Composite conductor, preparation method and application thereof, plating layer and composite substrate
By utilizing the oxygen evolution reaction technology of graphene oxide, nickel oxide and other materials in composite conductors, a graphene layer with defects at high temperatures is formed, which solves the problem of poor electrical conductivity of existing composite conductors and significantly improves electrical and thermal conductivity. .
Patent Information
- Application Number
- CN202410888142.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
AI Technical Summary
Existing composite conductors have poor electrical conductivity and are difficult to meet modern high requirements for electrical conductivity, thermal conductivity and stability.
By mixing materials such as graphene oxide, nickel oxide and metal oxides, electroplating is performed to form a coating, and an oxygen evolution reaction is performed at high temperatures to generate a defective graphene layer, reducing the number of nucleation sites and improving electrical and thermal conductivity. sex.
The electrical conductivity, thermal conductivity and mechanical strength of the composite conductor are significantly improved, a graphene layer with a larger graphene sheet diameter is formed, and the overall performance of the composite conductor is improved.
Smart Images

Figure CN118737566A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of conductor materials, and in particular to a composite conductor and a preparation method and application thereof, a coating and a composite substrate. Background Art
[0002] Graphene is a two-dimensional crystalline material with many advantages, such as high electrical conductivity, high thermal conductivity, high strength, high flexibility, strong chemical inertness, and excellent gas barrier properties, which makes graphene have great application prospects in many aspects.
[0003] Metal conductors are widely used in the fields of electricity, transportation, industrial equipment, electronic information, etc. due to their good electrical conductivity, thermal conductivity, ductility, etc. However, in recent years, with the increasingly severe energy and environmental problems and the development of high-tech, higher requirements have been placed on the electrical conductivity, thermal conductivity, stability and other properties of metal conductors.
[0004] In the prior art, graphene is usually compounded with a metal conductor, such as mixing copper powder with graphene powder, vapor-depositing a graphene layer on the surface of a copper substrate, etc., in an attempt to obtain a new material that combines the excellent properties of both metal and graphene.
[0005] However, the electrical conductivity of existing composite conductors is relatively poor and needs to be further improved. Summary of the invention
[0006] In view of this, the present application provides a composite conductor, aiming to improve the problem of poor conductivity of existing composite conductors.
[0007] The embodiment of the present application is implemented as follows: a method for preparing a composite conductor comprises the following steps: Mixing graphene oxide, a nickel compound and a solvent to obtain a first mixed solution, adding a base to the first mixed solution to obtain a second mixed solution, and heat-treating the second mixed solution to obtain a graphene oxide-nickel oxide composite; Mixing a metal oxide, a ligand, and a graphene oxide-nickel oxide composite, and heating at a first temperature to obtain a metal oxide-graphene oxide-nickel oxide composite; mixing the metal oxide-graphene oxide-nickel oxide composite with a base plating solution to obtain a plating solution; The plating solution is used to electroplate a metal substrate to obtain a composite substrate, wherein the composite substrate comprises a metal substrate and a plating layer bonded to at least one surface of the metal substrate, wherein the metal substrate comprises a first metal, and the plating layer comprises a second metal and a metal oxide-graphene oxide-nickel oxide composite; The composite substrate is placed in a deposition chamber, and a carbon source is introduced into the deposition chamber at a second temperature to react the metal oxide in the coating to generate a third metal, react the nickel oxide in the coating to generate nickel, and convert the graphene oxide in the coating to the first graphene, thereby obtaining a transition layer including the second metal, the third metal, nickel and the first graphene, and forming a graphene layer including the second graphene on the surface of the transition layer to obtain a composite conductor.
[0008] Correspondingly, an embodiment of the present application also provides a composite conductor, comprising a metal substrate, a transition layer located on at least one surface of the metal substrate, and a graphene layer located on a surface of the transition layer away from the metal substrate, wherein the metal substrate comprises a first metal, the transition layer comprises nickel, a second metal, a third metal and a first graphene, and the graphene layer comprises a second graphene.
[0009] Correspondingly, an embodiment of the present application further provides a coating, wherein the coating includes a second metal and a metal oxide-graphene oxide-nickel oxide composite.
[0010] Correspondingly, an embodiment of the present application further provides a composite substrate, which includes a metal substrate and the coating bonded to at least one surface of the metal substrate.
[0011] Correspondingly, an embodiment of the present application also provides an application of the above-mentioned composite conductor as a wire or cable or an electrical contact.
[0012] The preparation method of the composite conductor described in the present application is to prepare a coating including a second metal and a metal oxide-graphene oxide-nickel oxide composite on the surface of a metal substrate, and then deposit graphene. In this way, the metal oxide, graphene oxide, and nickel oxide in the coating can undergo an oxygen evolution reaction at high temperature, and the metal oxide, graphene oxide, and nickel oxide are reduced and release oxygen (for example, taking copper oxide as an example, the following reaction can occur: CuO→CuO2). In this way, during the vapor deposition process, the surface of the coating can contain some oxygen. The presence of oxygen can not only catalyze and promote the decomposition of the carbon source into free carbon (CH4+O→CH3.; CH3+O CH2.; CH2+O→CH.; CH2+O→C.), but also passivate the second metal in the coating, reduce the activity of the second metal in the oxygen-containing region, and reduce the number of nucleation sites, so that the second graphene in the prepared graphene layer has a larger sheet diameter, and thus the prepared composite conductor has higher electrical conductivity, thermal conductivity, mechanical strength and stability.
[0013] In addition, metal oxides will change from metal oxides to metal suboxides and then to elemental metals (third metals) during the oxygen evolution reaction, which can further effectively reduce the number of nucleation sites.
[0014] In addition, the graphene oxide in the coating is reduced at high temperature to release oxygen and then converted into defective graphene, and the nickel oxide in the coating is reduced at high temperature to release oxygen and then converted into nickel, wherein part of the defective graphene can be absorbed by nickel molten carbon to form carbon nickel, and the structure of the defective graphene that is not absorbed is repaired under the conditions of vapor deposition to form a first graphene with complete structure and grains. The carbon nickel formed by the absorption of nickel molten carbon will not form a eutectic with the second metal, and the defective graphene in the carbon nickel can be released when the temperature is lowered, and form a second graphene with complete structure and grains at the vacancies or defects (positions where oxygen-containing functional groups or oxygen are removed) on the surface of the third metal formed after the reduction of the metal oxide and at the vacancies or defects (positions where oxygen-containing functional groups or oxygen are removed) on the surface of the nickel formed after the reduction of the nickel oxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0016] Figure 1 is a flow chart of a method for preparing a composite conductor provided in an embodiment of the present application; Figure 2 is a schematic structural diagram of a composite conductor provided in an embodiment of the present application; Figure 3 is a schematic structural diagram of another composite conductor provided in an embodiment of the present application; Figure 4 is a schematic structural diagram of a composite matrix provided in an embodiment of the present application; Figure 5 It is a schematic diagram of the structure of another composite matrix provided in an embodiment of the present application.
[0017] Reference numerals: DETAILED DESCRIPTION
[0018] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.
[0019] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.
[0020] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.
[0021] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0022] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0023] Graphene itself is easy to agglomerate and has poor wettability with metals, so the composite application of graphene and metals (such as copper) is more inclined to use vapor deposition. However, because there are more active sites on the metal surface, so far, the existing graphene formed by vapor deposition method is mostly small in grain size and poor in lattice orientation. The conductivity of the metal-graphene composite material formed by depositing the graphene layer on the metal substrate surface cannot achieve the expected effect.
[0024] Taking copper-graphene composite conductors as an example, the existing technology will reduce the number of active sites in the copper matrix by adding copper oxide to the copper matrix and using copper oxide to release oxygen at high temperature, while promoting the cracking of methane into free carbon or carbon atoms. Although this method can successfully prepare large lattice graphene and reduce the graphene grain spacing, after the copper oxide is reduced, the copper layer adjacent to the graphene layer will be reduced to copper because the copper oxide is reduced to copper and oxygen is removed in the copper matrix, leaving vacant sites or voids in the copper matrix. These vacant sites or voids reduce the overall conductivity of the copper-graphene composite conductor.
[0025] The technical solution of this application is as follows: First, please refer to Figures 1 to 5 The present invention provides a method for preparing a composite conductor 100, comprising the following steps: Step S11, mixing graphene oxide, a nickel compound and a solvent to obtain a first mixed solution, adding a base to the first mixed solution to obtain a second mixed solution, and heat-treating the second mixed solution to obtain a graphene oxide-nickel oxide composite; Step S12, mixing the metal oxide, the ligand, and the graphene oxide-nickel oxide composite, and heating at a first temperature to obtain the metal oxide-graphene oxide-nickel oxide composite; Step S13, mixing the metal oxide-graphene oxide-nickel oxide composite with a basic plating solution to obtain a plating solution; Step S14, electroplating the metal substrate 10 with the plating solution to obtain a composite substrate 200, wherein the composite substrate 200 includes the metal substrate 10 and a plating layer 201 bonded to at least one surface of the metal substrate 10, the metal substrate 10 includes a first metal, and the plating layer 201 includes a second metal and a metal oxide-graphene oxide-nickel oxide composite; Step S15, placing the composite substrate 200 in a deposition chamber, introducing a carbon source into the deposition chamber at a second temperature, causing the metal oxide in the coating 201 to react to generate a third metal, causing the nickel oxide in the coating 201 to react to generate nickel, and causing the graphene oxide in the coating 201 to convert into the first graphene, thereby obtaining a transition layer 20 including the second metal, the third metal, nickel and the first graphene, and forming a graphene layer 30 including the second graphene on the surface of the transition layer, thereby obtaining a composite conductor 100.
[0026] The preparation method of the composite conductor described in the present application is to prepare a coating 201 including a second metal and a metal oxide-graphene oxide-nickel oxide composite on the surface of a metal substrate 10, and then deposit graphene. In this way, the metal oxide, graphene oxide, and nickel oxide in the coating 201 can undergo an oxygen evolution reaction at a high temperature, and the metal oxide, graphene oxide, and nickel oxide are reduced and release oxygen (for example, taking copper oxide as an example, the following reaction can occur: CuO→CuO2). In this way, during the vapor deposition process, the surface of the coating 201 can contain some oxygen. The presence of oxygen can not only catalyze and promote the decomposition of the carbon source into free carbon (CH4+O→CH3.; CH3+O CH2.; CH2+O→CH.; CH2+O→C.), but also passivate the second metal in the coating 201, reduce the activity of the second metal in the oxygen-containing region, and reduce the number of nucleation sites, so that the second graphene in the prepared graphene layer has a larger sheet diameter, and thus the prepared composite conductor has higher electrical conductivity, thermal conductivity, mechanical strength and stability.
[0027] In addition, metal oxides will change from metal oxides to metal suboxides and then to elemental metals (third metals) during the oxygen evolution reaction, which can further effectively reduce the number of nucleation sites.
[0028] In addition, the graphene oxide in the coating 201 is reduced at high temperature to release oxygen and then converted into defective graphene, and the nickel oxide in the coating 201 is reduced at high temperature to release oxygen and then converted into nickel, wherein part of the defective graphene can be absorbed by nickel molten carbon to form carbon nickel, and the structure of the defective graphene that is not absorbed is repaired under the vapor deposition conditions to form the first graphene with complete structure and grains. The carbon nickel formed by the absorption of nickel molten carbon will not form a eutectic with the second metal, and the defective graphene in the carbon nickel can be released when the temperature is lowered, and the second graphene with complete structure and grains is formed at the vacancies or defects (the position where the oxygen-containing functional group is removed or the oxygen is removed) on the surface of the third metal formed after the reduction of the metal oxide and the vacancies or defects (the position where the oxygen-containing functional group is removed or the oxygen is removed) on the surface of the nickel formed after the reduction of the nickel oxide.
[0029] In addition, the metal oxide in the coating 201 is reduced to become a second metal, and impurities such as water and / or carbon dioxide are generated along with the oxygen evolution reaction and the graphene deposition process. These impurities can be discharged with the gas of the vapor deposition without introducing new impurities into the prepared composite conductor, thereby improving the electrical conductivity, thermal conductivity, mechanical strength, stability and other properties of the composite conductor.
[0030] In the step S11: In some embodiments, in the graphene oxide-nickel oxide composite, nickel oxide is bonded to the surface of the graphene oxide sheet structure.
[0031] It should be noted that in the first mixed solution, the graphene oxide has a two-dimensional sheet structure, and its surface has oxygen-containing functional groups. The nickel ions in the nickel compound can produce a coordination effect with the oxygen-containing functional groups, so that the nickel ions are adsorbed / connected to the surface of the graphene oxide. After adding alkali to the first mixed solution, the alkali can react with the nickel compound to generate nickel hydroxide, and the nickel hydroxide is adsorbed / connected to the surface of the graphene oxide. That is, the second mixed solution includes graphene oxide, nickel hydroxide and solvent, and at least part of the nickel hydroxide is adsorbed / connected to the surface of the graphene oxide. In this way, when the second mixed solution is heat-treated, the nickel hydroxide can be directly converted into nickel oxide in situ on the surface of the graphene oxide, so that the prepared nickel oxide is adsorbed / bound to the surface of the sheet structure of the graphene oxide, thereby forming a graphene oxide-nickel oxide composite.
[0032] In some embodiments, the nickel compound includes but is not limited to one or more of nickel acetate, nickel chloride, and nickel nitrate.
[0033] In some embodiments, the solvent includes but is not limited to water. It is understood that the water can be ordinary water, deionized water, ultrapure water, etc.
[0034] In some embodiments, the base includes but is not limited to aqueous ammonia.
[0035] In some embodiments, the mass ratio of the graphene oxide to the nickel compound is 1:(0.09-0.2), for example, 1:0.09, 1:0.1, 1:0.12, 1:0.13, 1:0.15, 1:0.16, 1:0.18, 1:0.2, etc. Within the ratio range, it is beneficial to prepare a graphene oxide-nickel oxide composite with a suitable nickel oxide content, and it is beneficial to make the prepared composite conductor have higher electrical conductivity, thermal conductivity, mechanical strength, stability and other properties.
[0036] In some embodiments, the base is added in an amount such that the pH value of the second mixed solution is 9-12, for example, 9, 10, 11, 12, etc.
[0037] It can be understood that there is no limit to the amount of the solvent added, as long as the graphene and the nickel compound can be fully dispersed and dissolved.
[0038] In some embodiments, the heat treatment of the second mixed solution comprises: B1, reacting the second mixed solution at a third temperature for a period of time T1, and then washing with water to obtain an insoluble matter; B2. heating the insoluble matter at a fourth temperature for a period of time T2.
[0039] In some embodiments, reacting the mixed solution at the third temperature for a period of time T1 includes: placing the mixed solution in an oil bath having the third temperature to react for a period of time T1.
[0040] In some embodiments, the third temperature is 70~130℃, for example, 70℃, 80℃, 90℃, 100℃, 110℃, 120℃, 130℃, etc., and the time T1 is 7~18 h, for example, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, etc.
[0041] In some embodiments, the fourth temperature is 220~280℃, for example, 220℃, 230℃, 240℃, 250℃, 260℃, 270℃, 280℃, etc., and the time T2 is 8~15 h, for example, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, etc.
[0042] In step S12: In some embodiments, the metal oxide includes, but is not limited to, one or more of copper oxide and aluminum oxide.
[0043] In some embodiments, the complexing agent includes, but is not limited to, one or more of sodium citrate.
[0044] In some embodiments, the mass ratio of the graphene oxide-nickel oxide composite to the ligand is 1:(7-18), for example, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, etc.
[0045] In some embodiments, the mass ratio of the metal oxide to the graphene oxide-nickel oxide composite is 1:(1.2-2.2), for example, 1:1.2, 1:1.3, 1:1.5, 1:1.6, 1:1.8, 1:1.9, 1:2.1, 1:2.1, 1:2.2, etc. Within the above range, it is beneficial to prepare a composite conductor 100 with higher electrical conductivity, thermal conductivity and mechanical strength.
[0046] In some embodiments, the first temperature is 85-95° C., for example, 85° C., 86° C., 88° C., 90° C., 92° C., 93° C., 95° C., etc., and the heating time at the first temperature is 6-7 h, for example, 6 h, 6.2 h, 6.3 h, 6.5 h, 6.6 h, 6.8 h, 7 h, etc. Within the temperature and time range, it is beneficial to promote the reaction, and it is beneficial to make the prepared metal oxide-graphene oxide-nickel oxide composite have better performance, so as to prepare the composite conductor 100 with higher electrical conductivity, thermal conductivity and mechanical strength.
[0047] When heated at the first temperature, the ligand can establish an oxygen bridge between the metal oxide and the oxygen-containing functional groups on the surface of graphene oxide, connect the metal oxide and graphene oxide together, and form a metal oxide-graphene oxide-nickel oxide complex with the graphene oxide-nickel oxide complex under the action of the ligand.
[0048] In some embodiments, in the metal oxide-graphene oxide-nickel oxide composite, the mass ratio of metal oxide, graphene oxide, and nickel oxide is 1:(1-1.9):(0.14-0.26).
[0049] In step S13: In some embodiments, the material of the metal matrix 10 includes a first metal, and the first metal includes one or more of a metal element and an alloy. The metal element includes, but is not limited to, one or more of Cu and Al, and the alloy includes, but is not limited to, one or more of a copper-nickel alloy, a copper-silver alloy, and a copper-zinc alloy.
[0050] See also Figure 2 or Figure 4 In some embodiments, the metal substrate 10 is a metal foil. Figure 3 or Figure 5 In other embodiments, the metal matrix 10 is metal particles. In other embodiments, the metal matrix 10 can also be a metal wire. The cross-sectional view of the metal wire can be referred to Figure 3 or Figure 5 .
[0051] In some embodiments, the base plating solution includes a metal salt, a cyanide, a hydroxide, a complexing agent, and an anode activator.
[0052] In some embodiments, the metal salt includes one or more of a copper salt and an aluminum salt. The copper salt includes but is not limited to cuprous cyanide, and the aluminum salt includes but is not limited to aluminum cyanide.
[0053] In some embodiments, the cyanide includes, but is not limited to, one or more of potassium cyanide and sodium cyanide.
[0054] In some embodiments, the hydroxide includes, but is not limited to, one or more of potassium hydroxide and sodium hydroxide.
[0055] In some embodiments, the complexing agent includes but is not limited to potassium thiocyanate.
[0056] In some embodiments, the anode activator includes, but is not limited to, one or more of potassium sodium tartrate, sodium tartrate, and potassium tartrate.
[0057] In some embodiments, a dispersant is further added to the base plating solution, and the dispersant includes but is not limited to one or more of benzoquinone polymers, sodium benzene sulfonate compounds, and amide compounds. The benzoquinone polymers include but are not limited to benzoquinone polymers. The sodium benzene sulfonate compounds include but are not limited to sodium alkylbenzene sulfonate, and further, the sodium alkylbenzene sulfonate includes but is not limited to one or more of sodium dodecyl sulfonate, sodium methylbenzene sulfonate, and sodium dimethylbenzene sulfonate. The amide compounds include but are not limited to one or more of vinyl bis stearamide, lauric acid diethanolamide, sodium pyrrolidone carboxylate, and polyacrylamide.
[0058] In some embodiments, in the plating solution, the concentration of the metal oxide-graphene oxide-nickel oxide composite is 0.5~2.5 g / L, for example, 0.5 g / L, 0.8 g / L, 0.9 g / L, 1.0 g / L, 1.2 g / L, 1.3 g / L, 1.5 g / L, 1.6 g / L, 1.8 g / L, 2.0 g / L, 2.1 g / L, 2.2 g / L, 2.5 g / L, etc.
[0059] In some embodiments, the concentration of the metal salt in the plating solution is 50~65 g / L, for example, 50 g / L, 51 g / L, 52 g / L, 53 g / L, 55 g / L, 56 g / L, 58 g / L, 60 g / L, 61 g / L, 62 g / L, 63 g / L, 64 g / L, 65 g / L, etc.
[0060] In some embodiments, the concentration of cyanide in the plating solution is 100-135 g / L, for example, 100 g / L, 112 g / L, 115 g / L, 116 g / L, 118 g / L, 120 g / L, 121 g / L, 123 g / L, 125 g / L, 126 g / L, 128 g / L, 130 g / L, 132 g / L, 133 g / L, 135 g / L, etc.
[0061] In some embodiments, in the plating solution, the concentration of the hydroxide is 11-16 g / L, for example, 11 g / L, 12 g / L, 13 g / L, 14 g / L, 15 g / L, 16 g / L, etc.
[0062] In some embodiments, in the plating solution, the concentration of the complexing agent is 12-18 g / L, for example, 12 g / L, 13 g / L, 14 g / L, 15 g / L, 16 g / L, 17 g / L, 18 g / L, etc.
[0063] In some embodiments, in the plating solution, the concentration of the anode activator is 17-28 g / L, for example, 17 g / L, 18 g / L, 19 g / L, 20 g / L, 21 g / L, 22 g / L, 23 g / L, 24 g / L, 25 g / L, 26 g / L, 27 g / L, 28 g / L, etc.
[0064] In some embodiments, the concentration of the dispersant in the plating solution is 20-35 g / L, for example, 20 g / L, 22 g / L, 23 g / L, 25 g / L, 26 g / L, 27 g / L, 28 g / L, 30 g / L, 31 g / L, 32 g / L, 33 g / L, 34 g / L, 35 g / L, etc.
[0065] In some embodiments, in the coating 201 , the mass ratio of the second metal to the metal oxide-graphene oxide-nickel oxide composite is (48-66): (0.05-2.5).
[0066] In step S14: In some embodiments, the current density of the electroplating is 0.2-0.5 A / m 2 , for example, 0.2 A / m 2 , 0.3 A / m 2 , 0.4 A / m 2 , 0.5 A / m 2 In the current density range, it is beneficial to prepare the coating layer 201 with good film-forming property, thereby facilitating the preparation of the composite conductor 100 with high electrical conductivity, thermal conductivity and mechanical strength.
[0067] In some embodiments, during electroplating, the temperature of the plating solution is 16-24° C., for example, 16° C., 17° C., 18° C., 19° C., 20° C., 21° C., 22° C., 23° C., 24° C., etc. Within the temperature range, it is beneficial to prepare a plating layer 201 with good film-forming properties, thereby facilitating the preparation of a composite conductor 100 with high electrical conductivity, thermal conductivity and mechanical strength.
[0068] In some embodiments, during electroplating, the pH of the plating solution is 7.5-10.5, for example, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, etc. Within the pH range, it is beneficial to prepare a coating 201 with good film-forming properties, thereby facilitating the preparation of a composite conductor 100 with high electrical conductivity, thermal conductivity and mechanical strength.
[0069] In some embodiments, the thickness of the coating layer 201 is 0.2-1.2 µm, for example, 0.2 µm, 0.3 µm, 0.5 µm, 0.6 µm, 0.8 µm, 1.0 µm, 1.1 µm, 1.2 µm, etc. Within the above range, it is beneficial to prepare a composite conductor 100 with higher electrical conductivity, thermal conductivity and mechanical strength.
[0070] In step S15: In some embodiments, the second temperature is 850-1050°C, for example, 850°C, 860°C, 880°C, 900°C, 920°C, 930°C, 950°C, 960°C, 980°C, 1000°C, 1020°C, 1030°C, 1050°C, etc. Within the temperature range, it is beneficial to make the metal oxide in the coating layer 201 undergo oxygen evolution reaction to release oxygen and generate the third metal, it is beneficial to make the nickel oxide in the coating layer 201 undergo oxygen evolution reaction to release oxygen and generate nickel, and it is beneficial to make the graphene oxide in the coating layer 201 undergo oxygen evolution reaction to release oxygen and form defective graphene.
[0071] The carbon source includes, but is not limited to, one or more carbon sources known for preparing graphene by vapor deposition, such as methane, natural gas, acetylene, and propane.
[0072] The gas flow rate of the carbon source is 15 to 100 sccm, for example, 15 sccm, 20 sccm, 30 sccm, 40 sccm, 50 sccm, 60 sccm, 70 sccm, 80 sccm, 90 sccm, 100 sccm, etc.
[0073] A protective gas is introduced at the same time as the carbon source is introduced. It is understood that the term "at the same time" in the present application means that the introduction of the carbon source and the introduction of the protective gas have a common time period, and there is no particular restriction on the order of starting to introduce the carbon source and starting to introduce the protective gas, and there is no particular restriction on the order of ending to introduce the carbon source and ending to introduce the protective gas. In at least one embodiment, the introduction of the carbon source and the introduction of the protective gas start and end at the same time.
[0074] The protective gas includes, but is not limited to, one or more of nitrogen, helium, argon, and xenon.
[0075] In some embodiments, the gas flow rate of the protective gas is 0-1000 sccm, for example, 10 sccm, 50 sccm, 100 sccm, 150 sccm, 200 sccm, 250 sccm, 300 sccm, 500 sccm, 600 sccm, 800 sccm, 900 sccm, 1000 sccm, etc. It can be understood that when the flow rate of the protective gas is 0, it means that the protective gas is not introduced.
[0076] In some embodiments, a reducing gas is introduced at the same time as the carbon source is introduced. It is understood that the "simultaneous" in the present application means that the introduction of the carbon source and the introduction of the reducing gas have a common time period, and there is no particular restriction on the order of starting to introduce the carbon source and starting to introduce the reducing gas, and there is no particular restriction on the order of ending to introduce the carbon source and ending to introduce the reducing gas. In at least one embodiment, the introduction of the carbon source and the introduction of the reducing gas start and end at the same time.
[0077] The reducing gas may be a reducing gas known to be used for preparing graphene by a vapor deposition method, for example, may include but is not limited to hydrogen.
[0078] In some embodiments, the flow rate of the reducing gas is 5 to 500 sccm, for example, 5 sccm, 10 sccm, 50 sccm, 100 sccm, 150 sccm, 200 sccm, 250 sccm, 300 sccm, 350 sccm, 400 sccm, 450 sccm, 500 sccm, etc.
[0079] In some embodiments, the time for introducing the carbon source is 15 to 30 min, for example, 15 min, 18 min, 20 min, 22 min, 23 min, 25 min, 26 min, 28 min, 30 min, etc.
[0080] After placing the composite substrate 200 in a deposition chamber and before introducing a carbon source into the deposition chamber at a second temperature, the method includes heating the composite substrate 200 to the second temperature at a heating rate V.
[0081] In some embodiments, the heating rate V is 10 to 20°C / min, for example, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min, 15°C / min, 16°C / min, 17°C / min, 18°C / min, 19°C / min, 20°C / min, etc.
[0082] In some embodiments, before the carbon source is introduced into the deposition chamber at the second temperature, the method includes: performing a pre-cracking treatment on the carbon source to release hydrogen atoms from the carbon source to form free carbon (ie, carbon radicals).
[0083] The pre-cracking treatment is beneficial for effectively reducing the content of carbon impurities (i.e., insufficiently cracked substances) in the graphene layer when graphene is subsequently deposited on the composite substrate 200, and can make the prepared graphene have larger crystal domains and fewer grain boundaries, which is beneficial for preparing a composite conductor 100 with better electrical conductivity and thermal conductivity.
[0084] In some embodiments, the pre-lysis is performed in a sub-lysis chamber.
[0085] In some embodiments, the pre-cracking temperature is 850~1050°C, for example, 850°C, 860°C, 880°C, 900°C, 920°C, 930°C, 950°C, 960°C, 980°C, 1000°C, 1020°C, 1030°C, 1050°C, etc.
[0086] In some embodiments, the pre-cracking medium includes, but is not limited to, one or more of copper oxide and aluminum oxide.
[0087] In some embodiments, the pre-lysed medium may be in the form of a membrane layer, a plate layer, or a particle.
[0088] In some embodiments, after the carbon source is introduced into the deposition chamber at the second temperature, the process further includes: cooling down. In this way, the defective graphene melted in nickel at high temperature can be released and form the first graphene with complete structure and grain at the vacancies or defects (positions where oxygen-containing functional groups or oxygen are removed) on the surface of the third metal formed after the reduction of the metal oxide and at the vacancies or defects (positions where oxygen-containing functional groups or oxygen are removed) on the surface of the nickel formed after the reduction of nickel oxide, thereby filling the gaps or defects caused by the lack of oxygen-containing functional groups and / or oxygen, and at the same time, the content of graphene in the composite conductor can be increased, and the overall electrical conductivity, thermal conductivity, mechanical strength, stability and other properties of the composite conductor can be improved.
[0089] In some embodiments, the cooling rate is 10-15°C / min, for example, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min, 15°C / min, etc. Within the range of the cooling rate, a first graphene with complete structure and grains can be formed at the vacancies or defects (positions where oxygen-containing functional groups or oxygen is removed) on the surface of the third metal that is effectively released from the nickel and formed after the reduction of the metal oxide, and at the vacancies or defects (positions where oxygen-containing functional groups or oxygen is removed) on the surface of the nickel formed after the reduction of the nickel oxide.
[0090] In some embodiments, the end point temperature of the cooling is room temperature.
[0091] Second, see Figure 2 An embodiment of the present application provides a composite conductor 100, comprising a metal substrate 10, a transition layer 20 located on at least one surface of the metal substrate 10, and a graphene layer 30 located on a surface of the transition layer 20 away from the metal substrate 10, wherein the metal substrate 10 includes a first metal, the transition layer 20 includes nickel, a second metal, a third metal and a first graphene, and the graphene layer 30 includes a second graphene.
[0092] In some embodiments, the first graphene is bonded to the surface of the nickel and / or the surface of the third metal.
[0093] In some embodiments, the metal matrix 10 may be metal particles, metal wires or metal foils.
[0094] In some embodiments, the first metal includes but is not limited to one or more of a metal element and an alloy. The metal element includes but is not limited to one or more of Cu and Al, and the alloy includes but is not limited to one or more of a copper-nickel alloy, a copper-silver alloy, and a copper-zinc alloy.
[0095] In some embodiments, the second metal and the third metal each independently include, but are not limited to, one or more of Cu and Al.
[0096] It can be understood that the second metal is the same as or different from the third metal. In at least one embodiment, the second metal is the same as the third metal.
[0097] In at least one embodiment, the first metal, the second metal and the third metal are the same. Further, in at least one embodiment, the first metal, the second metal and the third metal are Cu.
[0098] In some embodiments, at least a portion of the nickel in the transition layer 20 forms an alloy with the second metal and / or the third metal, that is, at least a portion of the nickel exists in the form of an alloy with the second metal and / or the third metal.
[0099] In some embodiments, in the transition layer 20, by mass percentage, the content of the first graphene is 8-35%, the content of the nickel is 5-15%, and the balance is the second metal and the third metal. Within the content range, the composite conductor 100 is advantageously provided with higher electrical conductivity, thermal conductivity and mechanical strength.
[0100] The average sheet diameter of the first graphene is smaller than the average sheet diameter of the second graphene.
[0101] In some embodiments, the average sheet diameter of the first graphene is 0.01-0.1 μm, for example, 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, etc.
[0102] In some embodiments, the average sheet diameter of the second graphene is 2-6 μm, for example, 2 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, 2.5 μm, 2.6 μm, 2.7 μm, 2.8 μm, 2.9 μm, 3 μm, 3.2 μm, 3.5 μm, 3.6 μm, 3.8 μm, 4 μm, 4.2 μm, 4.5 μm, 4.6 μm, 4.8 μm, 5 μm, 5.3 μm, 5.5 μm, 5.8 μm, 6 μm, etc.
[0103] In some embodiments, the transition layer 20 has a thickness of 0.5-1.8 μm, for example, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, etc. Within the thickness range, the composite conductor 100 is advantageously provided with higher electrical conductivity, thermal conductivity and mechanical strength.
[0104] The thickness of the graphene layer 30 is 3 to 10 layers of graphene, for example, 3 layers of graphene, 4 layers of graphene, 5 layers of graphene, 6 layers of graphene, 7 layers of graphene, 8 layers of graphene, 9 layers of graphene, 10 layers of graphene, etc. Within the thickness range, the composite conductor 100 is advantageously provided with higher electrical conductivity, thermal conductivity and mechanical strength.
[0105] The electrical conductivity of the composite conductor 100 is 120-128% (IACS, International Annealed Copper Standard), for example, 120%, 121%, 122%, 123%, 124%, 125%, 126%, 127%, 128%, etc. The electrical conductivity of the composite conductor 100 described in the present application is relatively high, and can reach up to 128%.
[0106] The thermal conductivity of the composite conductor 100 is 420-435 W / (m•k), for example, 420 W / (m•k), 422 W / (m•k), 425 W / (m•k), 426 W / (m•k), 428 W / (m•k), 430 W / (m•k), 432 W / (m•k), 433 W / (m•k), 435 W / (m•k), etc. The electrical conductivity of the composite conductor 100 described in the present application is relatively high, up to 435 W / (m•k).
[0107] The composite conductor 100 described in the present application includes the transition layer 20, and the transition layer 20 has a certain inlay connection effect, which can enhance the bonding strength between the graphene layer 30 and the metal matrix 10, and help improve the electrical conductivity, thermal conductivity and mechanical strength of the composite conductor 100. Further, the transition layer 20 has fewer defects, which can make the transition layer 20 have better electrical conductivity, thereby effectively improving the electrical conductivity of the composite conductor 100. Further, the transition layer 20 includes a second metal, a third metal, a first graphene and nickel, wherein the first graphene and nickel can further improve the electrical conductivity of the composite conductor. In addition, the second graphene in the graphene layer 30 of the composite conductor 100 has a larger sheet diameter, that is, a larger grain size, which can make the composite conductor 100 have higher electrical conductivity, thermal conductivity and mechanical strength.
[0108] Third, see Figures 4 and 5 The embodiment of the present application further provides a coating 201, wherein the coating 201 includes a second metal and a metal oxide-graphene oxide-nickel oxide composite.
[0109] In some embodiments, the second metal includes, but is not limited to, one or more of Cu and Al.
[0110] In some embodiments, the metal oxide in the metal oxide-graphene oxide-nickel oxide composite includes, but is not limited to, one or more of copper oxide and aluminum oxide.
[0111] In some embodiments, in the metal oxide-graphene oxide-nickel oxide composite, the mass ratio of metal oxide, graphene oxide, and nickel oxide is 1:(1-1.9):(0.14-0.26).
[0112] In some embodiments, in the coating 201 , the mass ratio of the second metal to the metal oxide-graphene oxide-nickel oxide composite is (48-66): (0.05-2.5).
[0113] Fourth, please refer to Figures 4 and 5The embodiment of the present application further provides a composite substrate 200 , which includes a metal substrate 10 and a coating 201 bonded to at least one surface of the metal substrate 10 .
[0114] The metal substrate 10 and the coating 201 are as described above and will not be described again herein.
[0115] In a fifth aspect, the embodiments of the present application also provide an application of a composite conductor 100 , which can be used in any device that requires electrical and / or thermal conductivity, such as conductors such as wires and cables and electrical contacts.
[0116] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.
[0117] Example 1 Step S11, weigh 1 g of graphene oxide, dissolve it in 50 ml of water, and disperse it by ultrasonic to obtain a graphene oxide aqueous solution; weigh 0.14 g of nickel acetate (0.8 mmol) and dissolve it in 2.5 L of water, and obtain a nickel acetate solution after it is completely dissolved; add the graphene oxide aqueous solution to the nickel acetate solution, stir it thoroughly, and then add ammonia water to adjust the pH value to about 11 to obtain a mixed solution; place the mixed solution in a 100° C. oil bath for reflux reaction for 10 hours, and after the reaction is completed, filter and wash the mixed solution with deionized water to obtain an insoluble matter, heat the insoluble matter to 250° C. in air, and react for 12 hours to obtain a graphene oxide-nickel oxide composite; Step S12, weighing 0.5 g of copper oxide, 0.8 g of graphene oxide-nickel oxide composite, and 12 g of sodium citrate, heating at 90° C., reacting for 6 hours, to obtain a copper oxide-graphene oxide-nickel oxide composite; Step S13, mixing the copper oxide-graphene oxide-nickel oxide composite, cuprous cyanide, KCN, potassium hydroxide, potassium thiocyanate, potassium sodium tartrate and sodium dodecyl sulfate to obtain a plating solution, wherein the concentration of the copper oxide-graphene oxide-nickel oxide composite in the plating solution is 1.5 g / L, the concentration of cuprous cyanide is 60 g / L, the concentration of KCN is 115 g / L, the concentration of potassium hydroxide is 13 g / L, the concentration of potassium thiocyanate is 15 g / L, the concentration of potassium sodium tartrate is 22 g / L, and the concentration of sodium dodecyl sulfate is 27 g / L; Step S14: electroplating the copper foil surface with the plating solution to obtain a composite substrate 200 including a plating layer 201 with a thickness of 0.5 μm, wherein the current density of the electroplating is 0.35 A / m 2 , the plating solution temperature is 20° C., the plating solution pH value is 9, and the plating layer 201 includes copper and a copper oxide-graphene oxide-nickel oxide composite; Step S15, in a deposition chamber, under nitrogen protection, the composite substrate 200 is heated to 950°C at a heating rate of 15°C / min, and then methane, hydrogen and nitrogen are introduced to carry out graphene deposition, wherein the methane introduction amount is 60 sccm, the hydrogen introduction amount is 250 sccm, the nitrogen or argon introduction amount is 500 sccm, and the introduction time is 22 min. After the deposition is completed, the temperature is cooled to room temperature at a cooling rate of 12°C / min to obtain a composite conductor 100.
[0118] The composite conductor 100 of this embodiment includes a metal substrate 10, a transition layer 20 and a graphene layer 30 stacked in sequence. The metal substrate 10 is a copper foil, the transition layer 20 includes copper, nickel and a first graphene, and the graphene layer 30 includes a second graphene.
[0119] Example 2 This embodiment is substantially the same as embodiment 1, except that, in this embodiment, the amount of nickel acetate used is 0.09 g.
[0120] Example 3 This embodiment is substantially the same as embodiment 1, except that, in this embodiment, the amount of nickel acetate used is 0.2 g.
[0121] Example 4 This embodiment is substantially the same as embodiment 1, except that, in this embodiment, the amount of sodium citrate used is 5.6 g.
[0122] Example 5 This embodiment is substantially the same as embodiment 1, except that, in this embodiment, the amount of sodium citrate used is 14 g.
[0123] Example 6 This embodiment is substantially the same as embodiment 1, except that, in this embodiment, the amount of copper oxide used is 0.66 g.
[0124] Example 7 This embodiment is substantially the same as embodiment 1, except that, in this embodiment, the amount of copper oxide used is 0.37 g.
[0125] Comparative Example 1 Step A, exposing the copper foil to air, using an electric heating plate to treat at 105°C for 3 h to obtain a pre-oxidized copper foil; placing the pre-oxidized copper foil in a quartz boat, pushing it into a CVD tube furnace and evacuating it to 0.1 Pa and stabilizing it for 2 min, and then reducing annealing at 1025°C for 35 min in a mixed gas atmosphere of Ar and H2 (volume ratio 2:1); The pre-oxidized copper foil comprises a metal layer and a metal oxide layer located on a surface of the metal layer, the metal oxide layer comprises a first metal oxide layer bonded to the metal layer and a second metal oxide layer bonded to a surface of the first metal oxide layer away from the metal layer, the metal layer comprises copper, the first metal oxide layer comprises copper oxide and cuprous oxide, the second metal oxide layer comprises cupric oxide, the thickness of the first metal oxide layer is 0.25 μm, the thickness of the second metal oxide layer is 0.325 μm, and the mass ratio of cupric oxide to cuprous oxide in the first metal oxide layer is 0.03:1; Among them, the oxygen content in the pre-oxidized copper foil obtained after the electric heating plate was treated at 105°C for 3 hours was about 225 ppm, and the oxygen content in the pre-oxidized copper foil after reduction annealing was about 60 ppm; Step B: Then, CH4 gas (flow rate 20 sccm) was introduced into the system for 60 min, and then the introduction of CH4 gas was stopped, and the furnace cover was opened to cool naturally to room temperature to obtain a composite conductor.
[0126] The electrical conductivity IACS, thermal conductivity and Vickers hardness HV of the composite conductors of Examples 1 to 7 and Comparative Example 1 are 0.2 The test was carried out and the test results are shown in Table 1.
[0127] Table 1:
[0128] From Table 1 we can see that: The electrical conductivity of the composite conductor 100 of Examples 1 to 7 is above 120%, and can be as high as 128%, which is significantly improved compared to the composite conductor of Comparative Example 1 and the electrical conductivity of copper of 100%. It can be seen that the composite conductor 100 of the present application has better electrical conductivity; The thermal conductivity of the composite conductor 100 of Examples 1 to 7 is above 420 W / (m•k), and can be as high as 435 W / (m•k), which is significantly improved compared with the thermal conductivity of the composite conductor of Comparative Example 1 and copper. It can be seen that the composite conductor 100 of the present application has better thermal conductivity; The Vickers hardness of the composite conductors 100 of Examples 1 to 7 is above 56.2, which is significantly improved compared to the Vickers hardness of the composite conductor of Comparative Example 1 and copper. It can be seen that the composite conductor 100 of the present application has a relatively strong hardness.
[0129] The technical solutions provided by the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for technical personnel in this field, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A method for preparing a composite conductor, It is characterized in that The steps include: Mixing graphene oxide, a nickel compound and a solvent to obtain a first mixed solution, adding a base to the first mixed solution to obtain a second mixed solution, and heat-treating the second mixed solution to obtain a graphene oxide-nickel oxide composite; Mixing a metal oxide, a ligand, and a graphene oxide-nickel oxide composite, and heating at a first temperature to obtain a metal oxide-graphene oxide-nickel oxide composite; mixing the metal oxide-graphene oxide-nickel oxide composite with a base plating solution to obtain a plating solution; The plating solution is used to electroplate a metal substrate to obtain a composite substrate, wherein the composite substrate comprises a metal substrate and a plating layer bonded to at least one surface of the metal substrate, wherein the metal substrate comprises a first metal, and the plating layer comprises a second metal and a metal oxide-graphene oxide-nickel oxide composite; The composite substrate is placed in a deposition chamber, and a carbon source is introduced into the deposition chamber at a second temperature to react the metal oxide in the coating to generate a third metal, react the nickel oxide in the coating to generate nickel, and convert the graphene oxide in the coating to the first graphene, thereby obtaining a transition layer including the second metal, the third metal, nickel and the first graphene, and forming a graphene layer including the second graphene on the surface of the transition layer to obtain a composite conductor.
2. The preparation method according to claim 1, It is characterized in that Includes at least one of the following features (1) to (8): (1) The nickel compound includes one or more of nickel acetate, nickel chloride, and nickel nitrate; (2) The solvent includes water; (3) The base includes aqueous ammonia; (4) The metal oxide includes one or more of copper oxide and aluminum oxide; (5) The complexing agent includes sodium citrate; (6) The first metal includes one or more of a metal element and an alloy, the metal element includes one or more of Cu and Al, and the alloy includes one or more of a copper-nickel alloy, a copper-silver alloy, and a copper-zinc alloy; (7) The basic plating solution includes a metal salt, a cyanide, a hydroxide, a complexing agent, and an anode activator; (8) The metal matrix is metal particles, metal wires or metal foil.
3. The preparation method according to claim 1, It is characterized in that The invention comprises at least one of the following features (1) to (12): (1) The mass ratio of the graphene oxide to the nickel compound is 1:(0.09-0.2); (2) The pH value of the second mixed solution is 9-12; (3) The mass ratio of the graphene oxide-nickel oxide composite to the coordination agent is 1:(7-18); (4) The mass ratio of the metal oxide to the graphene oxide-nickel oxide composite is 1:(1.2-2.2); (5) In the plating solution, the concentration of the metal oxide-graphene oxide-nickel oxide composite is 0.5-2.5 g / L; (6) The first temperature is 85-95° C., and the heating time at the first temperature is 6-7 h; (7) The second temperature is 850-1050°C; (8) The current density of the electroplating is controlled to be 0.2~0.5 A / m2; (9) The thickness of the coating is 0.2 to 1.2 µm; (10) The gas flow rate of the carbon source is 15-100 sccm; (11) In the metal oxide-graphene oxide-nickel oxide composite, the mass ratio of metal oxide, graphene oxide and nickel oxide is 1:(1-1.9):(0.14-0.26); (12) In the coating, the mass ratio of the second metal to the metal oxide-graphene oxide-nickel oxide composite is (48-66): (0.05-2.5).
4. The preparation method according to claim 1, It is characterized in that The heat treatment comprises: reacting the mixed solution at a third temperature for a period of time T1 to obtain an insoluble substance; and heating the insoluble matter at a fourth temperature for a period of time T2; Wherein, the third temperature is 70-130° C., and the time T1 is 7-18 h; the fourth temperature is 220-280° C., and the time T2 is 8-15 h.
5. The preparation method according to claim 1, It is characterized in that Includes at least one of the following features (1) to (3): (1) after placing the composite substrate in a deposition chamber and before introducing a carbon source into the deposition chamber at a second temperature, the method comprises: heating the composite substrate to the second temperature at a heating rate V, wherein the heating rate V is 10 to 20°C / min; (2) A protective gas is introduced while the carbon source is introduced, and the gas flow rate of the protective gas is 0-1000 sccm; (3) A reducing gas is introduced at the same time as the carbon source, and the flow rate of the reducing gas is 5-500 sccm.
6. The preparation method according to claim 1, It is characterized in that Before the carbon source is introduced into the deposition chamber at the second temperature, the step includes: performing a pre-cracking treatment on the carbon source; wherein, The pre-cracking temperature is 850-1050°C; and / or The pre-cracking medium includes one or more of copper oxide and aluminum oxide.
7. The preparation method according to claim 1, It is characterized in that After the carbon source is introduced into the deposition chamber at the second temperature, the process further includes: cooling down; wherein, The cooling rate is 10-15°C / min; and / or The end point temperature of the cooling is room temperature.
8. A composite conductor, It is characterized in that It includes a metal substrate, a transition layer located on at least one surface of the metal substrate, and a graphene layer located on a surface of the transition layer away from the metal substrate, wherein the metal substrate includes a first metal, the transition layer includes nickel, a second metal, a third metal and a first graphene, and the graphene layer includes a second graphene.
9. The composite conductor according to claim 8, It is characterized in that The invention comprises at least one of the following features (1) to (10): (1) The first metal includes one or more of a metal element and an alloy, the metal element includes one or more of Cu and Al, and the alloy includes one or more of a copper-nickel alloy, a copper-silver alloy, and a copper-zinc alloy; (2) The second metal and the third metal each independently include one or more of Cu and Al; (3) The second metal and the third metal are the same or different; (4) The average sheet diameter of the first graphene is smaller than the average sheet diameter of the second graphene; (5) The average sheet diameter of the first graphene is 0.01-0.1 μm; (6) The average sheet diameter of the second graphene is 2 to 6 μm; (7) In the transition layer, by mass percentage, the content of the first graphene is 8-35%, the content of the nickel is 5-15%, and the balance is the second metal and the third metal; (8) The thickness of the transition layer is 0.5-1.8 μm; (9) The thickness of the graphene layer is 3 to 10 layers of graphene; (10) The metal matrix is metal particles, metal wires or metal foil.
10. A coating, It is characterized in that The plating layer includes a second metal and a metal oxide-graphene oxide-nickel oxide composite.
11. The coating according to claim 10, It is characterized in that Includes at least one of the following features (1) to (4): (1) The second metal includes one or more of Cu and Al; (2) The metal oxide in the metal oxide-graphene oxide-nickel oxide composite includes one or more of copper oxide and aluminum oxide; (3) In the metal oxide-graphene oxide-nickel oxide composite, the mass ratio of metal oxide, graphene oxide and nickel oxide is 1:(1-1.9):(0.14-0.26); (4) In the coating, the mass ratio of the second metal to the metal oxide-graphene oxide-nickel oxide composite is (48-66): (0.05-2.5).
12. A composite matrix, It is characterized in that The composite substrate comprises a metal substrate and a coating as described in any one of claims 10 to 11 bonded to at least one surface of the metal substrate.
13. The composite matrix according to claim 12, It is characterized in that Includes at least one of the following features (1) to (2): (1) The metal matrix includes a first metal, and the first metal includes one or more of a metal element and an alloy, the metal element includes one or more of Cu and Al, and the alloy includes one or more of a copper-nickel alloy, a copper-silver alloy, and a copper-zinc alloy; (2) The metal matrix is metal particles, metal wires or metal foils.
14. Use of the composite conductor according to any one of claims 8 to 9 as an electric wire or cable or an electric contact.