Calculation method for multi-channel lap joint rate of laser cladding

By establishing a relationship model between the cross-section profile characteristic parameters of single-pass cladding and the critical overlap rate of multi-pass cladding, the accuracy and stability problems of the method for determining the overlap rate of laser cladding are solved, and high-precision multi-pass cladding is achieved. The calculation of the optimal overlap rate improves the flatness and forming accuracy of the cladding layer, and reduces the number of tests and costs.

CN118734584AActive Publication Date: 2024-10-01TAIYUAN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410894186.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-01
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

The existing method for determining the overlap rate of laser cladding lacks accuracy and stability, which affects the cladding quality and forming accuracy.

Method used

By establishing a relationship model between the profile characteristic parameters of a single-pass cladding section and the critical overlap rate of multi-pass cladding, an elliptical function is used to describe the cross-section of a single-pass cladding layer, and the applicability function of two adjacent cladding layers is established to ensure remelting. The amount of liquid metal in the expansion area and the overlap area is balanced, and the critical overlap rate of multi-pass cladding is calculated.

Benefits of technology

It achieves high-precision calculation of the optimal critical overlap ratio of multi-pass cladding, improves the surface flatness and forming accuracy of the cladding layer, reduces the number of tests and costs, has a wide range of applications, high calculation accuracy, and saves energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118734584A_ABST
    Figure CN118734584A_ABST
Patent Text Reader

Abstract

The invention discloses a method for calculating the multi-channel lap joint rate of laser cladding, and belongs to the technical field of laser cladding processes. In order to solve the problem that an existing method for determining the lap joint rate of laser cladding lacks accuracy and stability, firstly, a single-channel cladding section is determined as an elliptic function, and a cladding section height model, a width model and an elliptic function model which are represented by laser cladding key influence parameters are established; and then a distance model of the centers of any adjacent passes of cladding layers is determined, the above model is substituted into a multi-pass cladding critical overlap rate model, and an optimal critical overlap rate calculated value meeting actual working condition requirements is obtained. Compared with the prior art, the method has the following beneficial effects: (1) the overlap rate model is wide in application range; (2) the ellipse model is high in adaptability; (3) the calculation precision of the overlap rate model is high; (4) the overlap rate model has flexibility and comprehensive controllability; and (5) the product quality is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of laser cladding process, and in particular relates to a method for calculating the overlap rate of multiple passes of laser cladding. Background Art

[0002] As an emerging remanufacturing method, laser cladding has the advantages of fast melting and solidification rate, small thermal deformation of the substrate, controllable coating thickness and stable performance, and a wide range of material selection. However, facing the application requirements of surface modification or repair production of larger parts, the cost of upgrading high-energy and large-size laser beam spots is too high due to the limitations of equipment process parameters, so multi-pass overlapping cladding technology is particularly critical.

[0003] During the laser cladding process, multi-pass overlapping cladding involves issues such as overlap rate, surface flatness and structural defects. Among them, overlap rate is the main factor affecting the cladding quality. The degree of overlap rate being too large or too small will directly determine the macroscopic tilt amplitude and forming accuracy of the surface morphology of the cladding layer. At present, the main methods for determining the overlap rate of laser cladding are: differential line scanning method, color three-dimensional morphology measurement method, image processing-based method, etc. These methods require data processing and analysis, and have relatively high requirements for instruments, equipment and software. At the same time, repeated experiments and verification are required, and they lack accuracy and stability. Summary of the invention

[0004] In view of the problem that the existing laser cladding overlap rate determination method lacks accuracy and stability, the present invention provides a method for calculating the overlap rate of multiple passes of laser cladding. That is, by establishing a relationship model between the characteristic parameters of the single-pass cladding cross-section profile and the critical overlap rate of multiple passes cladding, a high-precision laser cladding optimal critical overlap rate calculation value that meets the requirements of actual working conditions is obtained.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for calculating the overlap rate of multiple passes of laser cladding, the method comprising the following steps:

[0007] S1: In order to simplify the theoretical calculation and analysis process, two cladding layers are randomly selected to complete the construction of the multi-layer overlap model, and the following assumptions are made:

[0008] (1) The cross-sectional profile of a single-pass cladding layer is completely and accurately a part of the elliptical function;

[0009] (2) During the multi-pass cladding process with the same process parameters, the cross-sectional shape, size and area of ​​the single-pass cladding layer remain unchanged;

[0010] (3) The molten pool has good fluidity, and the subsequent cladding layer is easy to spread and fill the remelting expansion area;

[0011] (4) Ignore the influence of the surface tension of the liquid metal cladding layer and the impact pressure of the shielding gas on the forming process;

[0012] S2: The cross-sectional profile of the single-pass cladding layer in step 1 is completely and accurately a part of the elliptical function, such as Figure 1 As shown in the figure, a Cartesian rectangular coordinate system is established with the boundary line between the cladding layer and the substrate in the horizontal direction as the X-axis and the symmetry axis of the cladding layer in the vertical direction as the Y-axis. Point O is the origin of the coordinate system, point O′ is the center of the first cladding layer ellipse, the width of the cladding layer is W, and the height of the cladding layer is H.

[0013] The elliptic function expression is:

[0014]

[0015] The calculation formula for the width W of a single cladding layer is:

[0016]

[0017] The calculation formula for the height H of a single cladding layer is:

[0018] H=bc

[0019] Among them, a, b, and c are the geometric structure parameters of the elliptical function, which are all functions of the process parameters of the single-channel cladding layer. y represents the ordinate of any point on the cross-sectional profile of the single-channel cladding layer, and x represents the abscissa of any point on the cross-sectional profile of the single-channel cladding layer. The diagnostic diagrams of a, b, and c are shown in Figure 2 shown.

[0020] S3: Select a suitable function as the applicability function of the cross-sectional profiles of two adjacent cladding layers;

[0021] Furthermore, the applicability functions of the cross-sectional profiles of two adjacent cladding layers in step S2 are respectively:

[0022]

[0023] Among them, y1 represents the ordinate of any point on the cross-sectional profile of the first cladding layer, y2 represents the ordinate of any point on the cross-sectional profile of the next cladding layer, and d is the distance between the centers of any adjacent cladding layers, such as Figure 3 As shown, point O′ is the center of the first cladding layer ellipse, and point O″ is the center of the next cladding layer ellipse.

[0024] S4: In order to ensure that a completely flat surface is formed between two adjacent cladding layers, the amount of liquid metal that needs to be filled in the remelted expansion area BEG should be equal to the amount of liquid metal that overlaps the overlap area CDG; and the ideal multi-layer overlap flatness requirement should be met, that is, points B, M, and E are on the same horizontal line; Figure 3 As shown;

[0025] The area of ​​each region of the cladding layer satisfies the following relationship: S BMG =S EMG =S DNG =S CNG ;

[0026] S5: Write the area relationship between the remelting expansion area BEG and the overlapping area CDG according to the area relationship of each area of ​​the cladding layer;

[0027] Furthermore, the area between the remelted expansion region BEG and the overlap region CDG in step S4 is expressed as:

[0028]

[0029] S6: Subtract the area of ​​the BEG and CDG regions and define the difference as g(d). When the ideal overlap state is met, S BEG =S CDG , solve for the value of d;

[0030] Furthermore, in step S5, the area difference between the remelted expansion region BEG and the overlap region CDG is defined as g(d):

[0031]

[0032] When the ideal overlap state is met, S BEG =S CDG , that is, g(d)=0, and the solution is:

[0033]

[0034] S7: Substitute the value of d into the critical overlap rate calculation formula to obtain the critical overlap rate of multiple cladding passes;

[0035] Furthermore, in step S6, the value of d is substituted into the critical overlap rate calculation formula: In the above, the critical overlap ratio of multiple cladding passes is:

[0036]

[0037] S8: Verify the multi-pass cladding quality under the optimal critical overlap rate and compare and analyze the multi-pass cladding quality under different overlap rates to verify the reliability of the multi-pass overlap model of the controllable process parameters of laser cladding; Figure 4 , as shown in 5.

[0038] Compared with the prior art, the present invention has the following advantages:

[0039] (1) The overlap rate model has a wide range of applications. The calculation method of the overlap rate of laser cladding multi-pass proposed in the present invention can arbitrarily select appropriate process parameters according to actual working conditions, and this model can be used to complete the collaborative optimization of the critical overlap rate of laser multi-pass cladding.

[0040] (2) The elliptical model has strong adaptability. The single-pass cladding cross-sectional profile applicability function - the elliptical model can automatically match the correspondence between the major axis, minor axis and X and Y axes according to the cross-sectional profile, and can adapt to the requirements of large changes in cross-sectional profiles caused by different parameter combinations.

[0041] (3) The overlap rate model has high calculation accuracy. The multi-pass cladding overlap rate model successfully maps the interaction between process parameters such as laser power, scanning speed, powder feeding rate and critical overlap rate, and has high calculation accuracy.

[0042] (4) The overlap rate model is flexible and comprehensively controllable. The calculation process is simple and has high versatility, which greatly improves the efficiency of selecting the critical overlap rate of multi-pass cladding. It does not require a large amount of test data, saves pre-test time and cost, consumes less energy, and has low production cost.

[0043] (5) Good product quality. The surface flatness of the multi-layer overlapped cladding layer is high, the uneven boundary and powder residue are effectively alleviated, and the composite interface is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is a schematic diagram of the cross-section profile feature model;

[0045] Figure 2 Diagnostic diagrams of geometric structure parameters a, b, c of the ellipse model. Figures (a), (c), and (e) are the residual distribution diagrams of geometric structure parameters a, b, and c respectively; Figures (b), (d), and (f) are the relationship diagrams between the experimental values ​​and predicted values ​​of geometric structure parameters a, b, and c respectively;

[0046] Figure 3 It is a schematic diagram of the multi-channel overlap theoretical calculation model;

[0047] Figure 4 The macroscopic morphology of the cladding layer with different overlap ratios. Among them: Figure (a) overlap ratio 16%; Figure (b) overlap ratio 26%; Figure (c) overlap ratio 36%;

[0048] Figure 5 The three-dimensional microstructures of the cladding layers with different overlap ratios are shown in Figure (a) with an overlap ratio of 16%, Figure (b) with an overlap ratio of 26%, and Figure (c) with an overlap ratio of 36%. DETAILED DESCRIPTION

[0049] In order to better explain the process technology scheme of the present invention, the present invention will be described in full and detail below through specific implementation methods in conjunction with the accompanying drawings in the embodiments of the present invention.

[0050] A method for calculating the overlap rate of multiple passes of laser cladding, wherein the base material is 27SiMn steel and the cladding layer material is GS-Fe01 alloy powder, comprises the following steps:

[0051] S1: In order to simplify the theoretical calculation and analysis process, two cladding layers are randomly selected to complete the construction of the multi-layer overlap model, and the following assumptions are made:

[0052] (1) The cross-sectional profile of a single-pass cladding layer is completely and accurately a part of the elliptical function;

[0053] (2) During the multi-pass cladding process with the same process parameters, the cross-sectional shape, size and area of ​​the single-pass cladding layer remain unchanged;

[0054] (3) The molten pool has good fluidity, and the subsequent cladding layer is easy to spread and fill the remelting expansion area;

[0055] (4) Ignore the influence of the surface tension of the liquid metal cladding layer and the impact pressure of the shielding gas on the forming process.

[0056] S2: The cross-sectional profile of a single-pass cladding layer is completely accurate as a part of the elliptical function, such as Figure 1 As shown, the elliptic function expression is: The calculation formula for the width W of a single cladding layer is: The calculation formula for the height H of a single cladding layer is: H=bc.

[0057] Among them: a, b, c are the geometric structure parameters of the applicability function, which are all functions of the process parameters of the single-pass cladding layer.

[0058] The following describes the calculation method of the geometric structure parameters a, b, and c of the suitability function:

[0059] (1) Based on the laser power (p), scanning speed (v), powder feeding rate (v f ) are the key input variables, and 16 groups of single-pass cladding orthogonal test schemes are constructed, see Table 1.

[0060] Table 1 16 groups of single-pass cladding orthogonal tests

[0061]

[0062] (2) An exponential regression model was selected and combined with polynomial and trigonometric function models to perform multivariate nonlinear fitting on 16 sets of data. The standard hedron hill climbing method and the general global optimization method were introduced to determine the optimal parameters of the model. MATLAB software was used to optimize the multiple parameters of the model in one go, and the objective function of the geometric structure parameters-process parameters of the suitability function was obtained.

[0063] a=0.39261(p 0.27230 v 0.00369 v f -0.40507 )+2.31260sin(v f +0.12452)-3.35727

[0064] b=6.12358×10 3 (p -0.72213 v -0.61507 v f 0.18576 )-0.4665lcos(p+1.99589)-0.95726

[0065] c=-9.26016×10 -5 (p -0.15465 v 2.34145 v f 0.02714 )-0.24563cos(v+0.11984)-0.28974cos(2p-963.25493)-7.69138×10 -7 v 3 +3.82432×10 -4 pv f 2 -6.91820×10 -8 p 2 +1.73812

[0066] Where p, v, and vf are the laser cladding process parameters laser power, scanning speed, and powder feeding rate, respectively; a, b, and c are the geometric structure parameters of the elliptic function, respectively.

[0067] (3) The fitting accuracy of the above model for the 16 sets of data can be tested through the diagnostic plots of the geometric structure parameters a, b, and c, where the diagnostic plots mainly include the residual distribution plot and the relationship plot between the test value and the predicted value.

[0068] like Figure 2 As shown in the figure, all the residual data points randomly fall in the horizontal band area within the range of (-0.1, 0.1), which does not contain any systematic distribution trend and predictability information, and fully meets the normality property, indicating that the model fits the data well. In addition, the coefficient of determination R2 They are all much larger than 0.9, which proves that the errors between the test values ​​and the predicted values ​​are small and have good correlation.

[0069] S3: The applicability functions of the cross-sectional profiles of two adjacent cladding layers are:

[0070]

[0071] Where: d is the distance between the centers of any adjacent cladding layers, such as Figure 3 shown.

[0072] S4: In order to ensure a completely flat surface between two adjacent cladding layers, the amount of liquid metal that needs to be filled in the remelting expansion area BEG should be equal to the amount of liquid metal that overlaps the overlapping area CDG, and the area of ​​each area of ​​the cladding layer should satisfy the following relationship: S BMG =S EMG =S DNG =S CNG And it meets the ideal multi-pass overlap flatness requirement, that is, points B, M, and E are on the same horizontal line. Figure 3 shown.

[0073] S5: The area of ​​BEG and CDG regions can be expressed as:

[0074]

[0075] S6: Define the area difference between the BEG and CDG regions as g(d):

[0076]

[0077] When the ideal overlap state is met, S BEG =S CDG , that is, g(d)=0, and the solution is:

[0078]

[0079] S7: Substitute the above formula into the critical overlap ratio calculation formula In the above, the critical overlap ratio of multiple cladding passes is:

[0080]

[0081] In summary, the multi-pass overlap model of laser cladding controllable process parameters is:

[0082] H=bc

[0083]

[0084] a=0.39261(p 0.27230 v 0.00369 vf -0.40507 )+2.31260sin(v f +0.12452)-3.35727

[0085] b=6.12358×10 3 (p -0.72213 v -0.61507 v f 0.18576 )-0.46651cos(p+1.99589)-0.95726

[0086] C = -9.26016 × 10 -5 (p- 0.15465 v 2.34145 v f 0.02714 )-0.24563cos(v+0.11984)-0.28974cos(2p-963.25493)-7.69138×10 -7 v 3 +3.82432×10 -4 pv f 2 -6.91820×10 -8 p 2 +1.73812

[0087]

[0088]

[0089] Based on a combination of laser single-pass cladding process parameters, namely, laser power of 744W, scanning speed of 233mm / min, powder feeding rate of 1.2r / min, and spot diameter of 2.5mm, a multivariate nonlinear mathematical model constructed with elliptic function coefficients a, b, and c as target response indicators is used to effectively predict the geometric structure parameters of the single-pass cladding cross-sectional profile applicability function. On this basis, the precise information of the cross-sectional profile width (W) and height (H) is further obtained, and the above parameters are substituted into the multi-pass overlap model of laser cladding controllable process parameters, and the optimal critical overlap rate of single-pass cladding suitable for this working condition is solved to be 26%.

[0090] S8: Multi-pass cladding quality verification under optimal critical overlap rate:

[0091] Comparison of the multi-pass cladding quality in three cases with overlap rates of 16%, 26%, and 36%. Figure 4 , Figure 5As shown in the figure. When the overlap rate is 16%, since the overlap area is much smaller than the remelting expansion area, large grooves are generated between each pass of the cladding layer and a flat surface cannot be formed. The average height difference between the bottom of the concave area and the top of the cladding layer is about 270μm, which does not meet the requirements of multi-pass cladding forming and is in a state of insufficient overlap. At the same time, the surface of the boundary area of ​​each pass of the cladding layer is not smooth, and a large number of unmelted metal powder particles are mixed in.

[0092] When the overlap rate increases to 26%, which is the critical overlap rate calculated by the multi-pass overlap model, the metal material in the overlap area of ​​the cladding layer basically fills the concave part of the remelting expansion area completely, the overall forming height of the cladding layer remains basically the same, there are no obvious grooves between each pass, the surface is smooth and flat and meets the requirements of multi-pass cladding forming, and only a small amount of powder residue exists between each pass.

[0093] When the overlap rate is increased to 36%, the area and climbing amplitude of the boundary climbing zone increase significantly, the maximum height difference reaches more than 3000μm, the grooves between each pass have completely disappeared, and a large number of black burnt areas appear on the surface of the cladding layer.

[0094] In summary, when the overlap rate is 26%, multi-pass cladding forming can obtain a cladding layer flatness that is relatively close to the expected result, which proves the reliability of the multi-pass overlap model with controllable process parameters of laser cladding.

[0095] The contents not described in detail in the specification of the present invention belong to the prior art known to the professional and technical personnel in the field. Although the illustrative specific embodiments of the present invention are described above to facilitate the understanding of the present invention by the technical personnel in the field, it should be clear that the present invention is not limited to the scope of the specific embodiments. For the ordinary technical personnel in the field, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.

Claims

1. A method for calculating the overlap rate of multiple passes of laser cladding, characterized in that: The method comprises the following steps: S1: Randomly select two cladding layers to complete the construction of the multi-layer overlap model, and make the following assumptions: (1) The cross-sectional profile of a single-pass cladding layer is completely and accurately a part of the elliptical function; (2) During the multi-pass cladding process with the same process parameters, the cross-sectional shape, size and area of ​​the single-pass cladding layer remain unchanged; (3) The molten pool has good fluidity, and the subsequent cladding layer is easy to spread and fill the remelting expansion area; (4) Ignore the influence of the surface tension of the liquid metal cladding layer and the impact pressure of the shielding gas on the forming process; S2: The cross-sectional profile of a single cladding layer is completely and accurately determined as a part of an elliptical function, and a Cartesian rectangular coordinate system is established with the horizontal boundary line between the cladding layer and the substrate as the X-axis and the vertical symmetry axis of the cladding layer as the Y-axis; S3: Select a suitable function as the applicability function of the cross-sectional profiles of two adjacent cladding layers; S4: Make the amount of liquid metal that needs to be filled in the remelting expansion area BEG equal to the amount of liquid metal that overlaps the overlap area CDG; and meet the requirements of flatness of multi-pass overlap in an ideal state; S5: Write the area relationship between the remelting expansion area BEG and the overlapping area CDG according to the area relationship of each area of ​​the cladding layer; S6: Subtract the area of ​​the BEG and CDG regions and define the difference as g(d). When the ideal overlap state is met, S BEG =S CDG , solve for the value of d; S7: Substitute the value of d into the critical overlap rate calculation formula to obtain the critical overlap rate of multiple cladding passes; S8: Verify the quality of multi-pass cladding at the optimal critical overlap rate.

2. The method for calculating the overlap ratio of multiple passes of laser cladding according to claim 1, characterized in that: In step S2, the cross-sectional profile of the single-channel cladding layer is completely and accurately a part of the elliptical function. The boundary line between the cladding layer and the substrate in the horizontal direction is the X-axis, and the axis of symmetry of the cladding layer in the vertical direction is the Y-axis. A Cartesian rectangular coordinate system is established, with point O as the origin of the coordinates, point O′ as the center of the first cladding layer ellipse, the cladding layer width is W, and the cladding layer height is H; then: The elliptic function expression is: The calculation formula for the width W of a single cladding layer is: The calculation formula for the height H of a single cladding layer is: H=bc Among them, a, b, and c are the geometric structure parameters of the elliptical function, which are all functions of the process parameters of the single-channel cladding layer. y represents the ordinate of any point on the cross-sectional profile of the single-channel cladding layer, and x represents the abscissa of any point on the cross-sectional profile of the single-channel cladding layer.

3. The method for calculating the overlap ratio of multiple passes of laser cladding according to claim 1, characterized in that: The applicability functions of the cross-sectional profiles of two adjacent cladding layers in step S3 are: Among them, y1 represents the ordinate of any point on the cross-sectional profile of the first cladding layer, y2 represents the ordinate of any point on the cross-sectional profile of the next cladding layer, and d is the distance between the centers of any adjacent cladding layers.

4. The method for calculating the overlap ratio of multiple passes of laser cladding according to claim 1, characterized in that: In step S4, the amount of liquid metal to be filled in the remelting expansion area BEG is kept equal to the amount of liquid metal overlapped in the overlap area CDG; and the requirements for flatness of multi-pass overlap in the ideal state are met, that is, points B, M, and E are on the same horizontal line; the area of ​​each area of ​​the cladding layer satisfies the following relationship: S BMG =S EMG =S DNG =S CNG .

5. The method for calculating the overlap ratio of multiple passes of laser cladding according to claim 1, characterized in that: The area between the remelting expansion area BEG and the overlapping area CDG in step S5 is expressed as:

6. The method for calculating the overlap ratio of multiple passes of laser cladding according to claim 1, characterized in that: In step S6, the area difference between the remelted expansion area BEG and the overlap area CDG is defined as g(d): When the ideal overlap state is met, S BEG =S CDG , that is, g(d)=0, and the solution is:

7. The method for calculating the overlap ratio of multiple passes of laser cladding according to claim 1, characterized in that: In step S7, the value of d is substituted into the critical overlap rate calculation formula. In the above, the critical overlap ratio of multiple cladding passes is:

8. The method for calculating the overlap ratio of multiple passes of laser cladding according to claim 1, characterized in that: The specific operation of step S8 is: to compare and analyze the multi-pass cladding quality under different overlap rates, and verify the reliability of the multi-pass overlap model of the laser cladding controllable process parameters.

Citation Information

Patent Citations

  • Calculation method for critical overlapping rate in laser cladding forming process for vertical surface

    CN107354453A

  • Method for optimizing technological parameters of laser cladding on circular arc surface

    CN108559994A

  • Method for optimizing parameters of laser cladding process on plane

    CN108559995A