Method for measuring thickness of chemical plating metal layer film
By setting the XRF test point on the front side of the wafer above the gate, using the insulating gate dielectric layer to avoid charge accumulation, and measuring on the back side, the problem of reduced electrical performance measurement accuracy caused by XRF measurement is solved and improves The accuracy of thickness measurement is improved.
Patent Information
- Application Number
- CN202410693101.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-10-01
AI Technical Summary
When measuring the thickness of double-sided plated wafers through X-ray fluorescence spectroscopy (XRF), it is easy to reduce the accuracy of subsequent electrical performance measurements, especially since the front measurement point is located above the device source. Affects the accuracy of electrical performance measurements.
By setting the first test point on the front side of the wafer in the area above the gate for XRF measurement, it is difficult to accumulate charges at the bottom of the insulating gate dielectric layer, thereby reducing the impact on subsequent electrical performance measurements, and setting the third test point on the back side. Two test points are measured to obtain the thickness of the chemically plated metal layer.
The accuracy of thickness measurement of double-sided plated wafers is improved and the impact on subsequent electrical performance measurements is reduced.
Smart Images

Figure CN118737868A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of semiconductor devices and integrated circuits, and in particular to a method for measuring the thickness of a chemically plated metal layer film. Background Art
[0002] Chemical plating (hereinafter referred to as "chemical plating") is a metal deposition process in which metal ions in the plating solution are reduced on a substrate with a catalytic surface under the catalytic action of a reducing agent to obtain free metal atoms, while the metal-like atoms formed by the decomposition of the reducing agent form a dense alloy coating.
[0003] On a wafer integrated with power devices (e.g., insulated-gate bipolar transistor (IGBT) devices), a chemically plated metal layer (typically, the chemically plated metal layer formed is a nickel-palladium-gold (NiPbAu) film) can be formed on the metal layer on the front and the metal layer on the back through a chemical plating process, thereby achieving efficient conductive interconnection.
[0004] Usually, when the thickness of a double-sided electroless-plated wafer is measured by X-ray fluorescence (XRF), the measurement point on the front side is located above the source of the device. However, measuring through this measurement point will cause the threshold voltage (V th ) offset, thus affecting the accuracy of electrical performance measurement. Summary of the invention
[0005] The present application provides a method for measuring the thickness of a chemically plated metal layer film, which can solve the problem provided in the related art that the thickness measurement of a double-sided chemically plated wafer by XRF easily leads to a decrease in the accuracy of subsequent electrical performance measurement. The method comprises:
[0006] A wafer is provided, wherein a semiconductor device and a first metal pad and a second metal pad located above the semiconductor device are integrated on the front side of the wafer, wherein the first metal pad is used to lead out a gate of the semiconductor device, and the second metal pad is used to lead out a source of the semiconductor device, and a metal layer is formed on the back side of the wafer, and a chemically plated metal layer is formed on the first metal pad, the second metal pad and the metal layer, and the chemically plated metal layer is a metal layer formed by a chemical plating process;
[0007] Measuring a first test point by XRF to obtain the thickness of the chemically plated metal layer on the front side of the wafer, wherein the first test point is located in the area where the first metal pad is located;
[0008] The thickness of the chemically plated metal layer on the back side of the wafer is obtained by measuring a second test point by XRF, wherein the second test point is located on the back side of the wafer and is opposite to the first test point.
[0009] In some embodiments, the electroless plated metal layer includes a nickel layer, a palladium layer, and a gold layer.
[0010] In some embodiments, the nickel layer has a thickness of 1 micrometer to 3 micrometers.
[0011] In some embodiments, the palladium layer has a thickness of 0.05 micrometers to 0.25 micrometers.
[0012] In some embodiments, the gold layer has a thickness of 0.03 micrometers to 0.07 micrometers.
[0013] In some embodiments, the wafer has a thickness of 50 microns to 100 microns.
[0014] The technical solution of this application has at least the following advantages:
[0015] When measuring the thickness of double-sided plated wafers using XRF, the test point on the front side is set in the area above the gate. Since there is an insulating gate dielectric layer under the gate, it is difficult for charge to accumulate at its bottom, thereby reducing the impact on subsequent electrical performance measurements and improving measurement accuracy. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0017] Figure 1 It is a flow chart of a method for measuring the thickness of a chemically plated metal layer provided by an exemplary embodiment of the present application;
[0018] Figure 2 is a front plan view of a double-sided chemically plated wafer provided by an exemplary embodiment of the present application;
[0019] Figure 3 is a top view of the back side of a double-sided chemically plated wafer provided by an exemplary embodiment of the present application;
[0020] Figure 4 It is a partial top view schematic diagram of the test area on the front side of the wafer;
[0021] Figure 5 is a partial top view schematic diagram of the test area on the back side of the wafer;
[0022] Figure 6 It is a schematic diagram of a local cross-section of the test area of the wafer. DETAILED DESCRIPTION
[0023] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in this application. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0024] In the description of the present application, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0025] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, it can also be the internal connection of two components, it can be a wireless connection, or it can be a wired connection. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0026] In addition, the technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0027] refer to Figure 1 , which shows a flow chart of a method for measuring the thickness of a chemically plated metal layer provided by an exemplary embodiment of the present application, such as Figure 1 As shown, the method includes:
[0028] Step S1, providing a wafer, the front side of the wafer integrating a semiconductor device and a first metal pad and a second metal pad located above the semiconductor device, the first metal pad being used to lead out a gate of the semiconductor device, the second metal pad being used to lead out a source of the semiconductor device, a metal layer being formed on the back side of the wafer, a chemically plated metal layer being formed on the first metal pad, the second metal pad and the metal layer, the chemically plated metal layer being a metal layer formed by a chemical plating process.
[0029] For example, Figure 2 and Figure 3 As shown, the semiconductor device ( Figure 2 and Figure 3 The device (not shown) may be a power device (for example, an IGBT device), and the surface of the back side of the wafer 200 is a chemically plated metal layer 212 .
[0030] refer to Figure 4 , which shows Figure 2 The front view of the area 201 shown by the dashed line; Figure 5 , which shows Figure 2 The back side top view of the area 201 shown by the dotted line; Figure 6 , which shows Figure 4 Schematic diagram of the cross section along the AA' direction. Figures 4 to 6 As shown, an interlayer dielectric (ILD) layer 230 is formed on the front side of the wafer 200, and a first metal pad 221 and a second metal pad 222 are formed in the interlayer dielectric layer 230. The first metal pad 221 leads to the gate of the semiconductor device, and the second metal pad 222 is used to lead to the source of the semiconductor device. The first metal pad 221 and the gate can be connected through a metal interconnect structure ( Figure 6 The second metal pad 222 and the source electrode can be electrically connected through a metal interconnect structure (not shown) formed in the interlayer dielectric layer 230. Figure 6 A metal layer 223 is formed on the back of the wafer 200, a chemically plated metal layer 211 is formed on the first metal pad 221 and the second metal pad 222, and a chemically plated metal layer 212 is formed on the metal layer 223.
[0031] Optionally, the electroless metal layer 212 includes a nickel layer, a palladium layer and a gold layer, wherein the thickness of the nickel layer is 1 micrometer (μm) to 3 micrometers, the thickness of the palladium layer is 0.05 micrometers to 0.25 micrometers, and the thickness of the gold layer is 0.03 micrometers to 0.07 micrometers; optionally, the thickness of the wafer 200 is 50 micrometers to 100 micrometers.
[0032] Step S2, measuring the first test point by XRF to obtain the thickness of the chemically plated metal layer on the front side of the wafer, the first test point is located in the area where the first metal pad is located.
[0033] Exemplarily, a position on the area where the first metal pad 221 is located (when viewed from a top view) can be selected as the first test point. Since the first metal pad 221 is used to lead out the gate of the semiconductor device, the gate of the semiconductor device is directly below it, and an insulating gate dielectric layer is formed below the gate. When XRF is used for measurement, the wafer surface is excited to produce free electrons that are not easy to penetrate, and it is difficult to form charge accumulation in the substrate below it.
[0034] Step S3, measuring the second test point by XRF to obtain the thickness of the chemically plated metal layer on the back side of the wafer, the second test point is located on the back side of the wafer and is opposite to the first test point.
[0035] For example, the coordinates of the second test point may be determined according to the coordinates of the first test point, and then the second test point may be measured by XRF to obtain the thickness of the chemically plated metal layer 212 on the back side.
[0036] To summarize, in the embodiment of the present application, during the thickness measurement of the double-sided plated wafer by XRF, the test point on the front side is set in the area above the gate. Since there is an insulating gate dielectric layer under the gate, it is difficult for charge to accumulate at its bottom, thereby reducing the impact on subsequent electrical performance measurements and improving the accuracy of the measurement.
[0037] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection created by this application.
Claims
1. A method for measuring the thickness of a chemically plated metal layer, characterized in that: include: A wafer is provided, wherein a semiconductor device and a first metal pad and a second metal pad located above the semiconductor device are integrated on the front side of the wafer, wherein the first metal pad is used to lead out a gate of the semiconductor device, and the second metal pad is used to lead out a source of the semiconductor device, and a metal layer is formed on the back side of the wafer, and a chemically plated metal layer is formed on the first metal pad, the second metal pad and the metal layer, and the chemically plated metal layer is a metal layer formed by a chemical plating process; Measuring a first test point by XRF to obtain the thickness of the chemically plated metal layer on the front side of the wafer, wherein the first test point is located in the area where the first metal pad is located; The thickness of the chemically plated metal layer on the back side of the wafer is obtained by measuring a second test point by XRF, wherein the second test point is located on the back side of the wafer and is opposite to the first test point.
2. The method according to claim 1, characterized in that The chemically plated metal layer comprises a nickel layer, a palladium layer and a gold layer.
3. The method according to claim 2, characterized in that The thickness of the nickel layer is 1 micron to 3 microns.
4. The method according to claim 3, characterized in that The thickness of the palladium layer is 0.05 micrometer to 0.25 micrometer.
5. The method according to claim 4, characterized in that The thickness of the gold layer is 0.03 micrometer to 0.07 micrometer.
6. The method according to any one of claims 1 to 5, characterized in that: The thickness of the wafer is 50 microns to 100 microns.