second liquid crystal phase difference film of the phase difference plate formed by stacking the substrate, the first liquid crystal phase difference film, the first adhesive layer, and the second liquid crystal phase difference film in sequence, a linear polarizing plate is attached thereto, and then, the substrate of the phase difference plate is removed, thereby manufacturing a polarizing plate formed by stacking the linear polarizing plate, the second liquid crystal phase difference film, the first adhesive layer, and the first liquid crystal phase difference film in sequence. From the viewpoint of thin filmization, it is preferred to peel off the substrate.

[0392] The method of polishing the end surface of the optical layered body includes the following steps, for example.

[0393] [a] a first step of stacking a plurality of optical layered bodies to obtain a layered product; and

[0394] [b] A second step of cutting the end surface of the obtained laminate by relatively moving a cutting tool having a cutting edge that rotates about a rotation axis relative to the laminate along the longitudinal direction of the end surface of the obtained laminate, thereby cutting the end surface of the laminate.

[0395] [1st step]

[0396] In the method for producing the optical layered body 1 , for example, after performing the first step (the above [a]), firstly, the four sides of the optical layered body having a square shape in plan view may be polished by the second step (the above [b]).

[0397] The first step is a step of stacking a plurality of raw optical laminates cut into a predetermined shape to obtain a laminate W. The number of raw laminates contained in the laminate W is not particularly limited, and the laminate W may be, for example, a laminate formed by stacking 100 to 500 laminates. The optical laminate constituting the laminate W may be, for example, an optical laminate cut from a long strip of optical laminate having a layer structure of an optical laminate.

[0398] The second step is a step of cutting the end surface of the laminated product W obtained in the first step using the rotating tool 60 to form an optical laminate having a polished end surface.

[0399] The cutting process performed in the second step is, for example, Figure 3 As shown, it can be performed by a device having a support portion 50 and two rotating tools 60. The support portion 50 is used to press the stacked material W from above and below, and fix the stacked material W in a manner that does not move during cutting and does not cause the stacked material to shift. The rotating tool 60 is used to cut the end surface of the stacked material W and can rotate around the rotation axis R.

[0400] The support part 50 includes: a flat plate-shaped substrate (a moving mechanism for the stacked object W) 51; a door-shaped frame 52 disposed on the substrate 51; a rotating table 53 disposed on the substrate 51 and rotatable about a central axis; and a cylinder (Japanese: シリンダ) 54 provided at a position opposite to the rotating table 53 in the frame 52 and movable up and down. The stacked object W is clamped and fixed by the rotating table 53 and the cylinder 54 via a clamp 55.

[0401] The rotating tool 60 has a disc-shaped rotating body that rotates around a rotation axis R. The rotation direction of the rotating body is Figure 3In the direction indicated by the arrow in . On the disk surface of the rotating body (the surface facing the end surface of the stack W and parallel to the end surface), a plurality of (for example, 2 to 10, preferably 3 to 7) cutting edges are arranged at intervals in the rotation direction of the rotating body. The rotation axis R is preferably set to pass through the center of the disk surface of the rotating body. The cutting edge is arranged in a manner protruding from the disk surface of the rotating body toward the end surface side of the stack W. When the cutting edge abuts against the end surface of the stack W, the rotating body rotates around the rotation axis R as the center, thereby being able to cut the end surface of the stack W.

[0402] Two rotating tools 60 are provided on both sides of the substrate 51 facing each other. The rotating tools 60 can move in the direction of the rotation axis R in accordance with the size of the stacked object W, and the substrate 51 can move in a manner of passing between the two rotating tools 60. During the cutting process, the stacked object W is fixed to the support portion 50, and after the position of the rotating tools 60 in the direction of the rotation axis R is appropriately adjusted, the rotating tools 60 are rotated around their rotation axis R as the center, and the substrate 51 is moved so that the stacked object W passes between the facing rotating tools 60. Thus, the rotating tools 60 can be relatively moved relative to the stacked object W in a direction parallel to the end face of the stacked object W and orthogonal to the stacking direction, while the cutting edge of the rotating tool 60 is brought into contact with the facing exposed end faces of the stacked object W to perform cutting of these end faces.

[0403] The relative moving speed between the stack W and the rotating tool 60 can be selected, for example, from the range of 200 mm / min to 5000 mm / min (more typically, from 500 mm / min to 3000 mm / min). The rotating speed of the rotating tool 60 can be selected, for example, from the range of 2000 rpm to 8000 rpm (more typically, from 2500 rpm to 6000 rpm).

[0404] As described above, the optical laminate of the present embodiment can suppress contamination generated on the end face during the grinding process. In addition, if the second adhesive bonding layer 34 is an adhesive layer or an adhesive layer, and the storage modulus at a temperature of 80° C. is 0.02 MPa or more, further 0.3 MPa or more, and particularly 0.04 MPa or more, cracks generated during the grinding process, local defects of the second adhesive bonding layer, etc. on the end face, so-called paste deficiency (Japanese: paste deficiency け), can be suppressed, and therefore it is preferred.

[0405] [Image display device]

[0406] Figure 4 FIG. 1 is a schematic cross-sectional view schematically showing an example of an image display device of this embodiment. Figure 4 As shown, the image display device 2 has Figure 1 The optical layered body 1 and the image display panel 40 are shown. In the image display device 2, the optical layered body 1 is arranged in a direction in which the linear polarizing plate 10 side is closer to the front side than the phase difference plate 30.

[0407] When the optical stack 1 is a circular polarizing plate, in the image display device 2, the incident light from the outside includes light reflected by the optical stack 1 and light transmitted from the optical stack 1. The optical stack 1 may be a structure having an anti-reflection layer at the front, and by providing the anti-reflection layer, the light reflected on the surface of the optical stack 1 (hereinafter also referred to as "external reflected light") can be reduced. The light transmitted from the optical stack 1 is reflected by the image display panel 40 and becomes reflected light (hereinafter also referred to as "internal reflected light"), which is absorbed by the optical stack 1. The internal reflected light is preferably completely absorbed by the optical stack 1, but a part is released from the front (hereinafter, this light is also referred to as "released internal reflected light").

[0408] The optical laminate 1 may include a pressure-sensitive adhesive layer on the rear surface thereof for bonding the optical laminate 1 to the image display panel 40 , thereby forming a polarizing plate with a pressure-sensitive adhesive layer.

[0409] The image display device is not particularly limited, and examples thereof include image display devices such as organic electroluminescence (organic EL) display devices, inorganic electroluminescence (inorganic EL) display devices, liquid crystal display devices, and electroluminescence display devices.

[0410] The image display device can be used as mobile devices such as smartphones and tablets, televisions, digital photo frames, electronic signs, measuring instruments or measuring instruments, office equipment, medical equipment, electronic computing equipment, and the like.

[0411] <Other layers that the image display device may have>

[0412] The image display device 2 may include layers other than the above-mentioned layers. Other layers that the image display device 2 may include are exemplified below.

[0413] (Touch sensor panel)

[0414] The touch sensor panel is a device (sensor) for detecting (sensing) a finger or the like in contact (touching) with the screen of the image display device, and is used as an input unit for detecting the position of the finger on the screen and inputting it to the image display device. The touch sensor panel can be arranged between the optical laminate 1 and the image display panel 40, or it can be arranged on the front side of the optical laminate 1. As a touch sensor panel, as long as it is a sensor capable of detecting the touched position, the detection method is not limited, and examples of touch sensor panels such as a resistive film method, an electrostatic capacitance coupling method, an optical sensor method, an ultrasonic method, an electromagnetic induction coupling method, a surface elastic wave method, and an infrared method can be illustrated. Due to the low cost, it is preferred to use a touch sensor panel of a resistive film method and an electrostatic capacitance coupling method.

[0415] An example of a resistive film touch sensor panel is composed of a pair of substrates arranged opposite to each other, an insulating spacer sandwiched between the pair of substrates, a transparent conductive film provided on the front of the inner side of each substrate as a resistive film, and a touch position detection circuit. In an image display device provided with a resistive film touch sensor panel, if the surface of the front panel is touched, the opposing resistive films are short-circuited and current flows through the resistive films. The touch position detection circuit detects the change in voltage at this time, and the touched position is detected.

[0416] An example of a touch sensor panel of electrostatic capacitance coupling type is composed of a substrate, a transparent electrode for position detection provided on the entire surface of the substrate, and a touch position detection circuit. In an image display device provided with a touch sensor panel of electrostatic capacitance coupling type, if the surface of the front panel is touched, the transparent electrode is grounded at the touched point via the electrostatic capacitance of the human body. The touch position detection circuit detects the grounding of the transparent electrode, and the touched position is detected. The electrostatic capacitance type touch sensor panel is divided into an active area (Japanese: active area) and an inactive area (Japanese: inactive area) located outside the above-mentioned active area. The active area is an area corresponding to the area (display part) where the screen is displayed by the display panel, and is an area that senses the user's touch. The inactive area is an area corresponding to the area (non-display part) where the screen is not displayed by the display device.

[0417] The thickness of the touch sensor panel may be, for example, not less than 5 μm and not more than 2000 μm, or not less than 5 μm and not more than 100 μm.

[0418] <Flexible image display device>

[0419] The image display device may be a flexible image display device. The flexible image display device is a bendable image display device. The flexible image display device comprises an image display element assembled with an optical fingerprint authentication system and capable of being bent, and a polarizing plate of the present invention. The bendable image display element is, for example, an organic EL display panel. The polarizing plate of the present invention is arranged on the visible side relative to the organic EL display panel, and is configured in a bendable form. The polarizing plate for the flexible image display device may further comprise a front panel and a touch sensor panel.

[0420] Preferably, a front panel, a polarizing plate of the present invention and a touch sensor panel are stacked in sequence from the visible side, or a front panel, a touch sensor panel and a polarizing plate of the present invention are stacked in sequence from the visible side. If there is a polarizer on the visible side relative to the touch sensor panel, it is not easy to observe the pattern of the touch sensor panel. As a result, the visibility of the displayed image becomes better. Therefore, it is further preferred to have a polarizing plate of the present invention on the visible side relative to the touch sensor panel, that is, a front panel, a polarizing plate of the present invention and a touch sensor panel are sequentially provided. Each component can be stacked using an adhesive, an adhesive, etc. In addition, a shading pattern formed on at least one side of any layer of the front panel, the polarizing plate, and the touch sensor panel can be provided.

[0421] In a flexible image display device having a front panel, a polarizing plate of the present invention and a bendable image display panel from the visible side, the front panel and the polarizing plate of the present invention constitute a polarizing plate with a front panel having a polarizing plate and a front panel. In the polarizing plate with a front panel, the front panel is usually arranged on the visible side of the polarizing plate, for example, by laminating with the polarizing plate using an adhesive or bonding agent.

[0422] In a flexible image display device having a touch sensor panel, a polarizing plate of the present invention, and a bendable image display panel from the visible side, the touch sensor panel and the polarizing plate of the present invention constitute a polarizing plate with a touch sensor panel having a polarizing plate and a touch sensor panel. In addition, in a flexible image display device having a polarizing plate of the present invention, a touch sensor panel, and a bendable image display element from the visible side, the touch sensor panel and the polarizing plate of the present invention constitute a polarizing plate with a touch sensor panel having a polarizing plate and a touch sensor panel. In the polarizing plate with a touch sensor panel, the touch sensor panel can be arranged on the back side (the side opposite to the visible side) compared to the polarizing plate, or it can be arranged on the visible side compared to the polarizing plate. The touch sensor panel and the polarizing plate are stacked, for example, by an adhesive or a bonding agent.

[0423] The polarizing plate of the present invention may be used as a polarizing plate with a front plate by laminating a front plate on the viewing side thereof. The polarizing plate with a front plate comprises the polarizing plate of the present invention and a front plate disposed on the viewing side thereof.

[0424] (Front Panel)

[0425] As the front panel, there can be cited a front panel including a hard coating on at least one side of glass or a resin film. As glass, for example, high-transmittance glass or tempered glass can be used. When using a particularly thin transparent surface material, chemically tempered glass is preferably used. The thickness of the glass can be, for example, 50 μm to 5 mm.

[0426] The front panel including a hard coating layer on at least one side of the resin film may not be rigid like conventional glass but may have flexible properties. The thickness of the hard coating layer is not particularly limited and may be, for example, 5 μm to 100 μm.

[0427] The resin film may be, for example, a film formed of a macromolecule such as a cycloolefin derivative having a unit of a monomer containing a cycloolefin such as norbornene or a polycyclic norbornene-based monomer, cellulose (diacetylcellulose, triacetylcellulose, acetylcellulose butyrate, isobutylcellulose, propionylcellulose, butyrylcellulose, acetylpropionylcellulose), ethylene-vinyl acetate copolymer, polycycloolefin, polyester, polystyrene, polyamide, polyetherimide, polyacrylic acid, polyimide, polyamideimide, polyethersulfone, polysulfone, polyethylene, polypropylene, polymethylpentene, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl acetal, polyetherketone, polyetheretherketone, polyethersulfone, polymethyl methacrylate, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyurethane, epoxy resin, etc. These macromolecules may be used alone or in combination of two or more.

[0428] The resin film may be an unstretched film or a stretched film, such as a uniaxially stretched film or a biaxially stretched film. As the resin film, from the aspect of excellent transparency and heat resistance, polyamide-imide film, polyimide film, uniaxially stretched polyester film, biaxially stretched polyester film are preferred. From the aspect of excellent transparency and heat resistance and the ability to cope with the large-scale film, cycloolefin derivative film and polymethyl methacrylate film are preferred. From the aspect of relatively easy to obtain a transparent and optically non-anisotropic resin film, triacetyl cellulose and isobutyl cellulose film are preferred. The thickness of the resin film is usually 5 to 200 μm, preferably 20 to 100 μm.

[0429] (Shading pattern)

[0430] The shading pattern is a component also called a frame, which can be formed on the display element side of the front panel. By having a shading pattern, the various wirings constituting the display device can be hidden without being observed by the user. There is no particular restriction on the color and material of the shading pattern, and it can be formed with a resin material having a variety of colors such as black, white, and gold. In one embodiment, the thickness of the shading pattern can be 2μm to 50μm, preferably 4μm to 30μm, and more preferably in the range of 6μm to 15μm. In addition, in order to suppress the mixing of bubbles caused by the height difference between the shading pattern and the display portion and the visibility of the boundary portion, the shading pattern can be given a shape.

[0431] [Example]

[0432] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples. The amounts expressed in "%" and "parts" in Examples and Comparative Examples are by mass % and by mass unless otherwise specified.

[0433] [Production of optical laminate]

[0434] 1. Preparation of Adhesive Composition

[0435] (1) Preparation of Adhesive 1 (Active Energy Ray-Curing Adhesive)

[0436] The following components were blended and mixed, and then degassed to prepare an active energy ray-curable adhesive.

[0437] [Cationically polymerizable compound]

[0438] Neopentyl glycol diglycidyl ether (trade name: EX-211L, manufactured by Nagase ChemteX Co., Ltd.) 30 parts by mass

[0439] 3-Ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane (trade name: OXT-221, manufactured by Toagosei Co., Ltd.) 13 parts by mass

[0440] · Bisphenol A type epoxy resin (trade name: EP-4100E, ADEKA Co., Ltd., viscosity 13 Pa·s (temperature 25° C.)) 45 parts by mass

[0441] · Aromatic oxetane compound (trade name: TCM-104, manufactured by TRONLY) 12 parts by mass

[0442] [Photocationic polymerization initiator]

[0443] CPI-100P, manufactured by San-Apro Co., Ltd., 50% propylene carbonate solution 2.25 parts by mass (solid content)

[0444] [Photosensitizing agent]

[0445] 1,4-diethoxynaphthalene 1 part by mass

[0446] The storage modulus of the adhesive 1 at a temperature of 23° C. was 2.45 GPa, the storage modulus at a temperature of 80° C. was 0.03 GPa, and the refractive index with respect to light of a wavelength of 589 nm was 1.54.

[0447] (2) Preparation of Adhesive 2 (Active Energy Ray-Curing Adhesive)

[0448] The following components were blended and mixed, and then degassed to prepare an active energy ray-curable adhesive.

[0449] [Cationically polymerizable compound]

[0450] 3',4'-Epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate (trade name: CEL2021P, manufactured by Daicel Corporation): 70 parts by mass

[0451] Neopentyl glycol diglycidyl ether (trade name: EX-211, manufactured by Nagase ChemteX Co., Ltd.): 20 parts by mass

[0452] 2-Ethylhexyl glycidyl ether (trade name: EX-121, manufactured by Nagase ChemteX Co., Ltd.): 10 parts by mass

[0453] [Photocationic polymerization initiator]

[0454] Cationic polymerization initiator (trade name: CPI-100P_50% solution propylene carbonate solution, manufactured by San-Apro Co., Ltd.)

[0455] : 4.5 parts by mass (substantial solid content 2.25 parts by mass)

[0456] [Photosensitizing agent]

[0457] 1,4-Diethoxynaphthalene: 2 parts by mass

[0458] The storage modulus of the adhesive 2 at a temperature of 23° C. was 2.63 GPa, the storage modulus at a temperature of 80° C. was 0.8 GPa, and the refractive index with respect to light of a wavelength of 589 nm was 1.51.

[0459] (3) Determination of storage modulus of adhesive

[0460] The prepared adhesive was applied to one side of a polyethylene terephthalate film (trade name "TOYOBOESTER Film E7002", manufactured by TOYOBO Co., Ltd.) using a coater (bar coater, manufactured by Daiichi Rika Co., Ltd.) so that the film thickness after curing would be about 10 μm. Next, an ultraviolet irradiation device (manufactured by Fusion UV Systems Co., Ltd.) was used to irradiate the film at a cumulative light intensity of 600 mJ / cm 2 (UV-B) irradiates ultraviolet rays to cure the adhesive. Cut it into a size of 5 mm × 30 mm, peel off the polyethylene terephthalate film, and obtain a cured film of the adhesive. For the cured film thus obtained, use the dynamic viscoelasticity measuring device "DVA-220" manufactured by IT Measurement and Control Co., Ltd. in a manner such that its long side becomes the stretching direction, hold it with a clamp interval of 2 cm, set the frequency of stretching and shrinking to 1 Hz, set the heating rate to 3°C / min, and calculate the storage modulus at temperatures of 23°C and 80°C.

[0461] (4) Measurement of the refractive index of the adhesive

[0462] The prepared adhesive was applied to one side of a stretched norbornene-based resin film [ZEONOR Film, manufactured by ZEON Corporation] using a bar coater [manufactured by Daiichi Rika Co., Ltd.], and then irradiated with an ultraviolet irradiation device [manufactured by Fusion UV Systems Co., Ltd.] at a cumulative light intensity of 600 mJ / cm 2 (UV-B) ultraviolet rays were irradiated to obtain a cured product. The film thickness of the cured product was about 30 μm. The norbornene-based resin film was peeled off from the cured product, and the refractive index (589 nm) of the cured product layer was measured using a multi-wavelength Abbe refractometer [“DR-M2” manufactured by ATAGO Co., Ltd.] at 25°C.

[0463] 2. Preparation of Adhesive Layer

[0464] (1) Preparation of Adhesive Layer 1 (Acrylic Adhesive Layer)

[0465] (Preparation of acrylic resin solution 1)

[0466] A mixed solution of 100 parts of ethyl acetate, 99.0 parts of butyl acrylate, 0.5 parts of 2-hydroxyethyl acrylate and 0.5 parts of acrylic acid was placed in a reaction container equipped with a condenser, a nitrogen inlet tube, a thermometer and a stirrer, and the internal temperature was raised to 55°C while replacing the air in the device with nitrogen to make it oxygen-free. Then, the entire amount of a solution prepared by dissolving 0.12 parts of azobisisobutyronitrile (polymerization initiator) in 10 parts of ethyl acetate was added. After adding the polymerization initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction container at an addition rate of 17.3 parts / hr while the internal temperature was maintained at 54-56°C. The addition of ethyl acetate was stopped at the time when the concentration of the (meth)acrylic resin reached 35% by mass, and the temperature was further maintained at the same temperature until 6 hours had passed since the addition of ethyl acetate was started. Finally, ethyl acetate was added to adjust the concentration of the (meth)acrylic resin to 20% by mass, and an acrylic resin solution 1 was prepared. The weight average molecular weight Mw of the obtained acrylic resin was 1.7 million, and the molecular weight distribution Mw / Mn was 3.9. It should be noted that Mw and Mn were measured as follows: two "TSKgelGMH" manufactured by Tosoh Corporation were connected in series in a GPC apparatus. HR -H(S)" as the column, tetrahydrofuran as the eluent, under the conditions of sample concentration 2 mg / mL, sample introduction volume 100 μL, temperature 40°C, flow rate 1 mL / min, measured by standard polystyrene conversion.

[0467] (Preparation of Adhesive Composition 1)

[0468] To 80 parts of the solid content of the acrylic resin solution 1 obtained above, 20 parts (solid content) of a difunctional acrylate (obtained from Shin-Nakamura Chemical Co., Ltd.; model "A-DOG"), 2.5 parts of a crosslinking agent (manufactured by Tosoh Corporation: trade name "Coronate L" (ethyl acetate solution of trimethylolpropane adduct of toluene diisocyanate (solid content concentration 75 mass%)) based on the effective ingredient, 1.5 parts of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals: trade name "Irgacure500"), and 0.3 parts of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name "KBM-403") were added, and ethyl acetate was further added in a manner to give a solid content concentration of 13%, thereby obtaining an adhesive composition 1. A-DOG is a diacrylate of an acetal compound of hydroxypivalaldehyde and trimethylolpropane, and has the structure of the following formula.

[0469]

[0470] (Preparation of Adhesive Layer 1)

[0471] Using an applicator, the adhesive composition 1 prepared above was applied to the release-treated surface of a spacer comprising a polyethylene terephthalate film ["PLZ-383030" obtained from LINTEC Co., Ltd.] that had been subjected to a release treatment in such a manner that the thickness after drying was 5 μm, and dried at 100°C for 1 minute to prepare an adhesive layer (adhesive sheet). Next, the surface of the obtained adhesive layer on the opposite side of the spacer was bonded to the release-treated surface of a spacer comprising a polyethylene terephthalate film ["PLR-381031" obtained from LINTEC Co., Ltd.] that had been subjected to a release treatment. Next, ultraviolet rays were irradiated under the following conditions to prepare an adhesive layer 1. The storage modulus of the obtained adhesive layer at a temperature of 23°C was 0.13 MPa, the storage modulus at a temperature of 80°C was 0.054 MPa, and the refractive index relative to light of a wavelength of 589 nm was 1.48.

[0472] <UV irradiation conditions>

[0473] ·Use Fusion UV lamp system (Fusion UV Systems) H Bulb

[0474] ·The cumulative amount of UVA in the UV wavelength region is 250mJ / cm 2 (Measurement device: measured value based on UV PowerPuckII manufactured by FusionUV)

[0475] (2) Preparation of Adhesive Layer 2 (Acrylic Adhesive Layer)

[0476] (Preparation of acrylic resin solution 2)

[0477] A mixed solution of 81.8 parts of ethyl acetate, 90.0 parts of butyl acrylate, 5.0 parts of methyl acrylate and 5.0 parts of acrylic acid was placed in a reaction vessel equipped with a condenser, a nitrogen inlet tube, a thermometer and a stirrer, and the internal temperature was raised to 55°C while replacing the air in the device with nitrogen to make it oxygen-free. Then, the entire amount of a solution prepared by dissolving 0.15 parts of azobisisobutyronitrile (polymerization initiator) in 10 parts of ethyl acetate was added. After adding the polymerization initiator, the temperature was maintained for 1 hour, and then ethyl acetate was continuously added to the reaction vessel at an addition rate of 17.3 parts / hr while the internal temperature was maintained at 54-56°C. The addition of ethyl acetate was stopped at the time when the concentration of the (meth)acrylic resin reached 35% by mass, and the temperature was further maintained at the same temperature until 6 hours had passed since the addition of ethyl acetate was started. Finally, ethyl acetate was added to adjust the concentration of the (meth)acrylic resin to 20% by mass, thereby preparing an acrylic resin solution 2. The weight average molecular weight Mw of the obtained acrylic resin was 1.6 million, and the molecular weight distribution Mw / Mn was 4.5. It should be noted that Mw and Mn were measured as follows: two "TSKgel GMH" manufactured by Tosoh Corporation were connected in series in a GPC apparatus. HR -H(S)" as the column, tetrahydrofuran as the eluent, under the conditions of sample concentration 2 mg / mL, sample introduction volume 100 μL, temperature 40°C, flow rate 1 mL / min, measured by standard polystyrene conversion.

[0478] (Preparation of Adhesive Composition 2)

[0479] To 100 parts of the solid content of the acrylic resin solution 2 obtained above, 0.15 parts of a cross-linking agent (manufactured by Tosoh Corporation: trade name "Coronate L" (ethyl acetate solution of trimethylolpropane adduct of toluene diisocyanate (solid content concentration 75 mass %)) and 0.2 parts of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name "KBM-403") were added in an effective ingredient basis, and ethyl acetate was further added in a manner to give a solid content concentration of 13%, thereby obtaining an adhesive composition 2.

[0480] (Preparation of Adhesive Layer 2)

[0481] The adhesive composition 2 prepared above was applied to the release-treated surface of a separator including a polyethylene terephthalate film ["PLR-382190" obtained from LINTEC Co., Ltd.] subjected to a release treatment using an applicator so that the thickness after drying was the thickness shown in Table 3, and dried at 100°C for 1 minute to prepare an adhesive layer. Next, the surface of the obtained adhesive layer on the opposite side to the separator was bonded to the release-treated surface of a separator including a polyethylene terephthalate film ["PET-251130" obtained from LINTEC Co., Ltd.] subjected to a release treatment, and then irradiated with ultraviolet rays under the same conditions as those in the preparation of the adhesive layer 1 to prepare an adhesive layer 2. The storage modulus of the obtained adhesive layer 2 at a temperature of 23°C was 0.026 MPa, the storage modulus at a temperature of 80°C was 0.019 MPa, and the refractive index with respect to light of a wavelength of 589 nm was 1.48.

[0482] (3) Measurement of storage modulus of adhesive layer

[0483] The storage modulus of the adhesive layer at 23°C and 80°C was measured using a viscoelasticity measuring device (MCR-301, Anton Paar). After the adhesive sheet was cut into 30 mm wide x 30 mm long, the spacer was peeled off, and multiple sheets were stacked in a manner to have a thickness of 200 μm and attached to a measuring table. Then, the sheet was bonded to a parallel plate with a diameter of 25 mm and measured in a temperature range of 20°C to 85°C, a frequency of 1.0 Hz, a deformation of 1%, and a heating rate of 10°C / min to obtain the storage modulus G' at 23°C and 80°C.

[0484] (4) Measurement of refractive index of adhesive layer

[0485] The refractive index (589 nm) of the obtained pressure-sensitive adhesive layer was measured under a 25° C. environment using a multi-wavelength Abbe refractometer [“DR-M2” manufactured by ATAGO Corporation].

[0486] 3. Preparation of polarizing film

[0487] A polyvinyl alcohol film having a thickness of 20 μm, a degree of polymerization of 2400, and a saponification degree of 99% or more is uniaxially stretched on a hot roller to a stretching ratio of 4.5 times, and while maintaining a tense state, is immersed in a dyeing bath at 28° C. containing 0.05 parts by mass of iodine and 5 parts by mass of potassium iodide relative to 100 parts by mass of water for 60 seconds.

[0488] Next, the film was immersed in a 64°C boric acid aqueous solution 1 containing 5.5 parts by mass of boric acid and 15 parts by mass of potassium iodide relative to 100 parts by mass of water for 110 seconds. Next, the film was immersed in a 67°C boric acid aqueous solution 2 containing 5.5 parts by mass of boric acid and 15 parts by mass of potassium iodide relative to 100 parts by mass of water for 30 seconds. Then, the film was washed with pure water at 10°C and dried to obtain a polarizer. The thickness of the polarizer was 8 μm and the boron content was 4.3% by mass.

[0489] 4. Preparation of Water-Based Adhesive

[0490] 3 parts by mass of carboxyl-modified polyvinyl alcohol ["KL-318" manufactured by Kuraray Co., Ltd.] were dissolved in 100 parts by mass of water to prepare a polyvinyl alcohol aqueous solution. A water-soluble polyamide epoxy resin ("Sumirez Resin 650 (30)" manufactured by Taoka Chemical Industry Co., Ltd., solid content concentration 30% by mass) was mixed in the obtained aqueous solution at a ratio of 1.5 parts by mass to 100 parts by mass of water to obtain a water-based adhesive.

[0491] 5. Fabrication of Linear Polarization Plate

[0492] On both sides of the polarizing film prepared above, a cyclic polyolefin resin film (HC-COP) with a hard coating (HC) layer as the first protective film and a triacetyl cellulose film (TAC) as the second protective film are bonded using a roll laminating machine with the aid of the aqueous adhesive obtained above. After bonding, a drying treatment is performed at 80°C for 3 minutes. The obtained roll is cut into a rectangle in such a way that the longitudinal direction becomes the absorption axis of PVA, and a linear polarizing plate 10 having protective films laminated on both sides of the polarizing film is obtained. The linear polarizing plate 10 has a layer structure of first protective film / adhesive layer / polarizer / adhesive layer / second protective film. The refractive index of the second protective film relative to light of a wavelength of 589nm is 1.48.

[0493] 6. Preparation of the First Liquid Crystal Retardation Film and the Second Liquid Crystal Retardation Film

[0494] (1) Preparation of oriented polymer composition (1)

[0495] Water was added to commercially available polyvinyl alcohol (polyvinyl alcohol 1000 completely saponified type, manufactured by Wako Pure Chemical Industries, Ltd.), and the mixture was heated at 100° C. for 1 hour to obtain an oriented polymer composition (1).

[0496] (2) Preparation of photo-aligned polymer composition (1)

[0497] The photo-alignment material of the following structure (weight average molecular weight: 50000, m:n=50:50) was produced according to the method described in Japanese Patent Application Laid-Open No. 2021-196514. 2 parts of the photo-alignment material and 98 parts of propylene glycol monomethyl ether (PGME, solvent) were mixed as components, and the obtained mixture was stirred at 80° C. for 1 hour to prepare a photo-alignment polymer composition (1).

[0498] Photo-oriented materials:

[0499]

[0500] (3) Production of polymerizable liquid crystal compounds

[0501] A polymerizable liquid crystal compound (A1) and a polymerizable liquid crystal compound (A2) having the structures shown below were prepared respectively. The polymerizable liquid crystal compound (A1) and the polymerizable liquid crystal compound (A2) were prepared in the same manner as the method described in JP-A-2010-244038.

[0502] Polymerizable liquid crystal compound (A1):

[0503]

[0504] Polymerizable liquid crystal compound (A2):

[0505]

[0506] (4) Preparation of Liquid Crystal Retardation Film-Forming Composition (Y1)

[0507] The polymerizable liquid crystal compound (A1) and the polymerizable liquid crystal compound (A2) were mixed in a mass ratio of 80:20 to obtain a mixture. With respect to 100 parts of the obtained mixture, a leveling agent "Megaface F-556" (manufactured by DIC), "Omnirad907" (manufactured by IGM Resin BV) as a photopolymerization initiator, and an ionic compound (B) were added. Furthermore, cyclopentanone was added, and the mixture was stirred at a temperature of 80°C for 1 hour to prepare a phase difference film forming composition (Y1). The addition amount of each component is shown in Table 1 below.

[0508] [Table 1]

[0509] Polymerizable liquid crystal compound (A1) 80 servings Polymerizable liquid crystal compound (A2) 20 servings Megaface F-556 0.1 part Omnirad907 2.5 servings Ionic compounds (B) 0.1 part Cyclopentanone 650 copies

[0510] Ionic compounds (B):

[0511]

[0512] (5) Preparation of Liquid Crystal Retardation Film-Forming Composition (Y2)

[0513] A polymerizable liquid crystal compound Paliocolor LC242 (manufactured by BASF Japan), a leveling agent "BYK-361N" (manufactured by BYK-Chemie) and a photopolymerization initiator "Omnirad907" (manufactured by IGM Resin BV) were added. Further, propylene glycol-1-monomethyl ether-2-acetate (PGME) was added, and the mixture was stirred at a temperature of 80° C. for 1 hour to prepare a phase difference film forming composition (Y2). The addition amount of each component is shown in Table 2 below.

[0514] [Table 2]

[0515] Polymerizable liquid crystal compound LC242 100 copies BYK-361N 0.1 part Omnirad907 2.5 servings PGME 400 copies

[0516] Polymerizable liquid crystal compound LC242:

[0517]

[0518] (6) Preparation of the First Liquid Crystal Retardation Film (Z1)

[0519] An oriented polymer composition (1) is coated on a triacetylcellulose film (TAC) (manufactured by Konica Minolta Co., Ltd., KC4UY) cut into a rectangular shape to form an oriented polymer film in such a manner that the thickness after heating and drying becomes 100 nm. The surface of the obtained oriented polymer film is subjected to a friction treatment so that the slow axis of the phase difference film (Z1) formed below forms an angle of -15° with the longitudinal direction of the above-mentioned TAC, and a phase difference layer forming composition (Y1) is coated thereon using a rod coater. The obtained coated film is dried at 100°C for 1 minute and then cooled to room temperature to obtain a dry film. Next, a high-pressure mercury lamp ("Unicure VB-15201BY-A" manufactured by USHIO Electric Co., Ltd.) is used to irradiate the above-mentioned dry film with an exposure amount of 1000mJ / cm2 in a nitrogen atmosphere. 2(365nm reference) ultraviolet light, thereby forming a first liquid crystal phase difference film (X1) in which the polymerizable liquid crystal compound is solidified in a state of being oriented in a horizontal direction relative to the substrate surface, and a phase difference film (Z1) comprising TAC / oriented film / first liquid crystal phase difference film (X1) (horizontally oriented liquid crystal solidified film) is obtained. The film thickness of the obtained first liquid crystal phase difference film (X1) was measured using a laser microscope, and the result was 1.8μm. The in-plane phase difference value was measured using KOBRA-WR manufactured by Prince Instruments Co., Ltd. As a result, the in-plane phase difference value at a wavelength of 550nm is Re(550)=270nm, and the in-plane phase difference value at a wavelength of 450nm is Re(450)=291nm. It should be noted that the phase difference value of TAC at a wavelength of 550nm is approximately 0, so it has no effect on the optical properties. The orientation angle is -15° relative to the length direction of the above-mentioned TAC. The first liquid crystal phase difference film satisfies formula (2).

[0520] (7) Preparation of the Second Liquid Crystal Retardation Film (Z2)

[0521] A photo-oriented polymer composition (1) was applied to a triacetylcellulose film (TAC) (manufactured by Konica Minolta Co., Ltd., KC4UY) cut into a rectangular shape. The obtained coating film was dried at 120°C for 2 minutes, and then cooled to room temperature to form a dry film. Furthermore, using a UV irradiation device, 100 mJ (313 nm reference) of polarized ultraviolet light was continuously irradiated at 75° relative to the length direction of the TAC to form a 100 nm photo-oriented film. A phase difference film forming composition (Y2) was applied thereon using a rod coater. The obtained coating film was dried at 100°C for 1 minute, and then cooled to room temperature to obtain a dry film. Next, a high-pressure mercury lamp was used to continuously irradiate the above-mentioned dry film with an exposure amount of 1000 mJ / cm 2(365nm reference) ultraviolet light, thereby forming a second liquid crystal phase difference film (X2) formed by curing the polymerizable liquid crystal compound in a state of being oriented in a horizontal direction relative to the substrate surface, and obtaining a phase difference film (Z2) comprising TAC / oriented film / second liquid crystal phase difference film (X2) (horizontally oriented liquid crystal cured film). The film thickness of the obtained second liquid crystal phase difference film (X2) was measured using a laser microscope, and the result was 1.0μm. The in-plane phase difference value was measured using KOBRA-WR manufactured by Prince Instruments Co., Ltd. As a result, the in-plane phase difference value at a wavelength of 550nm was Re(550)=142nm, and the in-plane phase difference value at a wavelength of 450nm was Re(450)=153.4nm. It should be noted that the phase difference value of TAC at a wavelength of 550nm is approximately 0, which has no effect on the optical properties. The orientation angle is 75° relative to the length direction of the above-mentioned TAC. The second liquid crystal phase difference film satisfies formula (3).

[0522] 7. Preparation of optical layered body (Examples 1 to 10, Comparative Examples 1 to 3)

[0523] (1) Fabrication of phase difference plate

[0524] The first liquid crystal retardation film (X1) of the first liquid crystal retardation film (Z1) and the second liquid crystal retardation film (X2) of the second liquid crystal retardation film (Z2) were subjected to corona treatment, respectively. Then, the corona-treated surfaces of the two were laminated with the aid of the second adhesive bonding layer described in Tables 3 and 4, to obtain a retardation plate in which TAC / aligned film / first liquid crystal retardation film (X2) / second adhesive bonding layer / second liquid crystal retardation film (X1) / aligned film / TAC were laminated in sequence.

[0525] When adhesives 1 and 2 are used to form the second adhesive bonding layer, the phase difference plate is produced as follows. An adhesive is applied to the corona-treated surface of either the first liquid crystal phase difference film (X1) or the second liquid crystal phase difference film (X2), and the first liquid crystal phase difference film (Z1) and the second liquid crystal phase difference film (Z2) are bonded together. Ultraviolet rays are irradiated from the side of the second liquid crystal phase difference film (Z2) to cure the ultraviolet curable adhesive and form an adhesive layer (second adhesive bonding layer). The UVA with a wavelength of 320nm to 390nm becomes 420mJ / cm 2 The thickness of the adhesive layer after curing was measured using a laser microscope (manufactured by Olympus Corporation, “LEXT”). The results are shown in Tables 3 and 4.

[0526] When the second adhesive bonding layer is formed using the adhesive layers 1 and 2, the phase difference plate is produced as follows: The first liquid crystal phase difference film (Z1) and the second liquid crystal phase difference film (Z2) are bonded together by placing the adhesive layers 1 and 2 between the first liquid crystal phase difference film (X1) and the second liquid crystal phase difference film (X2).

[0527] (Corona treatment)

[0528] The corona treatment apparatus used was AGF-B 10 manufactured by Kasuga Electric Co., Ltd. The corona treatment was performed once using the above-mentioned corona treatment apparatus under the conditions of an output of 0.3 kW and a treatment speed of 3 m / min.

[0529] (2) Preparation of optical laminate

[0530] The TAC substrate of the first liquid crystal retardation film (X1) is peeled off from the retardation plate formed by stacking TAC / oriented film / first liquid crystal retardation film (X1) / second adhesive layer / second liquid crystal retardation film (X2) / oriented film / TAC in sequence. The surface of the oriented film exposing the first liquid crystal retardation film (X1) and the surface of the second protective film (TAC film) of the linear polarizing plate 1 are laminated with the aid of the first adhesive layer described in Tables 3 and 4 in such a way that their respective longitudinal directions are in the same direction. The TAC substrate of the second liquid crystal retardation film (X2) is peeled off from the retardation plate to obtain an optical laminate. After the optical laminate is formed, the spacer on one side of the adhesive layer 2 prepared in a manner to have a thickness of 25 μm is peeled off and attached to the oriented film surface of the second liquid crystal retardation film (X2) of the optical laminate. Based on Figure 3 The end faces were polished by the method described in to obtain optical layered bodies of Examples 1 to 10 and Comparative Examples 1 to 3.

[0531] 8. Evaluation

[0532] (1) Inspection of uneven interference

[0533] After affixing an acrylic adhesive (film thickness of 25 μm) to the surface of the phase difference plate side of the optical laminate of the embodiment and the comparative example, it was cut into a size of 150 mm × 150 mm. The cut optical laminate with acrylic adhesive was attached to an aluminum reflector to obtain a test piece for observing interference unevenness. The test piece for observing interference unevenness was set on a table in such a way that the angle formed with the ground when the ground was set to 0° was 45°. A linear polarizing plate was set between the 3-wavelength fluorescent lamp as a light source and the test piece for observing interference unevenness. The test piece for observing interference unevenness was irradiated with light from the 3-wavelength fluorescent lamp from a direction of 90° (above the test piece for observing interference unevenness). When the observer observes the test piece from the 0° direction, the polarizing plate is set in a manner orthogonal to the absorption axis of the linear polarizing plate set in the 3-wavelength fluorescent lamp, and the sample is observed via the set polarizing plate.

[0534] A: No interference unevenness was observed

[0535] B: Slightly uneven interference is observed, but weaker than C

[0536] C: Slightly uneven interference is observed

[0537] D: Uneven interference is observed

[0538] (2) Determination of reflectivity

[0539] After the surface of the phase difference plate side of the optical laminate of the embodiment and the comparative example is bonded with an acrylic adhesive (film thickness 25 μm), it is cut into a size of 150 mm × 150 mm. The cut optical laminate with an acrylic adhesive is attached to a glass plate (Corning, Eagle XG, 0.7 mmt) in a manner that the adhesive side becomes the glass plate side, and a sample for measurement is prepared. The glass plate side of the sample for measurement is placed on a reflective plate (Alanod, MIRO5 5011GP) in a manner that the glass plate side of the sample for measurement is in contact with the reflective plate, and the reflectivity is measured using a spectrophotometer (CM2600d, KONICA MINOLTA Co., Ltd.). For the measurement, a mask with a diameter of φ of 8.0 mm for the opening when the light enters the integrating sphere from the evaluation sample is installed, and the reflectivity of the central part of the sample for measurement is measured in SCI mode.

[0540] A: 4.95% or more and less than 5.00%

[0541] B: 5.00% or more and less than 5.05%

[0542] C: 5.05% or more and less than 5.20%

[0543] D: 5.20% or more

[0544] (3) Evaluation of end surface grinding

[0545] 300 optical layered bodies were stacked and their end faces were polished using a rotating tool. One optical layered body was taken out from the polished layered body and its end face was observed using an optical microscope (VHX-7000, 100 times field of view) to evaluate the maximum size of cracks and paste defects.

[0546] A: The maximum size of cracks and paste defects is less than 100μm

[0547] B: The maximum size of cracks and paste defects is 100 μm or more and less than 250 μm

[0548] C: The maximum size of cracks and paste defects is 250 μm or more and less than 500 μm

[0549] D: The maximum size of cracks and paste defects is 500 μm or more

[0550] [Table 3]

[0551]

[0552]

Claims

1. An optical laminate, which is an optical laminate comprising a first protective film, an adhesive layer, a polarizer, an adhesive layer, a second protective film, a first adhesive bonding layer, a first liquid crystal retardation film, a second adhesive bonding layer, and a second liquid crystal retardation film laminated in sequence. When the refractive index of the second protective film with respect to light of a wavelength of 589 nm is N aII The refractive index of the first adhesive layer with respect to light of wavelength 589 nm is N bI When the second protective film and the first adhesive bonding layer satisfy the following formula (1): |N aII -N bI |<0.1···(1), The first liquid crystal retardation film and the second liquid crystal retardation film each independently satisfy the following formula (2) or formula (3): nx>ny≥nz···(2) nx<ny≤nz···(3), The thickness of the second adhesive layer is 2.8 μm to 20 μm. In formulas (2) and (3), nx represents the principal refractive index in the refractive index ellipsoid formed by the first liquid crystal retardation film or the second liquid crystal retardation film in a direction parallel to the plane of the first liquid crystal retardation film or the second liquid crystal retardation film, ny represents the refractive index in the refractive index ellipsoid in a direction parallel to the plane and orthogonal to the direction of nx, and nz represents the refractive index in the refractive index ellipsoid in a direction perpendicular to the plane.

2. The optical layered body according to claim 1, wherein: The thickness of the first adhesive layer is in the range of 1 μm to 3 μm.

3. The optical layered body according to claim 1 or 2, wherein: The refractive index N of the first adhesive layer bI It is 1.48~1.

54.

4. The optical layered body according to claim 1 or 2, wherein: The refractive index of the second tackiness adhesive layer with respect to light of a wavelength of 589 nm is 1.50 to 1.

57.

5. The optical layered body according to claim 1 or 2, wherein: The second adhesive layer has a storage modulus of 0.04 MPa or more at a temperature of 80°C.

6. The optical layered body according to claim 1 or 2, wherein: The first adhesive layer has a storage modulus of 0.02 GPa or more and 5 GPa or less at a temperature of 80° C.

7. An optical laminate, which is an optical laminate comprising a first protective film, an adhesive layer, a polarizer, an adhesive layer, a second protective film, a first adhesive bonding layer, a first liquid crystal retardation film, a second adhesive bonding layer, and a second liquid crystal retardation film laminated in sequence. The storage modulus of the first adhesive layer at a temperature of 80° C. is greater than 0.4 GPa. The first liquid crystal retardation film and the second liquid crystal retardation film each independently satisfy the following formula (2) or formula (3): nx>ny≥nz···(2) nx<ny≤nz···(3), The thickness of the second adhesive layer is 2.8 μm to 20 μm. In formula (2) and formula (3), nx represents the principal refractive index in the refractive index ellipsoid formed by the first liquid crystal retardation film or the second liquid crystal retardation film in a direction parallel to the plane of the first liquid crystal retardation film or the second liquid crystal retardation film, ny represents the refractive index in the refractive index ellipsoid in a direction parallel to the plane and orthogonal to the direction of nx, and nz represents the refractive index in the refractive index ellipsoid in a direction perpendicular to the plane.

8. The optical layered body according to claim 7, wherein: The thickness of the first adhesive layer is in the range of 1 μm to 3 μm.

9. The optical layered body according to claim 7 or 8, wherein: The refractive index N of the first adhesive layer with respect to light of wavelength 589 nm is bI It is 1.48~1.

54.

10. The optical layered body according to claim 7 or 8, wherein: The refractive index of the second tackiness adhesive layer with respect to light of a wavelength of 589 nm is 1.50 to 1.

57.

11. The optical layered body according to claim 7 or 8, wherein: The second adhesive layer has a storage modulus of 0.04 MPa or more at a temperature of 80°C.