WO3 / BiVO4 / Ti3C2Tx composite photo-anode and preparation method and application thereof

By introducing Ti3C2Tx into the WO3/BiVO4 composite material, a WO3/BiVO4/Ti3C2Tx composite photoanode is formed, which solves the problems of complex preparation process and insufficient photoelectrocatalytic performance in the existing technology, achieving more efficient photoelectrocatalysis and stability, and is applicable In the fields of photoelectrocatalysis, batteries and photovoltaic devices.

CN118737708APending Publication Date: 2024-10-01SHENZHEN RES INST OF WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410773831.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing preparation methods of WO3/BiVO4 composite materials have problems such as long reaction time, complex processes, low efficiency, high energy consumption, and the inability to accurately control the bismuth vanadate composite loading, and the photoelectrocatalytic performance and stability need to be improved.

Method used

Using WO3/BiVO4/Ti3C2Tx composite photoanode, worm-shaped BiVO4 is loaded on the surface of nanoplate-shaped WO3 through a nano-stacked structure, and flake-shaped Ti3C2Tx is attached to its outer surface, using acidic tungsten The WO3/BiVO4 composite film is prepared by electrochemical deposition of the source solution and the bismuth source solution, and then the Ti3C2Tx solution is coated on the surface for heat treatment to form a WO3/BiVO4/Ti3C2Tx composite photoanode.

Benefits of technology

It simplifies the preparation process of WO3, improves the flexibility of BiVO4 load and photoelectrocatalytic performance, and significantly improves the stability and application potential of composite photoanode, especially in the fields of photoelectrocatalysis, batteries and photovoltaic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737708A_ABST
    Figure CN118737708A_ABST
Patent Text Reader

Abstract

The invention provides a WO3 / BiVO4 / Ti3C2Tx composite photo-anode as well as a preparation method and application thereof. The method comprises the following steps: firstly, preparing a WO3 film in situ by adopting a hydrothermal method, and converting the WO3 film into a monoclinic crystal form through heat treatment; performing electrochemical deposition in a three-electrode system by taking the WO3 thin film as a working electrode to obtain a bismuth oxyiodide / tungsten trioxide composite thin film; dropwise adding a vanadium source solution on the surface of the bismuth oxyiodide / tungsten trioxide composite film, and carrying out heat treatment to obtain a WO3 / BiVO4 composite film; and finally, spin-coating a Ti3C2Tx solution on the surface of the composite film, and carrying out heat treatment under a protective atmosphere to obtain the WO3 / BiVO4 / Ti3C2Tx composite photo-anode. The preparation method has the advantages of being simple, green, efficient, easy to implement and the like, and the prepared composite photoanode is excellent in comprehensive performance and has large application potential in the fields of energy and environment such as photoelectrocatalysis, batteries, photovoltaic devices and photodegradation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy and electrode materials, and in particular to a WO3 / BiVO4 / Ti3C2T x Composite photoanode and preparation method and application thereof. Background Art

[0002] Tungsten trioxide (WO3) is an n-type binary metal oxide semiconductor with a corresponding band gap of visible light (2.6-2.8eV), a long hole diffusion distance (about 150nm) and a high electron Hall mobility (about 12cm 2 v -1 s -1 ) and other characteristics. Monoclinic tungsten trioxide also exhibits excellent corrosion resistance and chemical stability, so it has received extensive attention in the field of photoelectrocatalysis and has become a photoanode semiconductor material with broad application prospects.

[0003] However, due to the slow kinetics of photogenerated holes and charge transfer at the WO3 / electrolyte interface, carriers are easily recombined, resulting in reduced photocatalytic efficiency. The commonly used and effective solution to this situation is to construct a composite photoanode, that is, to build a heterojunction structure. When semiconductors with different energy band structures are combined into a heterojunction structure, the different energy band properties of multiple semiconductors can be combined, and the photocurrent conversion efficiency can be enhanced through synergistic effects, reducing the probability of carrier recombination.

[0004] Bismuth vanadate (BiVO4) has a bandgap of 2.4 eV. It is often selected as a heterojunction semiconductor for compounding with tungsten trioxide. The compounding of the two can significantly improve the efficiency of carrier separation and inhibit the recombination of photogenerated holes. At present, the commonly used method for preparing WO3 / BiVO4 composite materials is the drop coating-heat treatment method, that is, the vanadium source and bismuth source are drop coated on the tungsten trioxide film and heat treated, and the drop coating-heat treatment process is repeated many times. However, this method has the problems of long reaction time, complicated process, low efficiency, high energy consumption, and inability to accurately control the composite loading of bismuth vanadate. In addition, the photoelectrocatalytic performance and stability of existing WO3 / BiVO4 composite materials also need to be improved. Summary of the invention

[0005] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a WO3 / BiVO4 / Ti3C2T x A composite photoanode comprising the following components in weight percentage: 57.8%-72.7% WO3, 28.1%-41.9% BiVO4 and 0.1%-0.3% Ti3C2T x .

[0006] Specifically, the composite photoanode has a nano-stacked structure, in which worm-like BiVO4 is loaded on the surface of nano-plate-like WO3 to form WO3 / BiVO4, and the outer surface of WO3 / BiVO4 is attached with flake Ti3C2T x Formation of WO3 / BiVO4 / Ti3C2T x .

[0007] More specifically, the Ti3C2T x The number of floors shall not exceed 20.

[0008] Specifically, the Ti3C2T x It is titanium carbide terminated with hydroxyl or fluorine atoms, that is, the end group T x Any one selected from -OH, -F, etc.

[0009] The second object of the present invention is to provide the above-mentioned WO3 / BiVO4 / Ti3C2T x The preparation method of the composite photoanode comprises the following steps: firstly, preparing an acidic tungsten source solution and using it to prepare a WO3 film; then, immersing the WO3 film in an acidic solution containing a bismuth source for electrochemical deposition, taking it out and dripping a solution containing a vanadium source on the surface of the film, and obtaining a WO3 / BiVO4 composite film after heat treatment; finally, coating the surface of the WO3 / BiVO4 composite film with a Ti3C2T x The solution was heat treated under protective atmosphere to obtain WO3 / BiVO4 / Ti3C2T x Composite photoanode.

[0010] Specifically, the preparation method of the acidic tungsten source solution is as follows: tungsten source, organic acid and solvent are uniformly mixed in a certain proportion, wherein the concentration of tungsten source in the solution is 0.03-0.06 mol / L, and the concentration of organic acid is 0.1-0.5 mol / L.

[0011] More specifically, the tungsten source is a mixture of tungstic acid and sodium tungstate in a mass ratio of 0.5:1-1:1, the organic acid is oxalic acid, and the solvent is water. Compared with a single-component tungsten source, a two-component tungsten source of tungstic acid + sodium tungstate has a faster hydrolysis rate in an acidic solution, can precipitate tungstate ions faster, and has a cost advantage.

[0012] Specifically, the preparation method of the WO3 film is as follows: immerse a substrate (such as tin-plated glass) in an acidic tungsten source solution, then heat it to 100-180°C and keep it warm for 6-18h, then take out the substrate, wash it with deionized water 2-3 times and dry it at 40-60°C, finally place the dried substrate in an air atmosphere, and heat treat it at 300-600°C for 1-3h to obtain a substrate with a monoclinic WO3 film on its surface, that is, a monoclinic WO3 film is prepared on the substrate carrier.

[0013] Specifically, the acidic solution containing the bismuth source is formed by mixing two solutions in a volume ratio of 1:1-10:1. The preparation method of the first solution is: dissolve potassium iodide and bismuth nitrate in water, and then add concentrated nitric acid to adjust the pH to 1.5-2.5. The preparation method of the second solution is: dissolve p-benzoquinone in ethanol. During the electrodeposition process, p-benzoquinone is reduced to hydroquinone, which increases the pH of the mixed solution and precipitates bismuth iodate. If the target solution is directly mixed at one time, it is easy to cause p-benzoquinone to react directly with potassium iodide, thereby causing the solution to denature, and it is easy to make the pH of the solution unstable, causing the deposition process to fail. .

[0014] More specifically, the concentration of potassium iodide in the first solution is 0.1-0.6 mol / L, and the mass ratio of bismuth nitrate to potassium iodide is 1:1-1:20; the concentration of p-benzoquinone in the second solution is 0.1-0.5 mol / L.

[0015] Specifically, the electrochemical deposition is achieved through an electrochemical workstation, and a three-electrode system is used, wherein the working electrode is a substrate with a WO3 film on the surface, the counter electrode is a platinum electrode, the reference electrode is a silver / silver chloride electrode, the applied bias voltage is -0.5V to -0.1V, and the deposition time is 50-500 seconds.

[0016] Specifically, the solution containing the vanadium source is a vanadyl acetylacetonate solution, and its concentration is 0.1-0.5 mol / L.

[0017] Specifically, after a solution containing a vanadium source is dripped onto the surface of the film, it is transferred to an air atmosphere and kept at 350-500° C. for reaction for 1-5 hours, and then an alkali solution (such as sodium hydroxide) is used to wash away the incompletely reacted bismuth iodide oxide and vanadium acetylacetonate.

[0018] Specifically, the Ti3C2T x The solution is specifically Ti3C2T x An aqueous solution with a concentration of 0.025-0.05 g / mL.

[0019] Specifically, the Ti3C2T x The solution is coated on the surface of the WO3 / BiVO4 composite film, and then transferred to an inert atmosphere (such as nitrogen, helium) and heated to 100-150°C for 1-3 hours.

[0020] The third object of the present invention is to provide the above-mentioned WO3 / BiVO4 / Ti3C2T x The application of composite photoanodes in energy and environment such as photoelectrocatalysis, batteries, photovoltaic devices, photodegradation, etc.

[0021] The present invention first deposits worm-like bismuth vanadate on monoclinic tungsten trioxide, and then uses Ti3C2T x After modification, WO3 / BiVO4 / Ti3C2T was finally obtained. x Composite photoanode. By adjusting the deposition time of bismuth vanadate, the loading thickness of bismuth vanadate in the composite photoanode can be flexibly adjusted. The composite photoanode thus prepared exhibits good electrocatalytic performance and stability, and has good application potential in energy and environmental fields such as photoelectrocatalysis, batteries, photovoltaic devices, and photodegradation.

[0022] Compared with the prior art, the advancement of the present invention is mainly reflected in the following points:

[0023] 1. The preparation method of WO3 is relatively simple and low-cost. WO3 is directly prepared by a hydrothermal method, and then a simple heat treatment is used to convert it into monoclinic WO3 with better performance.

[0024] 2. The method of loading BiVO4 on WO3 is relatively simple and easy to implement. The electrodeposition-heat treatment method replaces the traditional drop coating-heat treatment method, eliminating a series of cumbersome steps and processes. More importantly, the loading amount of BiVO4 is flexible and controllable.

[0025] 3. Nano-WO3 / BiVO4 photoanode was modified with Ti3C2Tx, and the comprehensive performance of the photoanode material was improved through strong interaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The XRD pattern of the composite photoanode prepared in Example 1-3;

[0027] Figure 2 WO3 / BiVO4 / Ti3C2T prepared in Example 1 x SEM image of the composite photoanode;

[0028] Figure 3 WO3 / BiVO4 / Ti3C2T prepared in Example 2 x SEM image of the composite photoanode;

[0029] Figure 4 This is a SEM photo of the WO3 / BiVO4 composite photoanode prepared in Example 3;

[0030] Figure 5 The graph is a relationship curve between the photocurrent density and bias voltage of the composite photoanode prepared in Examples 1-3. DETAILED DESCRIPTION

[0031] In order to enable ordinary technicians in the field to fully understand the technical solutions and beneficial effects of the present invention, further description is given below in conjunction with specific embodiments and drawings.

[0032] Example 1

[0033] Weigh 0.4g of tungstic acid and 0.6g of sodium tungstate and dissolve them in 20mL of water, then add 10mL of oxalic acid aqueous solution (concentration of 0.3mol / L) to obtain solution I. Transfer solution I to a polytetrafluoroethylene-lined hydrothermal autoclave, put in tin-coated glass (conductive surface facing down), heat to 100℃ and keep warm for 12h. After the reaction, take out the tin-coated glass, wash it with deionized water 2-3 times, and then fully dry it at 60℃ to obtain sample I. Place sample I in an air atmosphere, heat to 300℃ and keep warm for 1h to obtain sample II.

[0034] Take 1.4g potassium iodide and 0.5g bismuth nitrate and dissolve them in 20mL water, then add an appropriate amount of concentrated nitric acid to adjust the pH of the mixture to 1.7 to obtain solution II. Take 0.2g p-benzoquinone and dissolve it in 10mL ethanol to obtain solution III. Mix solution II and solution III in a volume ratio of 3:1, and then use a three-electrode system for electrochemical deposition. A platinum electrode is selected as the counter electrode, a silver / silver chloride electrode is used as the reference electrode, sample II is used as the working electrode, a bias voltage of -0.1V (relative to the reference electrode), and the deposition time is 50 seconds. After the deposition, sample III is obtained.

[0035] Transfer sample III to an air atmosphere, add 0.1 mL of 0.2 mol / L acetylacetonato vanadium solution IV onto its surface, heat to 500°C and react for 3 hours, then wash away the remaining reactants with 1 mol / L sodium hydroxide solution and dry at room temperature to obtain sample IV.

[0036] Take 0.5g -OH-terminated Ti3C2T x Dissolve in 20 mL of water to obtain solution V. Take 1 mL of solution V and spin-coat it on the surface of sample IV, and dry it at room temperature to obtain sample V.

[0037] The sample V was transferred to an argon atmosphere and heated to 100 °C for 2 h to obtain nano-WO3 / BiVO4 / Ti3C2T x Composite photoanode material. After sampling and analysis, it was found that the content of WO3 in the composite photoanode material was 68.6%, the content of BiVO4 was 31.3%, and the content of Ti3C2T x The content is 0.1%.

[0038] Figure 1 The nano WO3 / BiVO4 / Ti3C2T prepared in Example 1 x XRD spectrum of composite photoanode material. It can be seen from the figure that the sample has characteristic diffraction peaks of bismuth vanadate and tungsten trioxide. XThe loading content of Ti3C2T is low (only 0.1%), and x The Ti3C2T is highly dispersed on the WO3 / BiVO4 surface, so the XRD spectrum does not clearly show the Ti3C2T x characteristic peaks.

[0039] Figure 2 The nano WO3 / BiVO4 / Ti3C2T prepared in Example 1 x SEM image of the composite photoanode material. It can be seen from the figure that the worm-like nano-bismuth vanadate particles are loaded on the nano-plate-like tungsten trioxide, there are flake Ti3C2T-OH on the surface of WO3 / BiVO4, and the morphology of WO3 / BiVO4 is not destroyed.

[0040] Example 2

[0041] This embodiment is basically the same as embodiment 1, except that the deposition time is 100 seconds, and -F-terminated Ti3C2T x As a modifier.

[0042] The sampling test results show that the content of WO3 in the composite photoanode material prepared in this embodiment is 62.3%, the content of BiVO4 is 37.6%, and the content of Ti3C2T x The content is 0.1%.

[0043] The nano WO3 / BiVO4 / Ti3C2T prepared in this embodiment x The XRD spectrum of the composite photoanode material is shown in Figure 1 As shown. Figure 1 It can be seen that the sample also has characteristic diffraction peaks of bismuth vanadate and tungsten trioxide.

[0044] The nano WO3 / BiVO4 / Ti3C2T prepared in this embodiment x SEM images of composite photoanode materials are shown in Figure 3 It can also be seen from the figure that the worm-like nano-bismuth vanadate particles are loaded on the nano-plate-like tungsten trioxide, there are flake Ti3C2T-F on the surface of WO3 / BiVO4, and the morphology of WO3 / BiVO4 is not destroyed.

[0045] Example 3

[0046] This embodiment is basically the same as Embodiment 1, except that the deposition time is 200 seconds and no Ti3C2Tx is loaded.

[0047] The sampling test results show that the content of WO3 in the composite photoanode material prepared in this embodiment is 54.7%, and the content of BiVO4 is 45.3%.

[0048] The XRD spectrum of the nano-WO3 / BiVO4 composite photoanode material prepared in this embodiment is as follows: Figure 1 As shown. Figure 1 It can be seen that the sample also has characteristic diffraction peaks of bismuth vanadate and tungsten trioxide.

[0049] The SEM image of the nano-WO3 / BiVO4 composite photoanode material prepared in this embodiment is as follows: Figure 3 As shown in the figure, it can also be seen that the worm-like nano-bismuth vanadate particles are loaded on the nano-plate-like tungsten trioxide, but the surface of WO3 / BiVO4 is relatively smooth and there is no Ti3C2T x exist.

[0050] In order to fully understand the performance of the three photoanodes prepared in Examples 1-3, samples were taken for photoelectrochemical tests to evaluate the relationship between the photocurrent density of the three photoanodes and the applied bias voltage under a simulated sunlight environment. The Autolab electrochemical workstation was used for photoelectrochemical testing. The test system used was a traditional three-electrode system, in which the three photoanodes prepared were used as working electrodes (working area of ​​1×1 square centimeter), silver / silver chloride as a reference electrode, platinum as a counter electrode, and the electrolyte was a 0.1M phosphate buffer solution (pH=7). A xenon lamp was used as the light source for the photoelectric test, and a filter was added to simulate sunlight, where the simulated sunlight intensity was AM1.5G. The relationship between photocurrent and bias voltage was tested by linear sweep voltammetry, and the applied voltage range was 0.4-1.3V (compared to silver / silver chloride electrodes). Comparison of the photocurrent density values ​​of the three different photoanodes in Examples 1-3 when the applied bias voltage was 1.23V (water decomposition voltage) was explored to modify Ti3C2T x The photoelectric properties of the composite WO3 / BiVO4 photoanode are shown in the following table. Figure 5 shown.

[0051] Depend on Figure 5 It can be seen that when the bias voltage is 1.23 V, the photocurrent density of the WO3 / BiVO4 / Ti3C2T-OH photoanode in Example 1 is 1.53442 mA cm -2 The photocurrent density of the WO3 / BiV O4 / Ti3C2T-F photoanode in Example 2 is 1.41785 mA·cm -2 This indicates that Ti3C2T x The modified WO3 / BiVO4 photoanode exhibited different performances in photoelectrocatalysis. Generally, -OH has stronger hydrophilicity than -F in photoelectrocatalytic water decomposition, so the photocurrent density of the WO3 / BiVO4 / Ti3C2T-OH photoanode in Example 1 was higher. However, compared with Example 3, when the bias voltage was 1.23V, the photocurrent density of the unmodified Ti3C2T xThe photocurrent density of the WO3 / BiVO4 photoanode is 0.82397 mA cm -2 This indicates that Ti3C2T x Modification of the WO3 / BiVO4 photoanode can significantly increase its photocurrent density, that is, improve the photoelectrocatalytic performance.

Claims

1. WO3 / BiVO4 / Ti3C2T x A composite photoanode, characterized in that The composite photoanode includes the following components in weight percentage: 57.8%-72.7% WO3, 28.1%-41.9% BiVO4, 0.1%-0.3% Ti3C2T x .

2. WO3 / BiVO4 / Ti3C2T as claimed in claim 1 x A composite photoanode, characterized in that: T x Any one selected from -OH, -F.

3. WO3 / BiVO4 / Ti3C2T as claimed in any one of claims 1 to 2 x The preparation method of the composite photoanode is characterized in that The method comprises the following steps: preparing an acidic tungsten source solution and using the solution to prepare a WO3 film; immersing the WO3 film in an acidic solution containing a bismuth source for electrochemical deposition, taking the film out and dripping a solution containing a vanadium source on the film surface, and obtaining a WO3 / BiVO4 composite film after heat treatment; coating the surface of the WO3 / BiVO4 composite film with a Ti3C2T x The solution was heat treated under protective atmosphere to obtain WO3 / BiVO4 / Ti3C2T x Composite photoanode.

4. The method according to claim 3, characterized in that The preparation method of the acidic tungsten source solution is as follows: tungsten source, organic acid and solvent are uniformly mixed in a certain proportion, wherein the tungsten source is a mixture of tungstic acid and sodium tungstate with a mass ratio of 0.5:1-1:1, the organic acid is oxalic acid, and the solvent is water. The concentration of the tungsten source in the acidic tungsten source solution is 0.03-0.06 mol / L, and the concentration of the organic acid is 0.1-0.5 mol / L.

5. The method according to claim 3, characterized in that The preparation method of the WO3 film is as follows: immersing the substrate in an acidic tungsten source solution, then heating it to 100-180°C for heat preservation reaction, taking out the substrate, washing, drying it, placing it in an air atmosphere, and heat treating it at 300-600°C to obtain a substrate with a monoclinic WO3 film loaded on its surface.

6. The method according to claim 3, characterized in that: The acidic solution containing a bismuth source is prepared by mixing two solutions in a volume ratio of 1:1-10:1, wherein the first solution is prepared by dissolving potassium iodide and bismuth nitrate in water, and then adding concentrated nitric acid to adjust the pH to 1.5-2.5, the concentration of potassium iodide in the solution is 0.1-0.6 mol / L, and the mass ratio of bismuth nitrate to potassium iodide is 1:1-1:20; the second solution is prepared by dissolving p-benzoquinone in ethanol, and the concentration of p-benzoquinone in the solution is 0.1-0.5 mol / L.

7. The method according to claim 3, characterized in that: Electrochemical deposition was achieved by an electrochemical workstation and a three-electrode system was used, wherein the working electrode was a substrate with a WO3 film on the surface, the counter electrode was a platinum electrode, the reference electrode was a silver / silver chloride electrode, the applied bias was -0.5 V to -0.1 V, and the deposition time was 50-500 seconds.

8. The method according to claim 3, characterized in that: After a solution containing a vanadium source is dripped onto the surface of the film, it is transferred to an air atmosphere and kept reacting at 350-500° C., and then washed with an alkali solution; the solution containing a vanadium source is specifically a vanadium acetylacetonate solution with a concentration of 0.1-0.5 mol / L.

9. The method according to claim 3, characterized in that: The Ti3C2T x The solution is coated on the surface of the WO3 / BiVO4 composite film, and then transferred to an inert atmosphere and heated to 100-150°C for heat preservation reaction; the Ti3C2T x The solution is specifically Ti3C2T x An aqueous solution with a concentration of 0.025-0.05 g / mL.

10. WO3 / BiVO4 / Ti3C2T as claimed in any one of claims 1 to 2 x Applications of composite photoanodes in photoelectrocatalysis, batteries, photovoltaic devices, and photodegradation.