Method for realizing high-strength room-temperature bonding of wafer-level metal

By evaporating the metal layer on the wafer surface and performing patterning processing and wet activation, combined with argon ion bombardment, high-strength room-temperature bonding of wafer-level metals is achieved, which solves the problems of thermal stress and insufficient bonding area, and improves bonding efficiency. The composite strength and stability are maintained while maintaining compatibility with the original process.

CN118737841APending Publication Date: 2024-10-01NO 55 INST CHINA ELECTRONIC SCI & TECHNOLOGYGROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410744247.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, higher bonding temperatures will introduce thermal stress, affecting the stability and success of the metal bonding process, and the effective area of ​​wafer-level metal bonding is insufficient and the bonding strength is weak.

Method used

A metal layer is evaporated to prepare a metal layer on the surface of the wafer to be bonded, and is patterned and then subjected to wet activation treatment and argon ion bombardment. A high vacuum environment and bonding stress are set to achieve high-strength room temperature bonding of metals at the wafer level.

Benefits of technology

Through patterning processing and argon ion bombardment, the problems of bonding stress dispersion and thermal stress are solved, the bonding strength and effective area are improved, the reliability and stability of the wafer are ensured, and it is compatible with the original chip manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737841A_ABST
    Figure CN118737841A_ABST
Patent Text Reader

Abstract

The invention discloses a method for realizing wafer-level metal high-strength room-temperature bonding, which comprises the following steps of: respectively evaporating metal layers on the surfaces of wafers to be bonded, carrying out graphical processing on the surfaces of the metal layers of one or two wafers to be bonded, carrying out wet activation processing on the wafers to be bonded with the metal layers subjected to the graphical processing, and drying to obtain the wafer-level metal high-strength room-temperature bonding. The method comprises the following steps: bombarding the surface of a wafer to be bonded by using a composite ion beam mainly comprising argon ions, and setting conditions of a high-vacuum cavity environment, bonding stress and bonding time to realize high-strength room-temperature bonding of wafer-level metal; the patterned metal designed by the invention can solve the problem that the bonding stress is dispersed in the pressurized bonding process due to the large contact area of the whole surface of the wafer, the maximization of the pressure intensity in the unit area is realized, and meanwhile, the metal room-temperature bonding also solves the problem of thermal stress introduced by the traditional heating bonding; and the reliability and the stability of the wafer after metal bonding are further ensured, and a low-stress, room-temperature and high-reliability implementation method is provided for a wafer-level heterogeneous integration technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor process technology, and in particular to a method for achieving high-strength room-temperature bonding of wafer-level metals. Background Art

[0002] Wafers are the basic materials of the entire semiconductor technology. Wafer bonding technology is to tightly combine two homogeneous or heterogeneous wafers through chemical and physical effects, thereby realizing the electrical interconnection, functional integration and device packaging of micro-electromechanical systems. It has been widely used in RF devices, microwave photonic devices, information processing devices and 3D integrated logic circuits. Metal is widely used as an intermediate bonding layer in wafer bonding and packaging technology. However, limited by the principle of bonding by metal atom diffusion, metal bonding often requires a higher temperature (>300°C). For heterogeneous wafers, on the basis of thermal mismatch and lattice mismatch, higher bonding temperature will further introduce thermal stress, which greatly affects the stability and success of the metal bonding process.

[0003] In addition, since the wafer itself has a certain degree of warping, and the application of stress during the bonding process will result in too little force per unit area due to the large contact area of ​​the two wafers to be bonded, wafer-level full-surface bonding will have problems such as small effective bonding area and weak bonding strength. Therefore, it is urgent to develop a method that is both convenient and effective to achieve wafer-level metal room temperature bonding, increase the effective bonding area and bonding strength, and ensure the stability of the bonding process and compatibility with subsequent processes. Summary of the invention

[0004] Technical issues solved:

[0005] The technical problem to be solved by the present application is that, based on the thermal mismatch and lattice mismatch, a higher bonding temperature will further introduce thermal stress, greatly affecting the stability and success of the metal bonding process, and in view of the problems of insufficient effective bonding area and weak bonding strength, a method for achieving high-strength room-temperature bonding of metals at the wafer level is provided, wherein a metal layer is prepared by respectively evaporating the surface of a wafer to be bonded, the metal layer is patterned, the wafer to be bonded with the patterned metal layer is wet activated, and then dried, and the surface of the metal to be bonded is bombarded with a composite ion beam mainly composed of argon ions, and high vacuum chamber environment, bonding stress, bonding time and other conditions are set to achieve high-strength room-temperature bonding of metals at the wafer level.

[0006] Technical solution:

[0007] A method for achieving high-strength room-temperature bonding of wafer-level metals comprises the following steps:

[0008] The first step is to prepare a metal bonding layer by evaporation on the surface of the wafer to be bonded;

[0009] The second step is to perform patterning on the upper surface of the metal bonding layer of one or two wafers to be bonded;

[0010] The third step is to perform wet activation treatment on the wafer to be bonded after the patterning treatment, and then dry it;

[0011] The fourth step is to set a high vacuum degree in the bonding equipment chamber, bombard the surface of the wafer to be bonded with a composite ion beam mainly composed of argon ions or a single argon ion, set the bonding stress and bonding time parameters, and achieve wafer-level high-strength metal bonding at room temperature.

[0012] As a preferred technical solution of the present application: in the first step, the wafer to be bonded is a heterogeneous or homogeneous wafer of one or more semiconductors selected from Si, GaAs, GaN, InP, and SiC; the metal bonding layer is one or more selected from Cu, Sn, In, and Au, and the thickness of the metal bonding layer is between 50nm and 500nm.

[0013] As a preferred technical solution of the present application: the patterning treatment performed in the second step is performed on the upper surface of the metal bonding layer of one of the wafers to be bonded, or the upper surfaces of the metal bonding layers of both wafers to be bonded.

[0014] As a preferred technical solution of the present application: the second step is to pattern the upper surface of the metal bonding layer by using a photolithography method to prepare a groove or bump structure, thereby reducing the contact surface area of ​​the wafer to be bonded and increasing the pressure intensity per unit area. The width w of the groove or bump structure pattern is in the range of 1μm to 2μm, and the length h is in the range of 50nm to 500nm.

[0015] As a preferred technical solution of the present application: the photolithography method first coats photoresist on the surface of the wafer to be bonded, and uses a photolithography process to expose the pattern, with the energy set to 1750-2000 mj / cm 2 , the focal length is set to 0-1.5, the development time is set to 60-120s, and the Ti / Au layer is evaporated continuously for 20 / 500nm. After peeling, an Au bonding layer structure with a groove structure is prepared.

[0016] As a preferred technical solution of the present application: the wet activation treatment is to use a hydrochloric acid solution with a volume concentration of 5% or 10% and a mixed solution for immersion cleaning for 60 seconds respectively, wherein the mixed solution is composed of a hydrogen peroxide solution: ammonia solution: water in a volume ratio of 1:1:5, to clean and activate the surface of the wafer to be bonded, and the drying is to place the wafer to be bonded after the wet activation treatment on a 110°C hot plate for 10 minutes of drying.

[0017] As a preferred technical solution of this application: high vacuum means that the vacuum degree in the bonding equipment cavity is less than 10-6 Pa.

[0018] As a preferred technical solution of the present application: the composite ion beam mainly composed of argon ions is a composite ion beam of argon ions, oxygen ions and hydrogen ions, in which argon ions account for 70-80%, oxygen ions account for 10-20% and hydrogen ions account for 0-20%.

[0019] As a preferred technical solution of the present application: the composite ion beam mainly composed of argon ions is a composite ion beam of argon ions and oxygen ions, in which argon ions account for 70-80% and oxygen ions account for 10-20%, the gas flow rate of argon ions is 40sccm, the bombardment power is 120w, the gas flow rate of oxygen ions is 10sccm, the bombardment power is 90w, and the bombardment time is 5min. The surface of the wafer to be bonded is bombarded to activate and clean the surface.

[0020] As a preferred technical solution of the present application: the bonding stress is set to 9000-16000N, and the bonding time is 0.5-1h, so as to achieve wafer-level metal high-strength room temperature bonding.

[0021] Principle explanation: By setting a graphic structure on the surface of the wafer to be bonded after evaporating the metal bonding layer, the problem of dispersion of bonding stress during pressurized bonding due to the large contact area of ​​the entire wafer surface can be solved, and the pressure per unit area can be maximized, which can effectively improve the bonding strength and effective bonding area of ​​the entire wafer-level metal bonding.

[0022] Beneficial effects:

[0023] The method for achieving high-strength room-temperature bonding of wafer-level metals described in the present application adopts the above technical solution and has the following technical effects compared with the prior art:

[0024] 1. By setting a graphic structure on the surface of the wafer to be bonded after evaporating the metal bonding layer, the problem of bonding stress dispersion during pressure bonding can be solved due to the large contact area of ​​the entire surface of the wafer;

[0025] 2. Maximize the pressure per unit area. At the same time, room temperature metal bonding also solves the thermal stress problem introduced by low temperature bonding in traditional hot pressing, further ensuring the reliability and stability of the wafer after metal bonding;

[0026] 3. This method does not require changing the original chip manufacturing process and is compatible with the original process. It is a convenient and efficient method to enhance the room temperature bonding strength of wafer-level metals;

[0027] 4. By setting a graphic structure on the surface of the wafer to be bonded after evaporating the metal bonding layer, the problem of bonding stress dispersion during pressure bonding due to the large contact area of ​​the entire surface of the wafer can be solved, and the pressure per unit area can be maximized, which can effectively improve the bonding strength and effective bonding area of ​​the entire wafer-level metal bonding;

[0028] 5. By setting a graphic structure on the surface of the wafer to be bonded after evaporating the metal bonding layer, the problem of the dispersion of bonding stress during pressure bonding due to the large contact area of ​​the entire surface of the wafer can be solved, and the pressure can be maximized per unit area. At the same time, metal room temperature bonding also solves the thermal stress problem introduced by low temperature bonding in traditional hot pressing, further ensuring the reliability and stability of the wafer after metal bonding. This method does not require changing the original chip manufacturing process and is compatible with the original process. It is a convenient and efficient method to enhance the strength of wafer-level metal room temperature bonding. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic diagram of a process for realizing a wafer-level high-strength room-temperature metal bonding method provided in an embodiment of the present application;

[0030] Figure 2 For this application, a metal bonding layer is prepared by evaporating on the upper surfaces of two wafers to be bonded;

[0031] Figure 3 This is a schematic diagram of patterning preparation on the upper surface of the metal bonding layer of the wafer to be bonded in this application;

[0032] Figure 4 For the present application, the wafer to be bonded after the patterning treatment is subjected to wet activation treatment, and then a drying process is performed after the treatment.

[0033] Figure 5 In this application, the surface of the wafer to be bonded is bombarded with a composite ion beam of argon ions and oxygen ions to activate and clean the surface;

[0034] Figure 6 For this application, the bonding stress, bonding time and other parameters are set to achieve wafer-level metal high-strength room temperature bonding.

[0035] Explanation of reference numerals: 1. GaAs wafer to be bonded; 2. SiC wafer to be bonded; 3. Metal bonding layer. DETAILED DESCRIPTION

[0036] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0037] Embodiment 1:

[0038] A method for achieving high-strength room-temperature bonding of wafer-level metals, the specific steps are as follows:

[0039] Step S01, preparing a metal bonding layer 3 by evaporation on the surface of the wafer to be bonded;

[0040] Specifically, the wafer to be bonded is a heterogeneous or homogeneous wafer of one or more semiconductors selected from Si, GaAs, GaN, InP, and SiC. Figure 2 As shown, in this embodiment, the wafers to be bonded are selected as the wafer to be bonded GaAs 1 and the wafer to be bonded SiC2, and heterogeneous wafer bonding is performed;

[0041] Further, a metal bonding layer 3 is prepared by evaporation on the surface of the wafer to be bonded. The metal bonding layer 3 is one or more of Cu, Sn, In, and Au. The thickness of the metal bonding layer 3 is 50 nm to 500 nm. Figure 2 As shown, in this embodiment, the metal selected is Au, and the evaporated thickness is 500nm;

[0042] Step S02, performing patterning on the upper surface of the metal bonding layer of one or two wafers to be bonded;

[0043] Specifically, the patterning process is performed on the upper surface of the metal bonding layer of one of the wafers to be bonded, or the upper surfaces of the metal bonding layers of the two wafers to be bonded are patterned, such as Figure 3 As shown, in this embodiment, the surface of the metal bonding layer 3 of the GaAs wafer 1 to be bonded is subjected to patterning treatment;

[0044] The metal bonding layer 3 is further subjected to a graphic treatment, such as Figure 3 As shown in the figure, firstly, a photoresist is coated on the surface of the GaAs 1 wafer to be bonded, and the pattern is exposed using a photolithography process, with the energy set to 1750-2000 mj / cm 2 , the focal length is set to 0-1.5, the development time is set to 60-120s, and the Ti / Au layer is evaporated continuously for 20 / 500nm, and after peeling, an Au bonding layer structure with a groove structure is prepared;

[0045] Further, the width w of the groove or convex structure pattern is in the range of 1 μm to 2 μm, and the length h is in the range of 50 nm to 500 nm. The width w of the groove or convex structure pattern prepared in this embodiment is 2 μm, and the length h is 500 nm.

[0046] Step S03, performing wet activation treatment on the patterned wafer to be bonded, and drying after the treatment;

[0047] The wet activation treatment is to use a hydrochloric acid solution with a volume concentration of 5% or 10% and a mixed solution to soak and clean for 60 seconds respectively, wherein the mixed solution is composed of a volume ratio of hydrogen peroxide: ammonia solution: water = 1:1:5, to clean and activate the surface of the wafer to be bonded, and the drying is to place the wafer to be bonded after the wet activation treatment on a hot plate at 110°C for 10 minutes for drying. Figure 4 As shown;

[0048] Step S04, setting a high vacuum degree in the bonding equipment chamber, bombarding the surface of the wafer to be bonded with a composite ion beam mainly composed of argon ions or a single argon ion, setting bonding stress and bonding time parameters, and achieving wafer-level metal high-strength room temperature bonding;

[0049] Specifically, a high vacuum is set, and the surface of the wafer to be bonded is bombarded with a composite ion beam mainly composed of argon ions;

[0050] Further setting of high vacuum degree is to set the ambient vacuum degree in the bonding equipment cavity. In this embodiment, the vacuum degree is set to 10 -6 Pa;

[0051] The composite ion beam mainly composed of argon ions is a composite ion beam of argon ions and oxygen ions, in which argon ions account for 70-80% and oxygen ions account for 10-20%, the gas flow rate of argon ions is 40sccm, the bombardment power is 120w, the gas flow rate of oxygen ions is 10sccm, the bombardment power is 90w, and the bombardment time is 5min. The surface of the wafer to be bonded is bombarded to activate and clean the surface. Figure 5 As shown;

[0052] Specifically, the bonding stress is set to 9000-16000N, the bonding time is 0.5-1h, and high-strength room-temperature bonding of wafer-level metal is achieved. In this embodiment, the bonding force is set to 10000N, the bonding time is 40min, and the bonding temperature is room temperature, so as to achieve high-strength room-temperature bonding of wafer-level metal. Figure 6 shown.

[0053] In summary, the present invention discloses a method for achieving high-strength room-temperature bonding of wafer-level metals, by evaporating metal layers on the surfaces of wafers to be bonded, patterning the metal layers, wet-activating the wafers to be bonded with the patterned metal layers, drying, bombarding the surfaces of the wafers to be bonded with a composite ion beam mainly composed of argon ions, setting conditions such as a high vacuum chamber environment, bonding stress, and bonding time, to achieve high-strength room-temperature bonding of wafer-level metals. The patterned metal designed by the present invention can solve the problem of the dispersion of bonding stress during pressurized bonding due to the large contact area of ​​the entire surface of the wafer, and maximize the pressure per unit area. At the same time, metal room-temperature bonding also solves the problem of thermal stress introduced by traditional heated bonding, further ensuring the reliability and stability of the wafers after metal bonding, and providing a low-stress, room-temperature, and highly reliable implementation method for wafer-level heterogeneous integration technology.

[0054] Embodiment 2:

[0055] A method for achieving high-strength room-temperature bonding of wafer-level metals, the specific steps are as follows:

[0056] Step S01, preparing a metal bonding layer by evaporating on the surface of the wafer to be bonded;

[0057] Specifically, the wafer to be bonded is a heterogeneous or homogeneous wafer of one or more semiconductors of Si, GaAs, GaN, InP, and SiC. In this embodiment, the wafer to be bonded is selected as a Si wafer, and homogeneous wafer bonding is performed;

[0058] Further, a metal bonding layer is prepared by evaporation on the surface of the wafer to be bonded. The metal bonding layer is one or more of Cu, Sn, In, and Au. The thickness of the metal bonding layer is 50-500 nm. In this embodiment, the metal is Sn, and the evaporated thickness is 250 nm.

[0059] Step S02, performing patterning on the upper surface of the metal bonding layer of one or two wafers to be bonded;

[0060] Specifically, the patterning process is performed on the upper surface of the metal bonding layer of one of the wafers to be bonded, or the upper surfaces of the metal bonding layers of both wafers to be bonded. In this embodiment, the patterning process is performed on the surface of the metal bonding layer of the Si wafer to be bonded;

[0061] The metal bonding layer is further patterned. First, photoresist is coated on the surface of the wafer to be bonded, and the pattern is exposed using a photolithography process with an energy setting of 1750-2000 mj / cm 2, the focal length is set to 0-1.5, the development time is set to 60-120s, and the Ti / Ni / Sn / Au layers are evaporated continuously for 20 / 20 / 250 / 50nm. After peeling, a Sn bonding layer structure with a groove structure is prepared;

[0062] Further, the width w of the groove or convex structure pattern is in the range of 1 μm to 2 μm, and the length h is in the range of 50 nm to 500 nm. The width w of the groove or convex structure pattern prepared in this embodiment is 2 μm, and the length h is 250 nm.

[0063] Step S03, performing wet activation treatment on the patterned wafer to be bonded, and drying after the treatment;

[0064] The wet activation treatment is to use a hydrochloric acid solution with a volume concentration of 5% or 10% and a mixed solution to soak and clean for 60 seconds respectively, wherein the mixed solution is composed of a volume ratio of hydrogen peroxide: ammonia solution: water = 1:1:5, to clean and activate the surface of the wafer to be bonded, and the drying is to place the wafer to be bonded after the wet activation treatment on a hot plate at 110°C for 10 minutes of drying treatment;

[0065] Step S04, setting a high vacuum degree in the bonding equipment chamber, bombarding the surface of the wafer to be bonded with a composite ion beam mainly composed of argon ions or a single argon ion, setting bonding stress and bonding time parameters, and achieving wafer-level metal high-strength room temperature bonding;

[0066] Specifically, a high vacuum is set, and the surface of the wafer to be bonded is bombarded with a single argon ion;

[0067] Further setting the high vacuum degree is to set the ambient vacuum degree in the bonding equipment cavity. In this embodiment, the vacuum degree is set to 5E-6pa;

[0068] The single argon ion bombards the metal surface to be bonded, playing the role of activation and further cleaning;

[0069] Further set a suitable gas flow rate and bombardment power to bombard the metal surface of the wafer to be bonded. In this embodiment, the gas flow rate of argon ions is set to 40 sccm and the bombardment power is set to 120w;

[0070] Specifically, the bonding stress is set to 9000-16000N, and the bonding time is 0.5-1h to achieve high-strength room-temperature bonding of wafer-level metals. In this embodiment, the bonding force is set to 16000N, the bonding time is 60min, and the bonding temperature is room temperature to achieve high-strength room-temperature bonding of wafer-level metals.

[0071] The above-described embodiments are only preferred embodiments of the present invention, and the embodiments are not intended to limit the patent protection scope of the present invention. Therefore, all equivalent changes made using the description and drawings of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for achieving high-strength room-temperature bonding of wafer-level metals. It is characterized in that The following steps are involved: The first step is to prepare a metal bonding layer by evaporation on the surface of the wafer to be bonded; The second step is to perform patterning on the upper surface of the metal bonding layer of one or two wafers to be bonded; The third step is to perform wet activation treatment on the wafer to be bonded after the patterning treatment, and then dry it; The fourth step is to set a high vacuum degree in the bonding equipment chamber, bombard the surface of the wafer to be bonded with a composite ion beam mainly composed of argon ions or a single argon ion, set the bonding stress and bonding time parameters, and achieve wafer-level high-strength metal bonding at room temperature.

2. A method for achieving high-strength room-temperature bonding of wafer-level metals according to claim 1, Features: In the first step, the wafer to be bonded is a heterogeneous or homogeneous wafer of one or more semiconductors selected from Si, GaAs, GaN, InP, and SiC; the metal bonding layer is one or more selected from Cu, Sn, In, and Au, and the thickness of the metal bonding layer is between 50 nm and 500 nm.

3. A method for achieving wafer-level high-strength room-temperature metal bonding according to claim 1, Features: The second step is to perform the patterning process on the upper surface of the metal bonding layer of one of the wafers to be bonded, or the patterning process is performed on the upper surfaces of the metal bonding layers of both wafers to be bonded.

4. A method for achieving wafer-level high-strength room-temperature metal bonding according to claim 1, Features: The second step is to pattern the upper surface of the metal bonding layer by using a photolithography method to prepare a groove or bump structure, reduce the contact surface area of ​​the wafer to be bonded, and increase the pressure intensity per unit area. The width w of the groove or bump structure pattern ranges from 1μm to 2μm, and the length h ranges from 50nm to 500nm.

5. A method for achieving wafer-level high-strength room-temperature metal bonding according to claim 4, Features: The photolithography method first coats photoresist on the surface of the wafer to be bonded, and uses a photolithography process to expose the pattern, with the energy set to 1750-2000 mj / cm 2 , the focal length is set to 0-1.5, the development time is set to 60-120s, and the Ti / Au layer is evaporated continuously for 20 / 500nm. After peeling, an Au bonding layer structure with a groove structure is prepared.

6. A method for achieving wafer-level high-strength room-temperature metal bonding according to claim 1, Features: The wet activation treatment is to use a hydrochloric acid solution and a mixed solution with a volume concentration of 5% or 10% for cleaning for 60 seconds respectively, wherein the solution is composed of a volume ratio of hydrogen peroxide: ammonia solution: water = 1:1:5, to clean and activate the surface of the wafer to be bonded, and the drying is to place the wafer to be bonded after the wet activation treatment on a 110°C hot plate for 10 minutes of drying.

7. A method for achieving wafer-level high-strength room-temperature metal bonding according to claim 1, Features: The high vacuum refers to the vacuum degree in the bonding equipment cavity being lower than 10 -6 Pa.

8. A method for achieving wafer-level high-strength room-temperature metal bonding according to claim 1, Features: The composite ion beam mainly composed of argon ions is a composite ion beam of argon ions, oxygen ions and hydrogen ions, in which argon ions account for 70-80%, oxygen ions account for 10-20% and hydrogen ions account for 0-20%.

9. A method for achieving wafer-level high-strength room-temperature metal bonding according to claim 8, Features: The composite ion beam mainly composed of argon ions is a composite ion beam of argon ions and oxygen ions, in which argon ions account for 70-80% and oxygen ions account for 10-20%. The gas flow rate of argon ions is 40sccm, the bombardment power is 120w, the gas flow rate of oxygen ions is 10sccm, the bombardment power is 90w, and the bombardment time is 5min. The surface of the wafer to be bonded is bombarded to activate and clean the surface.