High-power microwave protection and heating integrated conductive transparent material for display and preparation method thereof
Through the electron beam evaporation process and multi-layer coating design, the problem of conductive transparent materials that are difficult to achieve multiple functions in the existing technology is solved, and high light transmittance, low reflectivity and good electromagnetic compatibility are achieved to meet the needs of high-end applications.
Patent Information
- Application Number
- CN202410761832.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to achieve high transmittance, low reflectivity, good electromagnetic compatibility, normal use in low-temperature environments, high surface hardness and low color difference at the same time with the existing technology. Conductive transparent materials integrating high-power microwave protection and heating for display , and the arrangement and combination of multi-layer coatings have not been studied in depth.
Through the electron beam evaporation process, coatings of different chemical compositions and thicknesses are sequentially superimposed on one or both sides of the base layer. The composite coating structure is designed to be T1R1Y1R2T2R3Y2R4T3R5T4F. It is combined with indium tin oxide, lanthanum titanate, magnesium fluoride and other materials to optimize the coating thickness and sequence to achieve multiple functions.
It achieves excellent electromagnetic shielding performance, sunlight readability, normal use in low-temperature environments and good electromagnetic compatibility, meeting the high-end needs of military, medical, aerospace and other applications. It has excellent anti-glare properties, high transmittance and low reflectivity. .
Smart Images

Figure CN118737530A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of optical and electrical materials, and in particular to a conductive transparent material integrated with high-power microwave protection and heating for display and a preparation method thereof. Background Art
[0002] With the continuous development of science and technology, the application prospects of materials with both optical and electrical properties are becoming increasingly broad, and at the same time, higher requirements are placed on the performance of materials.
[0003] In the military, medical, aerospace and other high-end technology fields, the requirements for display screens are getting higher and higher. The light-transmitting materials used in high-end display screens need to have the following properties at the same time: 1. High light transmittance; 2. Low reflectivity (readable in sunlight or strong light environment); 3. Good electromagnetic compatibility (EYC); 4. Normal use in low temperature environment (good conductivity); 5. High surface hardness; 6. Low color difference, for visible light (380 nanometers-780 nanometers) total transmission color difference: AX, AY <0.002, color neutral. This puts high demands on the preparation of conductive transparent materials for integrated high-power microwave protection and heating for display, and also greatly increases the difficulty of the preparation process of conductive transparent materials for integrated high-power microwave protection and heating for display.
[0004] In the photovoltaic field, high-end photovoltaic glass not only has high requirements for light transmittance, but also requires good electromagnetic compatibility, surface hardness, self-cleaning ability, etc. Currently, there is no relevant material that can meet the above requirements.
[0005] In order to meet the composite performance requirements of light-transmitting conductive materials, existing technical solutions include gluing multiple pieces of glass with different properties to achieve this: for example, Chinese invention patent CN201610847264.X, light-transmitting materials with different properties are glued together to obtain a composite material that has electromagnetic shielding, sunlight readability and resistance to severe cold; another technical route of the prior art is to use surface coating technology to achieve the composite performance of light-transmitting materials: for example, Chinese invention patent CN201810056467.6, uses coating technology to produce eight film layers on a substrate to achieve the composite performance of anti-glare, reduced surface reflection and increased light transmittance.
[0006] In the prior art, the mainstream technologies for vacuum coating the surface of substrates include evaporation coating, sputtering coating and ion film coating. Electron beam evaporation is a type of vacuum evaporation coating, which is a method of using electron beams to directly heat and evaporate dielectric materials under vacuum conditions, so that the dielectric materials evaporate and gasify and are transported to the substrate, and condense on the surface of the substrate to form a coating. In the electron beam heating device, the heated dielectric material is placed in a crucible with a cooling device to prevent the dielectric material from reacting with the crucible wall after evaporation and affecting the quality of the coating. Therefore, the electron beam evaporation deposition method can prepare high-purity thin film coatings. At the same time, multiple crucibles can be placed in the same evaporation deposition device to achieve simultaneous or separate evaporation and deposition of multiple different dielectric materials. Electron beam evaporation can evaporate and form coatings for dielectric materials of various physical properties.
[0007] In the prior art, the technologies that can achieve transparent material shielding include: nano silver wire printing technology, metal wire mesh interlayer technology, carbon nanotube and ITO coating technology.
[0008] Nano silver wire printing technology (i.e. shielding film) is achieved by coating a glue layer on the PV material (referring to polyvinyl polymer compounds represented by polyvinyl alcohol), and then embossing regular or irregular nano silver wires with extremely fine gaps on the glue layer. The silver wires play a shielding role; micron-level gaps are left between the silver wires, and the transmittance of the substrate material itself in the gap is an indicator of the transmittance of the entire shielding film. It is precisely because of the existence of light-transmitting gaps that the electromagnetic shielding surface is not continuous, so under the same resistance value, the shielding performance of nano silver wire printing technology is worse than that of ITO coating. In addition, because PV material is a soft film and the thermal expansion and contraction coefficients of glass materials are very different, the environmental adaptability is poor, and the silver wires are highly oxidizable, which will affect the reliability of the product in a high humidity and temperature environment for a long time.
[0009] The metal mesh and glass are glued together with hot melt adhesive, and the metal mesh is sandwiched between two layers of glass to achieve shielding effect. The gap in the middle of the mesh determines the transmittance index. The larger the gap, the better the transmittance but the worse the shielding effect, and vice versa. When the metal mesh sandwich technology is used in display products, moiré fringes will appear, which directly affects the human-computer interaction effect. Therefore, the metal mesh sandwich process is not suitable for high-end display products such as military, medical, and aerospace.
[0010] ITO coating is an indium tin oxide semiconductor film. Indium tin oxide semiconductor films usually have two key performance indicators: resistivity and transmittance. There is a correlation between the surface resistance (R), film thickness (d) and resistivity (ρ) of ITO coating. By adjusting different film thicknesses and resistivities, ITO films with different surface resistances (R) can be obtained. However, it is difficult for existing technologies to take into account both shielding properties and transmittance: the thicker the ITO film layer, the smaller the surface resistance of the ITO film, and the smaller the light transmittance.
[0011] As mentioned above, existing technologies are mostly used to solve single problems in application scenarios: such as shielding problems, transmittance problems or anti-glare problems, but it is impossible to solve multiple problems in use applications at the same time by integrating a multi-layer structure of several nano-transparent materials on a piece of glass.
[0012] In view of the above, there is no in-depth research on the use of multiple different chemical compositions and multi-layer coatings to improve the comprehensive performance of conductive transparent materials, and there is no research result on how to arrange and combine the multi-layer coatings to achieve the best synergistic effect. In view of this, the structural design and preparation process of multi-layer composite transparent optical and electrical materials is still a technical field to be studied. Summary of the invention
[0013] In view of the deficiencies in the above-mentioned prior art, the present invention provides a conductive transparent material with integrated high-power microwave protection and heating for display and a preparation method thereof. Through the electron beam evaporation process, coatings with different chemical compositions and thicknesses are sequentially superimposed on one side or both sides of the substrate layer to achieve excellent electromagnetic shielding performance, readability in sunlight, normal use in low temperature environments (-55℃~-60℃) and good electromagnetic compatibility, etc., to meet high-end requirements such as military, medical, and aerospace. The patent of this invention utilizes the special design of composite materials and multi-layer nano-transparent materials to achieve multiple functions, while solving the problems of electromagnetic shielding, sunlight readability and cold resistance, and at the same time has excellent anti-glare properties.
[0014] The present invention provides a conductive transparent material for high-power microwave protection and heating for display, comprising a transparent substrate layer and a composite coating attached to at least one side of the substrate layer, wherein the composite coating is composed of coatings of different dielectric materials, and the arrangement order of each coating in the composite coating is T1R1Y1R2T2R3Y2R4T3R5T4F, wherein T1, T2, T3 and T4 all represent lanthanum titanate material layers, R1, R2, R3, R4 and R5 all represent silicon dioxide material layers, Y1 and Y2 all represent indium tin oxide material layers, F represents magnesium fluoride material layers, T1 is close to the substrate layer, and F is far away from the substrate layer. Each coating in the composite coating is a single layer or multiple layers. Preferably, the indium tin oxide material layer is a multilayer.
[0015] Preferably, composite coatings are attached to two opposite sides of the base layer, and the composite coatings are symmetrically distributed with respect to the central axis of the base layer.
[0016] The base layer may be made of transparent materials such as optical glass or organic optical transparent plastic, and the present invention is not limited thereto.
[0017] The optical glass may be K9, BK7, BF33 or D263T, or the organic optically transparent plastic may be PET, PMMA, PC or TPU, etc., but the present invention is not limited thereto.
[0018] Preferably, the indium tin oxide material layer comprises 80 to 95 parts by weight of indium oxide and 5 to 20 parts by weight of tin oxide.
[0019] Preferably, the purity of the lanthanum titanate, silicon dioxide, indium oxide, tin oxide and magnesium fluoride is required to be 99% or above.
[0020] Preferably, the thickness of each layer of the composite coating is respectively as follows according to the arrangement order:
[0021] F 108.52~119.94nm, T4 131.43~145.27nm, R5 52.99~58.57nm,
[0022] T3 25.02~27.66nm, R4 47.09~52.05nm, Y2 578.55~639.45nm,
[0023] R3 47.27~52.25nm, T2 24.87~27.49nm, R2 45.66~50.46nm,
[0024] Y1 578.55~639.45nm, R1 38.11~42.13nm, T1 12.62~13.94nm.
[0025] More preferably, the thickness of each layer of the composite coating according to the arrangement order is:
[0026] F 114.23nm, T4 138.35nm, R5 55.78nm,
[0027] T3 26.34nm, R4 49.57nm, Y2 609nm,
[0028] R3 49.76nm, T2 26.18nm, R2 48.06nm,
[0029] Y1 609nm, R1 40.12nm, T1 13.28nm.
[0030] The present invention also provides a method for preparing the above-mentioned conductive transparent material with integrated high-power microwave protection and heating for display, comprising the following steps:
[0031] Step S1: clean the base layer with an ultrasonic cleaner, dry it, and then put it into the workpiece tray of the vacuum coating machine;
[0032] Step S2: gradually raise the temperature of the substrate layer from room temperature to 400°C, maintain the temperature at 350-400°C for 30-60 minutes, and the initial vacuum degree is 4.0×10 -4 ~8.0×10 -4 Pa;
[0033] Step S3: bombarding the surface of the substrate layer with an RF ion source for 5 to 10 minutes, with a gas flow rate of 40 to 80 sccm (standard milliliters per minute);
[0034] Step S4: using an electron beam evaporation process, evaporating various dielectric materials on the base layer in sequence according to the arrangement order of the coating layers in the composite coating, completing the evaporation of each coating layer in the composite coating, monitoring and controlling the thickness of each coating layer in real time through the coating machine, setting the thickness of each layer by the coating machine control system, and when the evaporation of the dielectric material of the previous coating layer is completed, the equipment automatically starts the coating of the next layer;
[0035] Step S5: After the evaporation is completed, the material is taken out after the temperature drops to room temperature, thereby obtaining a conductive transparent material with integrated high-power microwave protection and heating for display that has been coated.
[0036] The model of the coating machine used may be OTFC-1300DBI or OTFC-1800DBI. The numerals 1300 or 1800 in the coating machine model represent the size, and the present invention is not limited thereto.
[0037] The indium tin oxide material layer is evaporated once or multiple times by electron beam evaporation.
[0038] Preferably, when preparing a material containing composite coatings on both sides, the step S4 further comprises: after completing the evaporation of the composite coating on one side, flipping the base layer 180 degrees, and continuing to sequentially complete the coating layers of the composite coating on the other side of the base layer.
[0039] In the present invention, the materials used are divided into two categories, one is a transparent material that increases transparency: such as a lanthanum titanate material layer, a silicon dioxide material layer, and a magnesium fluoride material layer; the other is a transparent conductive material: such as an indium tin oxide material layer. The present invention needs to consider the optical indicators of the material refractive index, transmittance, reflectivity, and thickness according to each layer of material and perform theoretical formula calculations. The present invention also needs to consider the characteristics of the material itself and the design of the multi-layer material structure sequence and the matching of optical and electrical indicators of the present invention to conduct repeated experiments and tests, thereby optimizing the optical indicator test; the transparent conductive material used in the present invention must also consider the relationship between electromagnetic shielding performance and its material thickness. The thicker the thickness, the better the electromagnetic shielding performance, but the thicker the thickness, the correspondingly weakened the advantages of its transmittance and reflectivity indicators. In this regard, in order to achieve better indicators of the present invention, the multi-layer structure design principle is adopted and Mb / FTTRTRYYRTRYYRT / Jd / TRYYYYYYRTRYYYYYYRTRTTF / Air is proposed.
[0040] In addition, the ITO coating technology described in the present invention is used to achieve shielding, which is to evaporate the conductive transparent nano material ITO on a transparent material (such as glass) through vacuum high-temperature coating. The nano material has a very high density and forms a continuous electromagnetic shielding surface after film formation, which is equivalent to a closed metal plate isolating electromagnetic signals. The method provided by this application can be used to produce conductive transparent materials that protect against high-power microwaves and integrate heating, which can be used in various high-end display devices.
[0041] In summary, the beneficial technical effects achieved by the present invention are as follows: the conductive transparent material and nano transparent material prepared by the method of the present invention are theoretically designed and optimized with process parameters, and then the coatings with different chemical compositions and thicknesses are sequentially grown on one side or both sides of the substrate layer by electron beam evaporation process, achieving multiple functions, including good electromagnetic shielding, good optical properties, heating and other properties; that is, electromagnetic shielding, sunlight readability (anti-glare properties) and cold resistance are solved at the same time; and the high-end requirements of military, medical, aerospace and the like can be met. In particular, the reflection and attenuation of the shielding surface are utilized to prevent the magnetic lines of force or electromagnetic waves generated by the electromagnetic radiation source from entering the shielded area, and the material can be used normally in an environment with strong electromagnetic interference. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 . Schematic diagram of the top view structure of the composite coating of Examples 1-4 and Comparative Example 1. DETAILED DESCRIPTION
[0043] The exemplary embodiments of the present invention are described in detail below. Although these exemplary embodiments are described in sufficient detail to enable those skilled in the art to implement the present invention, it should be understood that other embodiments can be implemented and various changes can be made to the present invention without departing from the spirit and scope of the present invention. The principles and features of the present invention are described below in conjunction with the drawings and specific embodiments. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. The equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in this field according to these embodiments are all within the scope of protection of the present invention. The dielectric materials used in the following embodiments and comparative example 1 include lanthanum titanate, silicon dioxide, indium oxide, tin oxide, and magnesium fluoride, all of which are commercially available, and the purity requirement is 99% or more. In the material structure expression, Jd represents the substrate layer, Air represents the contact surface with the external environment, Mb represents the contact surface between the substrate layer and the lower panel (the lower panel is not limited, and can be a liquid crystal panel), T represents the lanthanum titanate material layer, R represents the silicon dioxide material layer, Y represents the indium tin oxide material layer, and F represents the magnesium fluoride material layer. In actual production, different types of coating machines can be selected according to the size of the transparent material, and the present invention does not limit this. It should also be noted that the external environment may be the atmosphere or vacuum environment, or other materials in contact with the conductive transparent material, and the present invention does not limit this.
[0044] The composite coating in each embodiment and comparative example 1 is composed of T, R, Y, and F layers stacked in a certain order, such as Figure 1 As shown, when superimposed, the topmost layer is a magnesium fluoride coating, the bottommost layer is a lanthanum titanate coating, and the indium tin oxide coating has an outer ring area around the overlapping area in addition to the overlapping area with other coatings, and the outer ring area is used to lead out the electrode. The electrode can be selected as needed, and specifically, a conductive copper foil or a conductive silver paste can be selected. Specifically, copper foil conductive strips or conductive silver paste are respectively bonded to the edges of the Y layer (indium tin oxide material layer) of the composite coating to lead out the edge electrodes around the edges. The conductive copper foil is bonded to the Y layer film, or the conductive silver paste is printed or the conductive material is used to lead out the electrodes without gaps around the edges, and then pressed into shape by lamination. This method is simple and easy to operate, has high bonding strength, is not easy to partially fall off, and has good conductivity.
[0045] Example 1
[0046] This embodiment provides a conductive transparent material, which is composed of a base layer of optical glass K9 (Note: the base layer can be optical glass K9, BK7, BF33 or D263T, or transparent materials such as organic optical plastics PET, PMMA, PC or TPU, which is not limited by the present invention) and a composite coating on the A surface. The material structure expression of this embodiment is: Mb / Jd / TRYYYYYYRTRYYYYYYRTRTTF / Air. The mass fractions of the chemical components of the indium tin oxide material layer are: 80 parts of indium oxide and 20 parts of tin oxide.
[0047] In the material expression, TRYYYYYYRTRYYYYYYYRTRTTF on the right side of Jd is the composite coating on surface A. The specific process steps are as follows.
[0048] Step S1: clean the base layer with an ultrasonic cleaner, dry it, and then put it into the workpiece tray of the vacuum coating machine.
[0049] Step S2: gradually raise the temperature of the substrate layer from room temperature to 400°C, and maintain the temperature between 350°C and 400°C for 60 minutes. Initial vacuum degree: 4.0×10 -4 Pa~8.0×10 -4 Pa.
[0050] Step S3: Use RF ion source to bombard the surface of the substrate layer for 10 minutes (note: the time is different from the above) with a gas flow rate of 80 sccm.
[0051] Step S4: Using electron beam evaporation process, evaporate various dielectric materials in turn to complete the evaporation of each layer of composite coating on surface A. The coating machine monitors and controls the thickness of each coating layer in real time, and the thickness of each coating layer is shown in Table 1. The coating machine control system sets the thickness of each layer. When the evaporation of the dielectric material of the previous coating layer is completed, the equipment automatically starts the coating of the next layer.
[0052] Step S5: After the evaporation is completed, the temperature of the vacuum chamber is lowered to a predetermined temperature, and the coated conductive transparent material with integrated high-power microwave protection and heating for display is taken out. The conductive transparent material with a material structure expressed as: Mb / Jd / TRYYYYYYRTRYYYYYYRTRTTF / Air is obtained.
[0053] Step S6: Print conductive silver paste on the four edges of the Y layer (indium tin oxide material layer) of the composite coating on the A surface to lead out the four edge electrodes.
[0054] Comparative Example 1
[0055] The same process as in Example 1 is used, and the thickness of each coating layer and the total thickness after coating are the same; the difference is that the order of coating each layer is different. The order of each coating layer and the preset thickness are shown in Table 1.
[0056] Table 1 Thickness of each coating layer in Example 1 and Comparative Example 1
[0057]
[0058] Example 2
[0059] The same process as in Example 1 is used, but the thickness of each layer of coating and the total thickness after coating are increased by 5% compared with Example 1. The mass fractions of the chemical components of the indium tin oxide material layer are: 95 parts of indium oxide and 5 parts of tin oxide. In step S2, the temperature of 350-400°C is maintained for 45 minutes. In step S3, the surface of the substrate layer is bombarded with an RF ion source for 8 minutes with a gas flow rate of 60 sccm. In step S6, conductive silver paste is printed on the edges of the Y layer (indium tin oxide material layer) of the composite coating on the A side to lead out the electrodes on the edges. The order and thickness of each coating layer are shown in Table 2.
[0060] Example 3
[0061] The same process as in Example 1 is used, but the thickness of each layer of coating and the total thickness after coating are reduced by 5% compared with Example 1. The mass fractions of the chemical components of the indium tin oxide material layer are: 90 parts of indium oxide and 10 parts of tin oxide. In step S2, the temperature of 350-400°C is maintained for 30 minutes. In step S3, the surface of the substrate layer is bombarded with an RF ion source for 5 minutes with a gas flow rate of 40 sccm. In step S6, conductive silver paste is printed on the edges of the Y layer (indium tin oxide material layer) of the composite coating on the A side, and the electrodes on the edges are drawn out. The order and thickness of each coating layer are shown in Table 2.
[0062] Table 2 Thickness of each coating layer in Example 2 and Example 3
[0063]
[0064] Example 4
[0065] The material structure expression provided in this embodiment is Mb / FTTRTRYYYYYYRTRYYYYYYRT / Jd / TRYYYYYYYRTRYYYYYYRTRTTF / Air. Among them, TRYYYYYYRTRYYYY YYRTRTTF on the right side of Jd is the composite coating on the A side; FTTRTRYYYYYYRTRYYYYYYRT on the left side of Jd is the composite coating on the B side. The specific process steps are the same as those in Example 1, but step S4 of this embodiment also includes: after the evaporation of the composite coating on the A side is completed, the base layer is turned 180 degrees, and the coating of each layer of the composite coating on the B side is continued on the other side of the base layer in sequence. After the evaporation is completed, a conductive transparent material with a structural expression of Mb / FTTRTRYYYYYYR TRYYYYYYRT / Jd / TRYYYYYYYRTRYYYYYYRTTF / Air is obtained. Then, the conductive silver paste is printed on the edges of the B-side coating.
[0066] The order and thickness of each coating layer in this embodiment are shown in Table 3.
[0067] Table 3 Thickness of each coating layer of Example 4
[0068]
[0069]
[0070] Comparative test 1: Transmission test at different wavelengths
[0071] The test instrument used in this experiment is: UV-visible spectrophotometer, model V-670, test method: ISO9211-2-2010. The test results of each embodiment and comparative example 1 are shown in Table 4 (the actual test data is 6 decimal places, and the data provided in Table 4 retains 2 decimal places).
[0072] Table 4 Test results of transmission test at different wavelengths
[0073]
[0074]
[0075]
[0076]
[0077]
[0078]
[0079] Comparative test 2: reflection test at different wavelengths
[0080] The test instrument used in this experiment is: UV-visible spectrophotometer, model V-670, test method: ISO9211-2-2010. The test results of each embodiment and comparative example 1 are shown in Table 5.
[0081] Table 5 Test results of reflection test at different wavelengths
[0082]
[0083]
[0084]
[0085]
[0086]
[0087]
[0088]
[0089] Comparative test 3: Electromagnetic shielding performance test
[0090] The test method used in this experiment is the "flange coaxial device method", and the specific requirements are the same as GJB 6190-2008 "Shielding Effectiveness Test Standard". The flange coaxial test device is used with a spectrum analyzer to measure the time domain waveform parameters of square wave pulses of different amplitudes and pulse widths after passing through the coaxial device with or without shielding materials, thereby calculating the frequency domain shielding effectiveness of the material (expressed in dB). Relatively speaking, the lower the resistance value, the better the shielding performance. The relevant comparative test data are shown in Table 6.
[0091] In Table 6, the “380-780nm transmission” data is obtained by taking the average value of the data in Table 4; the “380-780nm reflection” data is obtained by taking the average value of the data in Table 5.
[0092] Table 6 Comparative test data summary
[0093] 380-780nm transmission 380-780nm reflection Shielding performance test results Example 1 85.16 1.3242 1.05Ω Example 2 81.12 1.5956 1.08Ω Example 3 83.83 1.6058 1.22Ω Example 4 80.97 4.2828 0.56Ω Comparative Example 1 81.06 2.2318 1.10Ω
[0094] The data in Table 6 show that Example 4 uses double-sided coating, so the shielding performance is better than that of Example 1, but the transmission performance and reflection performance are reduced. It can be seen that if the transmission performance, reflection performance and shielding performance are to be taken into account, Example 1 is the best solution.
[0095] Comparative test 4
[0096] The transmittance of the coated product obtained in Example 1 was compared with that of several commercially available products according to the method of the aforementioned comparative test 1; the reflectivity was compared according to the method of the aforementioned comparative test 2; and the shielding performance was compared according to the method of the aforementioned comparative test 3. The results are summarized in Table 7.
[0097] Table 7 Summary of comparative test data of commercially available products
[0098] 380-780nm transmission 380-780nm reflection Shielding performance test results Example 1 85.16 1.3242 1.05Ω Example 4 80.97 4.2828 0.56Ω Commercially available sample a 85.01 1.7482 7.2Ω Commercially available sample b 73.54 2.6330 5.6Ω Commercially available samples 88.28 5.6657 7.8Ω Commercially available samples 91.95 1.3746 9.8Ω
[0099] The above-mentioned commercially available sample a is the 15.6-inch shielding glass of Shenzhen Jing Company; the commercially available sample b is the 362.4*215.9*0.7 shielding glass of Taiyuan Xin Company, the commercially available sample c is the 400*500*1.1ITO shielding glass of Changzhou Bai Company, and the commercially available sample d is the 400*500*1.8AR / ITO glass of Wuhu Chang Company.
[0100] Experiments have shown that the product provided by the present invention has high transmittance, low reflectivity and high shielding performance, fills the market gap, and has excellent creativity and practicality.
[0101] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A conductive transparent material integrated with high-power microwave protection and heating for display, characterized in that: The conductive transparent material includes a transparent substrate layer and a composite coating attached to at least one side of the substrate layer, wherein the composite coating is composed of coatings of different dielectric materials, and the arrangement order of the coatings in the composite coating is T1R1Y1R2T2R3Y2R4T3R5T4F, wherein T1, T2, T3 and T4 all represent lanthanum titanate material layers, R1, R2, R3, R4 and R5 all represent silicon dioxide material layers, Y1 and Y2 all represent indium tin oxide material layers, F represents a magnesium fluoride material layer, T1 is close to the substrate layer, and F is far away from the substrate layer.
2. The conductive transparent material according to claim 1, characterized in that: The transparent substrate layer is optical glass or organic optical transparent plastic.
3. The conductive transparent material according to claim 1, characterized in that: Each coating layer in the composite coating is a single layer or multiple layers.
4. The conductive transparent material according to claim 3, characterized in that: The indium tin oxide material layer is a multi-layer layer.
5. The conductive transparent material according to claim 1, characterized in that: The indium tin oxide material layer comprises 80 to 95 parts by weight of indium oxide and 5 to 20 parts by weight of tin oxide.
6. The conductive transparent material according to any one of claims 1 to 5, characterized in that: The composite coatings are attached to two opposite sides of the base layer, and the composite coatings are symmetrically distributed relative to the central axis of the base layer.
7. The conductive transparent material according to claim 1, characterized in that: The thickness of each layer of the composite coating according to the arrangement order is: F 108.52~119.94nm, T4 131.43~145.27nm, R5 52.99~58.57nm, T3 25.02~27.66nm, R4 47.09~52.05nm, Y2 578.55~639.45nm, R3 47.27~52.25nm, T2 24.87~27.49nm, R2 45.66~50.46nm, Y1 578.55~639.45nm, R1 38.11~42.13nm, T1 12.62~13.94nm.
8. The conductive transparent material according to claim 7, characterized in that: The thickness of each layer of the composite coating according to the arrangement order is: F 114.23nm, T4 138.35nm, R5 55.78nm, T3 26.34nm, R4 49.57nm, Y2 609nm, R3 49.76nm, T2 26.18nm, R2 48.06nm, Y1 609nm, R1 40.12nm, T1 13.28nm.
9. The method for preparing the conductive transparent material for display with integrated high-power microwave protection and heating according to any one of claims 1 to 8, comprising the following steps: Step S1: clean the base layer with an ultrasonic cleaner, dry it, and then put it into the workpiece tray of the vacuum coating machine; Step S2: gradually raise the temperature of the substrate layer from room temperature to 400°C, maintain the temperature at 350-400°C for 30-60 minutes, and the initial vacuum degree is 4.0×10 -4 ~8.0×10 -4 Pa; Step S3: bombarding the surface of the substrate layer with an RF ion source for 5 to 10 minutes with a gas flow rate of 40 to 80 sccm; Step S4: using an electron beam evaporation process, evaporating various dielectric materials on the base layer in sequence according to the arrangement order of the coating layers in the composite coating, completing the evaporation of each coating layer in the composite coating, monitoring and controlling the thickness of each coating layer in real time through the coating machine, setting the thickness of each layer by the coating machine control system, and when the evaporation of the dielectric material of the previous coating layer is completed, the equipment automatically starts the coating of the next layer; Step S5: After the evaporation is completed, the material is taken out after the temperature drops to room temperature, thereby obtaining a conductive transparent material with integrated high-power microwave protection and heating for display that has been coated.