Solar cell and photovoltaic module

By arranging a passivation contact layer and a doping layer on the substrate surface of the solar cell, and arranging a passivation dielectric layer on the away side surface, the problem of high manufacturing cost is solved, and efficiency improvement and process simplification are achieved.

CN118738153APending Publication Date: 2024-10-01JINKO SOLAR (SHANGRAO) CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411067068.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The manufacturing cost of existing solar cells is high, making it difficult to reduce costs while improving efficiency.

Method used

The first surface of the substrate is used to set the passivation contact layer and the doping layer, and the first passivation dielectric layer is set on the away side surface. The passivation effect is achieved through the tunneling layer and the doped conductive layer, simplifying the process steps and reducing costs. .

Benefits of technology

The passivation effect and efficiency of solar cells are improved, while the production steps are simplified and the manufacturing cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738153A_ABST
    Figure CN118738153A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solar cells, in particular to a solar cell and a photovoltaic module. In the embodiment of the invention, the passivation contact layer is arranged in the first region of the first surface of the substrate, and the doped layer and the first passivation dielectric layer are arranged in the second region of the first surface of the substrate, so that on one hand, the passivation contact layer comprises the tunneling layer and the doped conductive layer, so that the first region can have a relatively good passivation effect; and on the other hand, the manufacturing steps of the doping layer are simpler and more convenient than those of the passivation contact layer, so that the passivation effect of the second region can be improved by the first passivation dielectric layer. Compared with the mode that the passivation contact layers are arranged in the first area and the second area, the manufacturing steps of the solar cell provided by the embodiment of the invention are simpler and more convenient. Compared with the mode that the first region and the second region are provided with the doping layers, the solar cell provided by the embodiment of the invention has a better passivation effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to solar cells and photovoltaic modules. Background Art

[0002] BC cell (Back Contact) is a type of solar cell. Its main feature is that the PN junction and metal electrode are both placed on the back of the solar cell, so that there is no electrode blocking the front of the solar cell, thereby increasing the area of ​​the cell absorbing sunlight, thereby improving the conversion efficiency and generating more electricity. However, in order to improve the efficiency of BC cells, the manufacturing cost is often too high. Summary of the invention

[0003] Based on this, it is necessary to provide a solar cell and a photovoltaic module to reduce the manufacturing cost while the solar cell has a certain efficiency.

[0004] According to one aspect of the present application, an embodiment of the present application provides a solar cell, including:

[0005] A substrate having a first surface and a second surface arranged opposite to each other; the first surface of the substrate comprises a first area and a second area adjacent to the first area;

[0006] A passivation contact layer is provided in the first region; the passivation contact layer comprises a tunneling layer and a doped conductive layer stacked and provided in the first region of the first surface;

[0007] a doped layer disposed in the second region; and

[0008] The first passivation dielectric layer is arranged on a surface of the doped layer which is away from the substrate.

[0009] In one embodiment, the first passivation dielectric layer includes at least a first doped oxide layer.

[0010] In one embodiment, the material of the first doped oxide layer includes doped silicon oxide;

[0011] Wherein, the doped element in the first doped oxide layer includes a P-type doping element; or

[0012] The elements doped in the first doped oxide layer include P-type doping elements and N-type doping elements.

[0013] In one embodiment, the doped element in the first doped oxide layer includes a P-type doped element, and the doped element in the first doped oxide layer includes boron; or

[0014] The elements doped in the first doped oxide layer include a P-type doping element and an N-type doping element, and the elements doped in the first doped oxide layer include boron and phosphorus.

[0015] In one of the embodiments, the solar cell further comprises a second passivation dielectric layer;

[0016] The second passivation dielectric layer is arranged on a surface of the doped conductive layer which is away from the tunneling layer.

[0017] In one embodiment, the thickness of the first passivation dielectric layer is greater than the thickness of the second passivation dielectric layer.

[0018] In one embodiment, the second passivation dielectric layer includes at least a second doped oxide layer.

[0019] In one embodiment, the material of the second doped oxide layer includes doped silicon oxide;

[0020] Wherein, the doped elements in the second doped oxide layer include N-type doping elements.

[0021] In one embodiment, the doped element in the second doped oxide layer includes phosphorus.

[0022] In one embodiment, the doped layer and the first surface define a separation plane; along the first direction, the dimension between the side surface of the doped conductive layer away from the substrate and the second surface is a first dimension, and the dimension between the separation plane and the second surface is a second dimension; the first dimension is less than or equal to the second dimension; and / or

[0023] The doped layer comprises a doped diffusion layer; and / or

[0024] The thickness of the first passivation dielectric layer is less than or equal to 300 nm and greater than or equal to 50 nm.

[0025] According to another aspect of the present application, an embodiment of the present application provides a photovoltaic assembly, including:

[0026] Battery string;

[0027] An encapsulation layer, used to cover the surface of the battery string; and

[0028] A cover plate, which is used to cover the surface of the packaging layer away from the battery string;

[0029] The battery string is formed by connecting the solar cells in any of the above embodiments.

[0030] In the above-mentioned solar cell and photovoltaic module, the solar cell at least includes a substrate, a passivation contact layer, a doping layer and a first passivation dielectric layer. By setting a passivation contact layer in the first region of the first surface of the substrate and setting a doping layer and a first passivation dielectric layer in the second region of the first surface of the substrate, on the one hand, since the passivation contact layer includes a tunneling layer and a doped conductive layer, the first region can have a better passivation effect. On the other hand, since the manufacturing steps of the doping layer are simpler than the manufacturing steps of the passivation contact layer, the first passivation dielectric layer can improve the passivation effect of the second region. Compared with the method of setting a passivation contact layer in both the first region and the second region, the manufacturing steps of the solar cell provided in the embodiment of the present application are simpler. Compared with the method of setting a doping layer in both the first region and the second region, the solar cell provided in the embodiment of the present application has a better passivation effect. Therefore, the solar cell provided in the embodiment of the present application not only has a certain passivation effect, and thus can have a certain efficiency, but also can simplify the process steps, and thus can reduce the manufacturing cost.

[0031] Additional aspects and advantages of the embodiments of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the embodiments below. The accompanying drawings are only for the purpose of illustrating the embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0033] Figure 1 is a schematic diagram of a cross-sectional structure of a solar cell in one embodiment of the present application;

[0034] Figure 2 is a schematic cross-sectional structure diagram of a solar cell in another embodiment of the present application;

[0035] Figure 3 is a schematic cross-sectional structural diagram of a solar cell in another embodiment of the present application;

[0036] Figure 4 is a schematic cross-sectional structural diagram of a solar cell in yet another embodiment of the present application;

[0037] Figure 5 is a schematic cross-sectional structural diagram of a solar cell in another embodiment of the present application;

[0038] Figure 6 is a schematic cross-sectional structural diagram of a solar cell in yet another embodiment of the present application;

[0039] Figure 7is a schematic cross-sectional structural diagram of a solar cell in yet another embodiment of the present application;

[0040] Figure 8 It is a schematic diagram of the structure of a photovoltaic module in one embodiment of the present application.

[0041] Description of reference numerals:

[0042] Solar cell 100;

[0043] Substrate 110, first surface m1, second surface m2, first area z1, second area z2;

[0044] Passivation contact layer 120, tunneling layer 121, doped conductive layer 122;

[0045] doped layer 130, separation plane s;

[0046] A first passivation dielectric layer 140, a first doped oxide layer 141;

[0047] A second passivation dielectric layer 150, a second doped oxide layer 151;

[0048] A first anti-reflection layer 160;

[0049] A first electrode 170a, a second electrode 170b;

[0050] Passivation film layer 180;

[0051] A second anti-reflection layer 190;

[0052] Isolation structure G;

[0053] Photovoltaic module 10, battery string 11, encapsulation layer 12, cover plate 13, conductive tape 14;

[0054] A first size h1, a second size h2, a first thickness d1, and a second thickness d2;

[0055] The first direction F1, the second direction F2, and the third direction F3. DETAILED DESCRIPTION

[0056] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0057] In the description of the present application, it should be understood that if the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. appear, the orientation or position relationship indicated by these terms is based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the present application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.

[0058] In addition, if the terms "first" or "second" appear, these terms are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of this application, if the term "plurality" appears, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0059] In this application, unless otherwise clearly specified and limited, if the terms "installed", "connected", "connected", "fixed" and the like appear, these terms should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly limited. It is worth noting that in the following description and the attached claims, "electrical connection" between one feature and another feature not only includes one feature directly contacting another feature to form an electric energy transmission or current transmission channel, but also includes an intermediate feature between one feature and another feature, and the one feature, the other feature and the intermediate feature between them form an electric energy transmission channel or a current transmission channel to achieve electric energy transmission or transmission. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0060] In the present application, unless otherwise clearly specified and limited, if there is a description that a first feature is "above" or "below" a second feature, etc., or similar descriptions appear, it may mean that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediate medium. Moreover, the first feature being "above", "above" and "above" the second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. The first feature being "below", "below" and "below" the second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0061] It should be noted that if an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. If an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. If any, the terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used in this application are for illustrative purposes only and do not represent the only implementation method.

[0062] The solar cell and photovoltaic module according to the embodiment of the present application are described below with reference to the accompanying drawings.

[0063] Figure 1 The cross-sectional structure diagram of a solar cell 100 in an embodiment of the present application is shown; for ease of explanation, only the contents related to the embodiment of the present application are shown. In the embodiment of the present application, for ease of explanation, the solar cell 100 is taken as a back contact solar cell 100 (Back Contact, BC) as an example for explanation.

[0064] Please refer to Figure 1 The embodiment of the present application provides a solar cell 100, including a substrate 110, a passivation contact layer 120, a doping layer 130 and a first passivation dielectric layer 140. In the embodiment of the present application, the first direction F1 is the thickness direction of the substrate 110, the second direction F2 and the third direction F3 may be the length direction and the width direction of the substrate 110, respectively, and the first direction F1, the second direction F2 and the third direction F3 are perpendicular to each other. It should be noted that the size of the substrate 110 along the length direction may be greater than or equal to the size in the width direction, and no specific limitation is made here.

[0065] The substrate 110 has doping elements in it, and the doping element type is N-type or P-type. The N-type element can be a V-group element such as phosphorus (P), bismuth (Bi), antimony (Sb), or arsenic (As), and the P-type element can be a III-group element such as boron (B), aluminum (Al), gallium (Ga), or indium (In). For example, when the substrate 110 is a P-type substrate, the doping element type inside it is P-type. For another example, when the substrate 110 is an N-type substrate, the doping element type inside it is N-type.

[0066] Exemplarily, the thickness of the substrate 110 may be 100 µm-240 µm. For example, the thickness of the substrate 110 may be 100 µm, 110 µm, 130 µm, 150 µm, 170 µm, 190 µm, 200 µm or 240 µm. The thickness may be selected according to the specific usage, and is not specifically limited here.

[0067] The substrate 110 has a first surface m1 and a second surface m2 that are arranged opposite to each other. The first surface m1 and the second surface m2 are arranged opposite to each other along a first direction F1. Both the first surface m1 and the second surface m2 can be used to receive incident light. In the embodiment of the present application, the first surface m1 of the substrate 110 is a backlight surface, and the second surface m2 of the substrate 110 is a light-receiving surface. It can be understood that the light-receiving surface and the backlight surface are relative, and the light-receiving surface is specifically the surface on which sunlight mainly irradiates in the solar cell 100 or on the substrate 110 in the photovoltaic module. With the development of solar cell 100 technology, the backlight surface will also receive energy from sunlight, mainly from reflected light or scattered light in the surrounding environment.

[0068] The first surface m1 and the second surface m2 of the substrate 110 may be provided with a velvet structure, which can increase the light absorption area, increase the photocurrent, and help improve the efficiency of the solar cell 100. Figure 1 For example, the case where the second surface m2 of the substrate 110 is provided with a velvet structure is illustrated. Exemplarily, the second surface m2 of the substrate 110 can be subjected to a velvet treatment so that the second surface m2 of the substrate 110 forms a velvet structure. The velvet structure can be a pyramid velvet structure. As a common velvet structure, the pyramid velvet structure not only reduces the reflectivity of the second surface m2 of the substrate 110, but also forms a light trap, enhances the absorption effect of the substrate 110 on the incident light, and increases the conversion efficiency of the solar cell 100. The second surface m2 of the substrate 110 can also be subjected to a velvet treatment according to the use requirements. Of course, the first area z1 of the first surface m1 can also be provided with a velvet structure.

[0069] The first surface m1 of the substrate 110 includes first regions z1 and second regions z2 alternately arranged along a preset direction. It can be understood that the preset direction is relative to the first surface m1. When the first surface m1 is substantially planar, the preset direction is substantially parallel to the first surface m1.

[0070] In the embodiment of the present application, Figure 1 For example, the case where the preset direction is the second direction F2 is illustrated. The first area z1 and the second area z2 are alternately arranged along the preset direction, which means that the areas adjacent to the first area z1 are all the second areas z2, and the areas adjacent to the second area z2 are all the first areas z1. For example, when multiple first areas z1 and second areas z2 are provided, combined with reference Figure 1 , can be arranged alternately along the second direction F2 in the order of the first area z1, the second area z2, the first area z1, the second area z2, the first area z1..., or can be arranged alternately along the second direction F2 in the order of the second area z2, the first area z1, the second area z2, the first area z1, the second area z2..., without specific limitation here. For another example, when there are two first areas z1 and one second area z2, they can be arranged alternately along the second direction F2 in the order of the first area z1, the second area z2, the first area z1. It can be set according to the specific usage, without specific limitation here. In addition, the size of the first area z1 and the second area z2 along the preset direction can also be set according to the actual usage requirements, without specific limitation here.

[0071] The passivation contact layer 120 is disposed in the first region z1. It can be understood that in the embodiment of the present application, the passivation contact layer 120 is located in the first region z1 of the backlight surface of the substrate 110. The passivation contact layer 120 can reduce the recombination of carriers on the surface of the substrate 110, thereby increasing the open circuit voltage of the solar cell 100 and improving the photoelectric conversion efficiency of the solar cell 100. Among them, the passivation contact layer 120 may include a tunneling layer 121 and a doped conductive layer 122. Specifically, the passivation contact layer 120 includes a tunneling layer 121 and a doped conductive layer 122 stacked in the first region z1 of the first surface m1. That is, the tunneling layer 121 and the doped conductive layer 122 are stacked in sequence on the first region z1 of the first surface m1 of the substrate 110 in a direction away from the second surface m2.

[0072] The tunneling layer 121 is used to achieve the interface passivation of the first area z1 of the first surface m1 of the substrate 110, and has the effect of chemical passivation. Specifically, by saturating the dangling bonds of the first area z1 of the first surface m1, the interface trapped state density of the first area z1 of the first surface m1 is reduced, thereby reducing the recombination center of the first area z1 of the first surface m1 to reduce the carrier recombination rate. Among them, the material of the tunneling layer 121 can be a dielectric material, for example, at least one of silicon oxide, amorphous silicon, polycrystalline silicon, silicon carbide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide. The material of the doped conductive layer 122 can be doped polysilicon, or doped polysilicon containing at least one element of oxygen, carbon, and nitrogen. Among them, the doping element type of the doped conductive layer 122 can be the same as or opposite to the doping element type of the substrate 110. In the embodiment of the present application, the tunneling layer 121 can be formed by low pressure chemical vapor deposition (LPCVD, Low Pressure Chemical Vapor Deposition). Of course, the tunnel layer 121 may also be manufactured by other processes such as thermal oxidation process, plasma oxidation process or nitric acid oxidation process, which is not specifically limited here.

[0073] Exemplarily, the thickness of the tunneling layer 121 may be 0.1 nm-5 nm. For example, the thickness of the tunneling layer 121 may be 0.1 nm, 0.3 nm, 0.5 nm, 1 nm, 2 nm, 3 nm, 4 nm or 5 nm. The thickness may be selected according to the specific use case and is not specifically limited here. By controlling the thickness of the tunneling layer 121, it is possible to suppress the reduction of the fill factor caused by the contact resistance while having a certain passivation effect.

[0074] Exemplarily, the material of the doped conductive layer 122 may be phosphorus-doped polysilicon. The thickness of the doped conductive layer 122 may be 100 nm-300 nm. For example, the thickness of the doped conductive layer 122 may be 100 nm, 120 nm, 150 nm, 180 nm, 200 nm, 230 nm or 300 nm. The thickness may be selected according to the specific use case and is not specifically limited here.

[0075] The doping layer 130 is disposed in the second region z2. It can be understood that in the embodiment of the present application, the doping layer 130 is located in the second region z2 of the backlight surface of the substrate 110. The doping element type of the doping layer 130 is opposite to the doping element type of the doping conductive layer 122. Exemplarily, the doping element type of the doping layer 130 is P-type, the doping element type of the doping conductive layer 122 is N-type, and the doping element type of the substrate 110 can be P-type or N-type.

[0076] The first passivation dielectric layer 140 is disposed on a side surface of the doping layer 130 away from the substrate 110. It can be understood that the first passivation dielectric layer 140 is located in the second region z2 of the first surface m1 of the substrate 110. That is, the doping layer 130 and the first passivation dielectric layer 140 are stacked in sequence on the second region z2 of the first surface m1 of the substrate 110 in a direction away from the second surface m2. The first passivation dielectric layer 140 is used to achieve passivation of the second region z2 of the first surface m1 of the substrate 110. Among them, the material of the first passivation dielectric layer 140 may include a single layer or a stack of one or more of a silicon oxide layer, an aluminum oxide layer, a gallium oxide layer, a titanium oxide layer, a silicon oxynitride layer, an aluminum oxynitride layer, and a silicon carbide layer. When the material of each layer in the multilayer stack is different, the first passivation dielectric layer 140 can be given a good passivation effect through multilayer coordination.

[0077] In the embodiment of the present application, by providing a passivation contact layer 120 in the first region z1 of the first surface m1 of the substrate 110 and providing a doping layer 130 and a first passivation dielectric layer 140 in the second region z2 of the first surface m1 of the substrate 110, on the one hand, since the passivation contact layer 120 includes a tunneling layer 121 and a doped conductive layer 122, the first region z1 can have a better passivation effect, and on the other hand, since the manufacturing steps of the doping layer 130 are simpler than those of the passivation contact layer 120, the first passivation dielectric layer 140 can improve the passivation effect of the second region z2. Therefore, compared with the method of providing the passivation contact layer 120 in both the first region z1 and the second region z2, the manufacturing steps of the solar cell 100 provided in the embodiment of the present application are simpler. Compared with the method of providing the doping layer 130 in both the first region z1 and the second region z2, the solar cell 100 provided in the embodiment of the present application has a better passivation effect. Therefore, the solar cell 100 provided in the embodiment of the present application not only has a certain passivation effect and thus can have a certain efficiency, but also can simplify the process steps and thus can reduce the manufacturing cost.

[0078] In some embodiments, please refer to Figure 1 , the first passivation dielectric layer 140 at least includes a first doped oxide layer 141. That is, when the first passivation dielectric layer 140 is a single-layer structure, the first passivation dielectric layer 140 is a first doped oxide layer 141; when the first passivation dielectric layer 140 is a multi-layer structure, the first passivation dielectric layer 140 includes other passivation dielectric layers capable of passivation in addition to the first doped oxide layer 141. Figure 1 As an example, it is illustrated that the first passivation dielectric layer 140 is a single-layer structure, and the first passivation dielectric layer 140 is the first doped oxide layer 141 .

[0079] The doping element type of the first doped oxide layer 141 may be the same as or different from the doping element type of the doping layer 130. Exemplarily, the doping element type of the first doped oxide layer 141 and the doping element type of the doping layer 130 are both P-type. The oxide in the first doped oxide layer 141 may be silicon oxide. Of course, it may also be other materials, which are not specifically limited here.

[0080] In this way, by setting the first doped oxide layer 141, it can not only be used for passivation, but also can be used to control the diffusion characteristics of the metal paste when forming the corresponding electrode in the second area z2 of the second surface m2 by screen printing the metal paste as shown later, which is beneficial for the corresponding electrode to form contact with the doping layer 130.

[0081] In some embodiments, please refer to Figure 1 The material of the first doped oxide layer 141 includes doped silicon oxide. The doped elements in the first doped oxide layer 141 include P-type doped elements; or the doped elements in the first doped oxide layer 141 include P-type doped elements and N-type doped elements.

[0082] The doping element type of the first doped oxide layer 141 can be set according to the manufacturing method of the first doped oxide layer 141 and the corresponding use requirements.

[0083] Exemplarily, the doping layer 130 and the initial doping oxide layer can be formed by doping boron into the first surface m1 of the substrate 110, and at this time, the material of the initial doping oxide layer is borosilicate glass (BSG). Subsequently, the doping layer 130 and the initial doping oxide layer located in the first region z1 of the first surface m1 of the substrate 110 are removed, and then the passivation contact layer 120 is made. After the doped conductive layer 122 in the passivation contact layer 120 is formed, since the doping element type of the doped conductive layer 122 is an N-type doping element (for example, phosphorus), the initial doping oxide layer is doped with an N-type doping element, forming an intermediate doped oxide layer. For example, the material of the intermediate doped oxide layer may include borosilicate glass and borophosphosilicate glass (BPSG), or may include borophosphosilicate glass. The process of forming the intermediate doped oxide layer can be controlled by the process of forming the doped conductive layer 122. For example, the process of forming the intermediate doped oxide layer can be controlled by controlling relevant parameters such as thickness, density and doping concentration. In the case where the material of the intermediate doped oxide layer includes borosilicate glass and borophosphosilicate glass, the borophosphosilicate glass layer can be removed by a related process (e.g., an etching process) to form the first doped oxide layer 141, or it can be left as is, and the intermediate doped oxide layer at this time can be used as the first doped oxide layer 141. That is, the material of the first doped oxide layer 141 can be borosilicate glass, or borosilicate glass and borophosphosilicate glass, or borophosphosilicate glass. There is no specific limitation here, and the required first doped oxide layer 141 can be set according to the specific usage.

[0084] It can be understood that after the passivation contact layer 120 is formed entirely on the first surface, the side walls of the doped layer 130 and the passivation contact layer 120 on the surface and side walls of the first passivation dielectric layer 140 as well as the layer when the doped conductive layer 122 is formed (for example, the phospho-silicate glass (PSG) layer shown later) can be removed again by patterning technology.

[0085] In this way, the material of the first doped oxide layer 141 can be flexibly selected according to the use requirements. Further, the first doped oxide layer 141 can be formed by doping the first surface m1 of the substrate 110 with a P-type doping element to form the doping layer 130, and the first doped oxide layer 141 can be further formed by the process of making the passivation contact layer 120. In this way, the first doped oxide layer 141 can be formed by the process of forming each layer in the solar cell 100, which further simplifies the process and further reduces the manufacturing cost.

[0086] In addition, in the process of forming the first doped oxide layer 141 by doping the first surface m1 of the substrate 110 with a P-type doping element to form the doping layer 130, in the process of forming the doped conductive layer 122, the first doped oxide layer 141 can block the doping element (for example, phosphorus) used to form the doped conductive layer 122 from entering the doping layer 130. In this way, the influence on the doping layer 130 can be reduced, which is beneficial to the formation of the PN junction of the solar cell 100, thereby improving the cell efficiency.

[0087] It is understood that the first doped oxide layer 141 may also be doped with other P-type doping elements. Alternatively, when the substrate 110 is a P-type substrate, the first doped oxide layer 141 may be formed by utilizing the doping process of the substrate 110 itself. In this case, the passivation of the second region z2 may be achieved by adding a passivation dielectric layer. For example, the material of the passivation dielectric layer may include aluminum oxide and silicon nitride. No specific limitation is made herein.

[0088] In some embodiments, please refer to Figure 1 , the elements doped in the first doped oxide layer 141 include P-type doping elements, and the elements doped in the first doped oxide layer 141 include boron; or, the elements doped in the first doped oxide layer 141 include P-type doping elements and N-type doping elements, and the elements doped in the first doped oxide layer 141 include boron and phosphorus.

[0089] In this way, the P-type doping element and the N-type doping element can be selected according to the usage, and no specific limitation is made here. In the case where the P-type doping element includes boron and / or the N-type doping element includes phosphorus, it can have a certain doping effect and a certain passivation effect at the same time.

[0090] Figure 2 A schematic cross-sectional structure diagram of a solar cell 100 in another embodiment of the present application is shown; for ease of explanation, only the contents related to the embodiment of the present application are shown.

[0091] In some embodiments, please refer to Figure 2 The solar cell 100 further includes a second passivation dielectric layer 150 . The second passivation dielectric layer 150 is disposed on a surface of the doped conductive layer 122 that is away from the tunneling layer 121 .

[0092] It can be understood that the second passivation dielectric layer 150 is located in the first area z1 of the first surface m1 of the substrate 110. That is, the tunneling layer 121, the doped conductive layer 122 and the second passivation dielectric layer 150 are stacked in sequence on the first area z1 of the first surface m1 of the substrate 110 in a direction away from the second surface m2. The second passivation dielectric layer 150 can achieve a certain passivation effect. Among them, the material of the second passivation dielectric layer 150 can include a single layer or a stack of one or more of a silicon oxide layer, an aluminum oxide layer, a gallium oxide layer, a titanium oxide layer, a silicon oxynitride layer, an aluminum oxynitride layer, and a silicon carbide layer. When the material of each layer in the multilayer stack is different, the second passivation dielectric layer 150 can be given a good passivation effect through multilayer coordination.

[0093] Exemplarily, the thickness of the second passivation dielectric layer 150 may be less than or equal to 30 nm. For example, the thickness of the second passivation dielectric layer 150 may be 1 nm, 2 nm, 5 nm, 9 nm, 11 nm, 15 nm, 18 nm, 20 nm, 25 nm, 28 nm or 30 nm. It may be set according to specific usage and is not specifically limited here.

[0094] In this way, by providing the second passivation dielectric layer 150 , it can be used in conjunction with the passivation contact structure to achieve a certain passivation effect.

[0095] In some embodiments, please refer to Figure 2 , the second passivation dielectric layer 150 at least includes a second doped oxide layer 151. That is, when the second passivation dielectric layer 150 is a single-layer structure, the second passivation dielectric layer 150 is a second doped oxide layer 151; when the second passivation dielectric layer 150 is a multi-layer structure, the second passivation dielectric layer 150 includes other passivation dielectric layers capable of passivation in addition to the second doped oxide layer 151. Figure 2 As an example, it is illustrated that the second passivation dielectric layer 150 is a single-layer structure, and the second passivation dielectric layer 150 is a second doped oxide layer 151 .

[0096] The doping element type of the second doped oxide layer 151 may be the same as the doping element type of the doped conductive layer 122. Exemplarily, the doping element type of the second doped oxide layer 151 and the doping element type of the doped conductive layer 122 are both N-type. The oxide in the second doped oxide layer 151 may be silicon oxide. Of course, it may also be other materials, which are not specifically limited here.

[0097] In this way, the second doped oxide layer 151 can be set not only for passivation, but also for controlling the diffusion characteristics of the metal paste when forming the corresponding electrode in the first area z1 of the second surface m2 by screen printing the metal paste as shown later, which is beneficial for the corresponding electrode to form contact with the doped conductive layer 122.

[0098] In some embodiments, please refer to Figure 2 The material of the second doped oxide layer 151 includes doped silicon oxide. The doped element in the second doped oxide layer 151 includes an N-type doping element. Exemplarily, the doped element in the second doped oxide layer 151 includes phosphorus.

[0099] The second doped oxide layer 151 can be provided according to the manufacturing method of the first doped oxide layer 141 and the corresponding use requirements. For example, in the process of forming the doped conductive layer 122 in the passivation contact layer 120, taking the doping element of the doped conductive layer 122 as phosphorus as an example, a phosphosilicate glass (PSG) layer can be formed, that is, the phosphosilicate glass layer can be used as the second doped oxide layer 151 in combination with the relevant processes illustrated in some of the aforementioned embodiments.

[0100] It is understandable that the second doped oxide layer 151 may also be doped with other N-type doping elements, which is not specifically limited herein.

[0101] In this way, the material of the second doped oxide layer 151 can be flexibly selected according to the use requirements. Further, the second doped oxide layer 151 can be formed by the process of forming the doped semiconductor layer. In this way, the second doped oxide layer 151 can be formed by the process of forming each layer in the solar cell 100, which further simplifies the process and further reduces the manufacturing cost. In addition, when the element doped in the second doped oxide layer 151 includes phosphorus, it can have a certain doping effect and a certain passivation effect at the same time.

[0102] In some embodiments, please refer to Figure 2 , the thickness of the first passivation dielectric layer 140 is greater than the thickness of the second passivation dielectric layer 150. That is, the thickness of the first passivation dielectric layer 140 is the first thickness d1, the thickness of the second passivation dielectric layer 150 is the second thickness d2, and the first thickness d1 is greater than the second thickness d2.

[0103] Specifically, with reference to Figure 2, taking the first passivation dielectric layer 140 as the first doped oxide layer 141, the second passivation dielectric layer 150 as the second doped oxide layer 151, the material of the first doped oxide layer 141 is borosilicate glass, and the material of the second doped oxide layer 151 is phosphosilicate glass as an example, in the case of forming the first doped oxide layer 141 by using the process of forming the doped layer 130, the inventors of the present application found that since phosphorus is more likely to replace silicon than boron, the phosphorus element in the corresponding gap is less and the boron element in the corresponding gap is more, so a longer oxidation time can be used during the boron diffusion process to absorb the boron in the corresponding gap, thereby improving the passivation effect of the first doped oxide layer 141. At the same time, the oxidation time for forming the second doped oxide layer 151 can be less than that for the first doped oxide layer 141. In this process, the thickness of the first doped oxide layer 141 formed using a longer oxidation time is greater than the thickness of the second doped oxide layer 151 formed using a shorter oxidation time.

[0104] Thus, on the one hand, by controlling the thickness of the first passivation dielectric layer 140 , the passivation effect can be further improved; on the other hand, by controlling the thickness of the second passivation dielectric layer 150 , the process time can be further saved, the production efficiency can be improved, and the manufacturing cost can be reduced.

[0105] Of course, in some other embodiments, please continue to refer to Figure 1 In the case where the second passivation dielectric layer 150 is formed during the formation of the doped conductive layer 122, the second passivation dielectric layer 150 may also be removed. The configuration may be made according to specific usage conditions and is not specifically limited herein.

[0106] Figure 3 FIG. 4 shows a cross-sectional structural schematic diagram of a solar cell 100 in another embodiment of the present application; Figure 4 FIG. 1 is a schematic cross-sectional view of a solar cell 100 in another embodiment of the present application; for ease of explanation, only the situation related to the embodiment of the present application is shown. Figure 3 The structure shown does not include the second passivation dielectric layer 150. Figure 4 In the structure shown, a second passivation dielectric layer 150 is provided.

[0107] In some embodiments, please refer to Figure 1 and Figure 2 , and combined with reference Figure 3 and Figure 4 The doped layer 130 and the first surface m1 define a separation plane s. Along the first direction F1, the dimension between the side surface of the doped conductive layer 122 away from the substrate 110 and the second surface m2 is a first dimension h1, and the dimension between the separation plane s and the second surface m2 is a second dimension h2. The first dimension h1 is less than or equal to the second dimension h2. Figure 1and Figure 2 As an example, the first size h1 is smaller than the second size h2. Figure 3 and Figure 4 As an example, the situation where the first size h1 is equal to the second size h2 is illustrated.

[0108] Specifically, taking the structure of the second region z2 of the first surface m1 of the substrate 110 as an example, and then the structure of the first region z1 of the first surface m1 of the substrate 110 is manufactured, the manufacturing process illustrated in some of the aforementioned embodiments can be combined with reference to the manufacturing process, in the case where the doping layer 130 and the first passivation dielectric layer 140 are formed by diffusion methods such as boron diffusion, the doping layer 130 is diffused on the first surface m1 toward the second surface m2, and the doping layer 130 has a certain diffusion depth. Subsequently, the first region z1 of the first surface m1 can be processed by a graphic technology (for example, an etching process) to remove the doping layer 130 and the first passivation dielectric layer 140 located in the first region z1. In this process, the first region z1 is recessed relative to the second region z2, and the size of the recess of the first region z1 along the first direction F1 can be approximately several microns. Then, a passivation contact layer 120 is formed in the first region z1, and the thickness of the passivation contact layer 120 is approximately 300nm. In this way, a situation is formed in which the structure height at the second area z2 of the first surface m1 is inconsistent with the structure height at the first area z1 of the first surface m1.

[0109] Thus, by controlling the first dimension h1 to be less than or equal to the second dimension h2, it is convenient to manufacture the passivation contact layer 120, and it is beneficial to form the required passivation contact layer 120 in the first region z1. In addition, when the doping layer 130 is manufactured by diffusion, since the diffusion temperature is higher, the influence on the manufacturing of the doped conductive layer 122 can be reduced by manufacturing the relevant structures on the second region z2 first and then manufacturing the relevant structures on the first region z1.

[0110] In some other practicable ways, in order to better remove the doping layer 130 on the first region z1 of the first surface m1, the etching depth can be controlled, and thus the first region z1 of the first surface m1 can be recessed relative to the second region z2. Of course, the first region z1 and the second region z2 of the first surface m1 can also be flush. That is, the selection and setting can be made according to the various structures on the first surface m1, and no specific limitation is made here.

[0111] In some embodiments, please refer to Figures 1 to 4 , the doping layer 130 includes a doped diffusion layer.

[0112] For example, the first surface m1 of the substrate 110 may be diffused in a diffusion furnace containing a P-type doping element to form a doped diffusion layer, and then patterned to retain only the doped diffusion layer located on the second region z2 of the first surface m1 of the substrate 110. Of course, a mask layer may be provided to cover the first region z1 of the first surface m1, and then the second region z2 of the first surface m1 not covered by the mask layer may be diffused to form doped diffusion portions separated from each other, and all the doped diffusion portions constitute a doped diffusion layer.

[0113] Exemplarily, the doping layer 130 may be a boron diffusion layer, and the diffusion depth of the doping layer 130 is 1µm-3µm. For example, the diffusion depth of the doping layer 130 may be 1µm, 1.2µm, 1.5µm, 2µm, or 3µm. It may be set according to the specific use case and is not specifically limited here.

[0114] In this way, different manufacturing methods can be flexibly selected to form the doped diffusion layer according to the use requirements, and no specific limitation is made here. In the case where the doped layer 130 includes the doped diffusion layer, the process of forming the doped diffusion layer can be used to manufacture the first passivation dielectric layer 140. In the case where the doped diffusion layer located in the second area z2 of the first surface m1 is formed by means of the above-mentioned graphic processing process, it is convenient to manufacture while being conducive to obtaining a doped diffusion layer with better doping effect.

[0115] In some embodiments, please refer to Figures 1 to 4 , the thickness of the first passivation dielectric layer 140 (i.e., the first thickness d1) is less than or equal to 300 nm and greater than or equal to 50 nm. Exemplarily, the first thickness d1 is greater than or equal to 80 nm and less than or equal to 200 nm. For example, the first thickness d1 may be 80 nm, 90 nm, 100 nm, 120 nm, 140 nm, 150 nm, 170 nm, 180 nm, 190 nm, or 200 nm.

[0116] In this way, by controlling the thickness of the first passivation dielectric layer 140 , the manufacturing cost can be reduced while having a certain passivation performance.

[0117] Figure 5 A schematic cross-sectional structure diagram of a solar cell 100 in another embodiment of the present application is shown; Figure 6 FIG. 1 is a schematic cross-sectional view of a solar cell 100 in another embodiment of the present application; for ease of explanation, only the contents related to the embodiment of the present application are shown. Figure 5 The structure shown does not include the second passivation dielectric layer 150. Figure 6 In the structure shown, a second passivation dielectric layer 150 is provided.

[0118] In some embodiments, please refer to Figure 5 and Figure 6 The solar cell 100 further includes a first electrode 170 a located in the first region z1 and in ohmic contact with the doped layer 130 , and a second electrode 170 b located in the second region z2 and in ohmic contact with the doped conductive layer 122 .

[0119] In the embodiment of the present application, the materials of the first electrode 170a and the second electrode 170b include, but are not limited to, one or more of aluminum (Al), titanium (Ti), nickel (Ni), cobalt (Co), silver (Ag), copper (Cu), and tin (Sn). The first electrode 170a and the second electrode 170b may be formed by one of screen printing, laser transfer, and electroplating. In the embodiment of the present application, the first electrode 170a and the second electrode 170b may be understood as metal grid lines, and the width and thickness of the metal grid lines are not limited.

[0120] Exemplarily, the first electrode 170a may be made of silver paste, and the second electrode 170b may be made of silver paste or silver aluminum paste. The width of the first electrode 170a may be 30µm-120µm. For example, the width of the first electrode 170a may be 30µm, 40µm, 50µm, 80µm, 90µm, 100µm, 110µm or 120µm. The width of the second electrode 170b may be 30µm-120µm. For example, the width of the second electrode 170b may be 30µm, 40µm, 50µm, 80µm, 90µm, 100µm, 110µm or 120µm. It can be set according to the specific use case, and is not specifically limited here.

[0121] In this way, by arranging the first electrode 170 a and the second electrode 170 b on the back side of the solar cell 100 , the influence of the front electrode of the solar cell 100 on the light absorption of the cell is significantly reduced, thereby improving the light absorption of the solar cell 100 .

[0122] In some embodiments, please refer to Figures 1 to 6 The solar cell 100 further includes a first anti-reflection layer 160 . The first anti-reflection layer 160 is located on a side of the passivation contact layer 120 away from the substrate 110 , and on a side of the doping layer 130 away from the substrate 110 .

[0123] Exemplarily, the first anti-reflection layer 160 is covered on the surface of the doped conductive layer 122 and the doped layer 130 on one side away from the substrate 110. The first anti-reflection layer 160 can adopt a single-layer structure or a multi-layer structure. In the multi-layer structure of the first anti-reflection layer 160, the material of each layer can be silicon oxide, silicon nitride or silicon oxynitride. The first electrode 170a and the second electrode 170b mentioned above can penetrate the first anti-reflection layer 160 to the corresponding layer, and then form an ohmic contact with the corresponding layer.

[0124] Exemplarily, the first anti-reflection layer 160 may be composed of a two-layer structure, and the materials of the two-layer structure may be aluminum oxide and silicon nitride, or aluminum oxide and silicon oxynitride. The thickness of the first anti-reflection layer 160 may be 60nm-180nm. For example, the thickness of the first anti-reflection layer 160 may be 60nm, 80nm, 100nm, 130nm, 150nm, 160nm, 170nm or 180nm. It can be set according to the specific use case and is not specifically limited here.

[0125] In this way, the first anti-reflection layer 160 is located on the backlight side of the solar cell 100, and has an anti-reflection effect on the back side of the solar cell 100. Optionally, in other embodiments, the first anti-reflection layer 160 may be omitted.

[0126] Figure 7 A schematic cross-sectional structure diagram of a solar cell 100 in another embodiment of the present application is shown; for ease of explanation, only the contents related to the embodiment of the present application are shown.

[0127] In some embodiments, please refer to Figure 7 The solar cell 100 further includes an isolation structure G, which is located between the first region z1 and the second region z2. The isolation structure G may be as follows: Figure 7 The groove shown is formed by a patterned etching process. Of course, the isolation structure G can also be formed by an insulating dielectric layer formed by depositing an insulating dielectric. Exemplarily, the portion of the first surface m1 corresponding to the isolation structure G is constructed as a velvet surface or a polished surface. Figure 7 Shows the condition of the velvet surface.

[0128] The isolation structure G may be located in the first region z1 of the first surface m1 and may penetrate the passivation contact layer 120. The isolation structure G may also be located in the second region z2 of the first surface m1 and may penetrate the doping layer 130 and extend into the substrate 110. The isolation structure G may also be located at a junction spanning the first region z1 and the second region z2.

[0129] In this way, by providing the isolation structure G, structures with different doping types can be isolated from each other.

[0130] In some embodiments, please refer to Figures 1 to 7 The portion of the first surface m1 located in the second area z2 is configured as a polished surface or a velvet surface. Figures 1 to 7 As an example, it is illustrated that the portion of the first surface m1 located in the second area z2 is configured as a polished surface.

[0131] In this way, it can be flexibly set according to usage requirements, and no specific restrictions are made here.

[0132] In some embodiments, please refer to Figures 1 to 7 The solar cell 100 further includes a passivation film layer 180 disposed on the second surface m2 of the substrate 110. The passivation film layer 180 may be a single-layer structure or a multi-layer structure, and the material of the passivation film layer 180 may be at least one of aluminum oxide, silicon oxide, silicon nitride, and silicon oxynitride. The passivation film layer 180. In addition, the passivation film layer 180 may be formed by chemical deposition. The passivation film layer 180 plays a role in surface passivation in the solar cell 100.

[0133] Exemplarily, the passivation film layer 180 may be an oxide layer, and its material may be aluminum oxide. The thickness of the passivation film layer 180 may be less than or equal to 10 nm. For example, the thickness of the passivation final layer 180 may be 1 nm, 3 nm, 6 nm, 8 nm, 9 nm or 10 nm. It may be set according to the specific use case, and is not specifically limited here.

[0134] In some embodiments, please refer to Figures 1 to 7 The solar cell 100 further includes a second anti-reflection layer 190, which is disposed on a surface of the passivation film layer 180 that is away from the substrate 110. The second anti-reflection layer 190 may be a single-layer structure or a multi-layer structure. In the multi-layer structure of the second anti-reflection layer 190, the material of each layer may be silicon oxide, silicon nitride, or silicon oxynitride.

[0135] Exemplarily, the second anti-reflection layer 190 may include a two-layer structure, and the materials of the two-layer structure may be silicon nitride and silicon oxynitride, respectively. The thickness of the second anti-reflection layer 190 may be 60nm-120nm. For example, the thickness of the second anti-reflection layer 190 may be 60nm, 65nm, 70nm, 80nm, 90nm, 100nm or 120nm. It can be set according to the specific use case and is not specifically limited here.

[0136] The following is a specific example to illustrate the method of making a solar cell. Figure 5 , the preparation method comprises the following steps:

[0137] Step S1, providing a substrate 110; the substrate 110 has a first surface m1 and a second surface m2 arranged opposite to each other, the first surface m1 is a backlight surface, the second surface m2 is a light-receiving surface, the first surface m1 of the substrate 110 includes first regions z1 and second regions z2 alternately arranged along a second direction F2, and the substrate 110 is an N-type substrate;

[0138] Step S2, forming an initial doping layer and an initial first passivation dielectric layer in the first surface m1 of the substrate 110 by a boron diffusion process; the doping element of the initial doping layer is boron, and the material of the initial first passivation dielectric layer is BSG;

[0139] Step S3, removing the initial doping layer and the initial first passivation dielectric layer located in the first region z1 of the first surface m1 by a patterning process, and forming the doping layer 130 and the first passivation dielectric layer 140 from the initial doping layer and the initial first passivation dielectric layer located in the second region z2; the first region z1 is recessed relative to the second region z2;

[0140] Step S4, forming an initial tunneling layer, an initial doped conductive layer, and a PSG layer in sequence on the first surface m1 of the substrate 110; the doping element of the initial doped conductive layer is phosphorus;

[0141] Step S5, removing the initial tunneling layer, the initial doped conductive layer and the PSG layer located in the second region z2 and the PSG layer located in the first region z1 by a patterning process, and the initial tunneling layer and the initial doped conductive layer located in the first region z1 form a tunneling layer 121 and a doped conductive layer 122;

[0142] Step S6, forming a first anti-reflection layer 160 on a surface of the first passivation dielectric layer 140 that is away from the doping layer 130 and a surface of the doped conductive layer 122 that is away from the tunneling layer 121;

[0143] Step S7, forming a first electrode 170a in the first region z1 and a second electrode 170b in the second region z2 by a metallization process; the first electrode 170a forms an ohmic contact with the doped conductive layer 122, and the second electrode 170b forms an ohmic contact with the doped layer 130;

[0144] Step S8 , forming a passivation film layer 180 and a second anti-reflection layer 190 stacked in sequence on the second surface m2 of the substrate 110 .

[0145] Another specific example is given below to illustrate the method of making a solar cell. Figure 5 , the preparation method comprises the following steps:

[0146] Step S1, providing a substrate 110; the substrate 110 has a first surface m1 and a second surface m2 arranged opposite to each other, the first surface m1 is a backlight surface, the second surface m2 is a light-receiving surface, the first surface m1 of the substrate 110 includes first regions z1 and second regions z2 alternately arranged along a second direction F2, and the substrate 110 is an N-type substrate;

[0147] Step S2, forming an initial doping layer and an initial first passivation dielectric layer in the first surface m1 of the substrate 110 by a boron diffusion process; the doping element of the initial doping layer is boron, and the material of the initial first passivation dielectric layer is BSG;

[0148] Step S3, removing the initial doping layer and the initial first passivation dielectric layer located in the first region z1 of the first surface m1 by a patterning process, and forming the doping layer 130 and the intermediate first passivation dielectric layer from the initial doping layer and the initial first passivation dielectric layer located in the second region z2; the first region z1 is recessed relative to the second region z2;

[0149] Step S4, forming an initial tunneling layer, an initial doped conductive layer, and a PSG layer in sequence on the first surface m1 of the substrate 110; the doping element of the initial doped conductive layer is phosphorus, and the intermediate first passivation dielectric layer is doped with phosphorus to form a first passivation dielectric layer 140, and the material of the first passivation dielectric layer 140 includes BSG and BPSG;

[0150] Step S5, removing the initial tunneling layer, the initial doped conductive layer and the PSG layer located in the second region z2 and the PSG layer located in the first region z1 by a patterning process, and the initial tunneling layer and the initial doped conductive layer located in the first region z1 form a tunneling layer 121 and a doped conductive layer 122;

[0151] Step S6, forming a first anti-reflection layer 160 on a surface of the first passivation dielectric layer 140 that is away from the doping layer 130 and a surface of the doped conductive layer 122 that is away from the tunneling layer 121;

[0152] Step S7, forming a first electrode 170a in the first region z1 and a second electrode 170b in the second region z2 by a metallization process; the first electrode 170a forms an ohmic contact with the doped conductive layer 122, and the second electrode 170b forms an ohmic contact with the doped layer 130;

[0153] Step S8 , forming a passivation film layer 180 and a second anti-reflection layer 190 stacked in sequence on the second surface m2 of the substrate 110 .

[0154] Thus, the corresponding solar cell can be manufactured by manufacturing the various layer structures in the solar cell illustrated in the above embodiments. It can be understood that the above manufacturing method is only for illustration and other methods can be used for manufacturing, which is not specifically limited here.

[0155] It should be noted that some of the steps or stages illustrated above are not necessarily executed at the same time, but can be executed at different times, and the execution order of these steps or stages is not necessarily sequential, but can be executed in turn or alternately with other steps or at least part of the steps or stages in other steps. It can be selected according to specific usage requirements and is not specifically limited here.

[0156] Figure 8A schematic structural diagram of a photovoltaic assembly in an embodiment of the present application is shown; for ease of explanation, only the contents related to the embodiment of the present application are shown.

[0157] Based on the same invention concept, please refer to Figure 8 , an embodiment of the present application provides a photovoltaic module 10, including a cell string 11, an encapsulation layer 12 and a cover plate 13. The encapsulation layer 12 is used to cover the surface of the cell string 11. The cover plate 13 is used to cover the surface of the encapsulation layer 12 away from the cell string 11. Among them, the cell string 11 is formed by connecting the solar cells in any of the above embodiments. Furthermore, the solar cells are electrically connected in the form of a whole piece or multiple pieces to form a plurality of cell strings 11, and the plurality of cell strings 11 are electrically connected in series and / or in parallel.

[0158] In some embodiments, the plurality of cell strings 11 may be electrically connected via conductive ribbons 14. The encapsulation layer 12 covers the front and back sides of the solar cell.

[0159] In some embodiments, the encapsulation layer 12 may be an organic encapsulation film such as an ethylene-vinyl acetate copolymer (EVA) film, a polyethylene octene copolymer (POE) film, or a polyethylene terephthalate (PET) film.

[0160] In some embodiments, the cover plate 13 may be a glass cover plate, a plastic cover plate or other light-transmitting cover plate.

[0161] In some embodiments, the surface of the cover plate 13 facing the encapsulation layer 12 may be a concave-convex surface, thereby increasing the utilization rate of the incident light.

[0162] The photovoltaic module 10 also has the advantages of the above solar cells, which will not be described in detail here.

[0163] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0164] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A solar cell, characterized in that: include: A substrate having a first surface and a second surface arranged opposite to each other; the first surface of the substrate comprises first areas and second areas alternately arranged along a preset direction; A passivation contact layer is provided in the first region; the passivation contact layer comprises a tunneling layer and a doped conductive layer stacked in the first region of the first surface; a doping layer, disposed in the second region; and The first passivation dielectric layer is disposed on a surface of the doped layer that is away from the substrate.

2. The solar cell according to claim 1, characterized in that The first passivation dielectric layer at least includes a first doped oxide layer.

3. The solar cell according to claim 2, characterized in that: The material of the first doped oxide layer includes doped silicon oxide; Wherein, the doped element in the first doped oxide layer includes a P-type doping element; or The elements doped in the first doped oxide layer include P-type doping elements and N-type doping elements.

4. The solar cell according to claim 3, characterized in that: The element doped in the first doped oxide layer includes a P-type doping element, and the element doped in the first doped oxide layer includes boron; or The elements doped in the first doped oxide layer include a P-type doping element and an N-type doping element, and the elements doped in the first doped oxide layer include boron and phosphorus.

5. The solar cell according to any one of claims 1 to 4, characterized in that: The solar cell further comprises a second passivation dielectric layer; The second passivation dielectric layer is disposed on a surface of the doped conductive layer that is away from the tunneling layer.

6. The solar cell according to claim 5, characterized in that: The thickness of the first passivation dielectric layer is greater than the thickness of the second passivation dielectric layer.

7. The solar cell according to claim 5, characterized in that: The second passivation dielectric layer at least includes a second doped oxide layer.

8. The solar cell according to claim 7, characterized in that: The material of the second doped oxide layer includes doped silicon oxide; Wherein, the doped elements in the second doped oxide layer include N-type doping elements.

9. The solar cell according to any one of claims 1 to 4, characterized in that: The doped layer and the first surface define a separation plane; along the first direction, the dimension between the side surface of the doped conductive layer away from the substrate and the second surface is a first dimension, and the dimension between the separation plane and the second surface is a second dimension; the first dimension is less than or equal to the second dimension; and / or The doping layer comprises a doped diffusion layer; and / or The thickness of the first passivation dielectric layer is less than or equal to 300 nm and greater than or equal to 50 nm.

10. A photovoltaic module, characterized in that: include: Battery string; An encapsulation layer, used to cover the surface of the battery string; and A cover plate, the cover plate is used to cover the surface of the packaging layer away from the battery string; Wherein, the battery string is formed by connecting a plurality of solar cells according to any one of claims 1 to 9.

Citation Information

Cited By

  • Back contact battery piece, photovoltaic module and preparation method of back contact battery piece

    CN120201815A

  • Back contact battery and photovoltaic module

    CN121924839A