Photovoltaic module and preparation process thereof
By using transparent edge sealing tape and photovoltaic waterproof tape for waterproof sealing in photovoltaic modules, the defects of black butyl tape during lamination are solved, achieving more efficient waterproofing and longer service life.
Patent Information
- Application Number
- CN202410816850.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
AI Technical Summary
In existing photovoltaic modules, the black butyl tape easily melts and blocks the cells during lamination, or is squeezed out by the encapsulant, resulting in gaps or channels between the front glass and the back glass, allowing water vapor to enter the laminate. Affects the power generation efficiency and service life of photovoltaic modules.
Use transparent edge sealing glue and/or photovoltaic waterproof tape to waterproof the laminate. Transparent edge sealing glue such as transparent POE film or transparent butyl glue is applied around the cell pack and pasted on the four sides of the laminate. Photovoltaic waterproof tape ensures waterproofing without affecting the view of the cells.
It effectively prevents water vapor from entering the laminated parts, avoids oxidation of the cells, and improves the power generation rate and service life of the photovoltaic modules. At the same time, the transparent edge sealing glue does not block the cells, ensuring the normal power generation efficiency of the photovoltaic modules.
Smart Images

Figure CN118738175A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photovoltaic modules, and in particular to a photovoltaic module and a preparation process of the photovoltaic module. Background Art
[0002] Solar photovoltaic power generation is a technology that uses the semiconductor photovoltaic effect to convert light energy into electrical energy. Using solar energy for photovoltaic power generation is a sustainable and clean energy generation method and one of the effective ways to solve the earth's pollution and energy shortages. Therefore, photovoltaic modules, as the core components of solar power generation, have broad market prospects and huge application value.
[0003] The waterproof sealing of the laminate of photovoltaic modules is one of the important factors that lead to the attenuation of the power generation efficiency of photovoltaic modules. At present, black butyl strips are mostly used on the market to waterproof and seal the laminates to meet the waterproofness of photovoltaic modules. However, this black butyl strip is prone to the following problems when laminating the laminate: 1. After the black butyl adhesive melts, it will penetrate inward and may block the cells, thereby affecting the power generation efficiency of the photovoltaic module; 2. The black butyl adhesive strip will be squeezed out by the packaging adhesive, so that there will be a gap or channel between the front glass and the back glass. Water vapor will enter the laminate through the gap or channel, causing the cells to be invaded or oxidized by water vapor, causing the power generation rate of the photovoltaic module to decay and the service life to be reduced. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a photovoltaic module and a process for preparing the photovoltaic module.
[0005] In order to achieve the above-mentioned object of the invention, a technical solution adopted by the present invention is: to provide a photovoltaic module, including a frame and a laminated member arranged in the frame, wherein the laminated member includes:
[0006] Front glass;
[0007] A rear glass, arranged opposite to the front glass;
[0008] A battery cell group, formed by welding a plurality of battery cells, wherein the battery cell group is arranged between the front glass and the back glass;
[0009] Packaging glue, bonding the battery cell group to the front glass and the back glass respectively, wherein the packaging glue is liquid silicone;
[0010] The photovoltaic assembly further comprises a waterproof edge sealing structure for sealing the gap between the front glass and the back glass, and the waterproof edge sealing structure is a transparent edge sealing adhesive and / or a photovoltaic waterproof tape.
[0011] Furthermore, the material of the liquid silicone comprises divinyl-terminated polydimethylsiloxane, polydimethylsiloxane, hydrogen-containing polysiloxane, an inhibitor, a platinum-containing catalyst and a silane coupling agent.
[0012] Furthermore, the transparent edge sealing adhesive is arranged between the front glass and the back glass and surrounds the four sides of the battery cell group;
[0013] The transparent edge sealing adhesive is made of transparent POE adhesive film or transparent butyl adhesive.
[0014] Furthermore, the photovoltaic waterproof tape is adhered to four side surfaces of the front glass and the back glass.
[0015] The present invention also provides a process for preparing a photovoltaic module, which is used to prepare the above-mentioned photovoltaic module, comprising the following steps:
[0016] Apply liquid silicone to the front glass and back glass surfaces respectively;
[0017] Welding multiple battery cells into a whole to form a battery cell group;
[0018] Placing the cell group on the front glass surface with liquid silicone applied, and then placing the back glass on top of the cell group to form a primary laminate;
[0019] Degassing and laminating the primary laminate to form a laminate;
[0020] Install the laminate inside the frame.
[0021] Furthermore, before placing the back glass on the battery cell group, it also includes applying transparent edge sealing glue on the edge of the front glass surface not covered by the battery cell group, and the transparent edge sealing glue is a transparent POE adhesive film or a transparent butyl adhesive.
[0022] Furthermore, before debubbling and laminating the primary laminate, the method further includes adding transparent butyl adhesive into the gap between the front glass and the back glass by hot injection molding.
[0023] Furthermore, before framing the laminate, the method further includes sticking photovoltaic waterproof tapes on four sides of the laminate.
[0024] Furthermore, in the process of applying liquid silicone to the front glass surface and the back glass surface, bubbles in the liquid silicone applied to the front glass surface and the back glass surface are removed by ultrasonic vibration; or
[0025] After the liquid silicone is applied to the front glass surface and the back glass surface, bubbles in the liquid silicone applied to the front glass surface and the back glass surface are removed by vacuuming and letting the liquid silicone stand.
[0026] Furthermore, the liquid silicone is applied to the front glass and the back glass surfaces by brushing, spraying or scraping.
[0027] The present invention uses transparent edge sealing glue and / or photovoltaic waterproof tape to waterproof the lamination, which can meet the waterproof requirements of photovoltaic modules. Since the edge sealing glue is transparent, it will not block the battery cells even if it melts during lamination. At the same time, photovoltaic waterproof tape is pasted on the four sides of the laminate after lamination, and water vapor cannot enter the laminate, thereby not reducing the power generation rate and service life of the photovoltaic module. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram of the structure of a photovoltaic module in Embodiment 1 of the present invention;
[0029] Figure 2 A cross-sectional view of a laminated member in Example 1 of the present invention with transparent edge-sealing adhesive applied thereto;
[0030] Figure 3 This is an end view of the laminate in Example 1 of the present invention after transparent edge sealing glue is pasted;
[0031] Figure 4 This is an end view of the laminate in Example 1 of the present invention after transparent edge sealing glue is applied and pasted.
[0032] Explanation of symbols:
[0033] 1. Frame; 2. Laminated parts; 21. Front glass; 22. Back glass; 23. Battery cell group; 31. Transparent edge sealing adhesive 31; 32. Photovoltaic waterproof tape 32. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.
[0035] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0036] In the present application, the terms "upper", "lower", "left", "right", "front", "back", "top", "bottom", "inner", "outer", "middle", "vertical", "horizontal", "lateral", "longitudinal" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings. These terms are mainly used to better describe the present application and its embodiments, and are not used to limit the indicated devices, elements or components to have a specific orientation, or to be constructed and operated in a specific orientation.
[0037] In addition, some of the above terms may be used to express other meanings in addition to indicating orientation or positional relationship. For example, the term "on" may also be used to express a certain dependency or connection relationship in some cases. For those of ordinary skill in the art, the specific meanings of these terms in this application can be understood according to specific circumstances.
[0038] In addition, the terms "installed", "set", "provided with", "connected", "connected", and "socketed" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection, or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, elements, or components. For those of ordinary skill in the art, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0039] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0040] Embodiment 1
[0041] Reference Figure 1The present invention provides a photovoltaic module, comprising a frame 1 and a laminate 2 arranged in the frame 1, wherein the laminate 2 comprises a front glass 21 and a back glass 22 arranged opposite to each other, and a cell group 23 arranged between the front glass 21 and the back glass 22, the cell group 23 is formed by welding a plurality of cells, and the cell group 23 is respectively bonded to the front glass 21 and the back glass 22 by a packaging glue, and the packaging glue is liquid silicone. The photovoltaic module also includes a waterproof edge sealing structure for sealing the gap between the front glass 21 and the back glass 22, and the waterproof edge sealing structure is a transparent edge sealing glue 31 and / or a photovoltaic waterproof tape 32.
[0042] The present invention uses transparent edge sealing glue 31 and / or photovoltaic waterproof tape 32 to waterproof and seal the laminate 2, which can meet the waterproof requirements of the photovoltaic module. Since the edge sealing glue 31 is transparent, it will not block the battery cells even if it melts during lamination. At the same time, after lamination, photovoltaic waterproof tape 32 is pasted on the four sides of the laminate 2, and water vapor cannot enter the laminate 2, thereby not reducing the power generation rate and service life of the photovoltaic module.
[0043] Furthermore, the light transmittance of the liquid silicone is 92%-95%, and the materials of the liquid silicone include divinyl-terminated polydimethylsiloxane, polydimethylsiloxane, hydrogen-containing polysiloxane, inhibitor, platinum-containing catalyst and silane coupling agent.
[0044] Furthermore, the mass percentage of polydimethylsiloxane is 80%-85%, the mass percentage of hydrogen-containing polysiloxane is 8-13%, the mass percentage of inhibitor is 2%-5%, the mass percentage of silane coupling agent is 1-2%, and the mass percentage of catalyst is 4ppm-8ppm.
[0045] The viscosity of liquid silicone is an important factor affecting its bonding effect. If the viscosity of liquid silicone is too high, it will lose fluidity, and if the viscosity is too low, it will be easily squeezed out by lamination. The viscosity of liquid silicone can be changed by regulating the different molecular weights of divinyl-terminated polydimethylsiloxane, polydimethylsiloxane and hydrogen-containing polysiloxane, so that the liquid silicone has a good bonding effect. In this embodiment, the molecular weight of divinyl-terminated polydimethylsiloxane is 186-800000, and a combination of high molecular weight vinyl siloxane and low molecular weight vinyl siloxane is used; the molecular weight of polydimethylsiloxane is 162-1000000; the molecular weight of hydrogen-containing polysiloxane is 134-10000.
[0046] Reference Figure 2When the waterproof edge sealing structure is a transparent edge sealing adhesive 31, the transparent edge sealing adhesive 31 is applied between the front glass 21 and the back glass 22 and is arranged around the battery cell group 23. The transparent edge sealing adhesive 31 is used to bond the front glass 21 and the back glass 22 together for waterproof sealing to prevent water vapor from invading the laminate 2 and to prevent the metal parts in the laminate 2 from being oxidized.
[0047] Furthermore, the transparent edge-sealing adhesive 31 may be made of a transparent POE adhesive film or a transparent butyl adhesive. When the POE adhesive film is used to bond and seal the front glass 21 and the back glass 22, since the POE adhesive film is pre-cured, when the laminate 2 is laminated, the POE adhesive film will neither melt in the direction of the battery cell nor be washed out, and the POE adhesive film also has a high water vapor barrier capacity and a high volume resistivity. When the transparent butyl adhesive is used to bond and seal the front glass 21 and the back glass 22, since the butyl adhesive is transparent, when the laminate is laminated, even if the transparent butyl adhesive melts in the direction of the battery cell, the transparent butyl adhesive will not block the battery cell.
[0048] Reference Figure 3 When the waterproof edge sealing structure is a photovoltaic waterproof tape 32 , the photovoltaic waterproof tape 32 is pasted on the four sides of the laminate 2 .
[0049] As a preferred embodiment, the photovoltaic waterproof tape 32 can extend from the side of the laminate 2 to the top surface of the front glass 21 and the bottom surface of the back glass 22, so that the photovoltaic waterproof tape 32 is located between the front glass 21 and the frame 1 and between the glass surface glass 22 and the frame 1, thereby avoiding the frame 1 from pressing directly on the glass and playing a certain pressure buffering role.
[0050] The photovoltaic waterproof tape 32 can be made of butyl waterproof tape, which includes an anti-oxidation coating, metal aluminum foil, precision non-woven fabric and butyl rubber.
[0051] Furthermore, if Figure 2 and Figure 3 As shown, the transparent edge sealing adhesive 31 and the photovoltaic waterproof tape 32 can be used separately. Figure 4 As shown, the transparent edge sealing adhesive 31 and the photovoltaic waterproof tape 32 can also be used in combination.
[0052] Embodiment 2
[0053] The present invention also provides a process for preparing a photovoltaic module, which can be used to prepare the photovoltaic module in implementation one.
[0054] The preparation process of photovoltaic modules includes the following steps:
[0055] Apply liquid silicone to the surface of the front glass 21 and the back glass 22 respectively;
[0056] Welding multiple battery cells into a whole to form a battery cell group 23;
[0057] The battery cell group 23 is placed on the surface of the front glass 21 with liquid silicone applied thereto, and then the back glass 22 is placed on the battery cell group 23 to form a primary laminate;
[0058] Degassing and laminating the primary laminate to form a laminate 2;
[0059] The laminate 2 is mounted in the frame 1 .
[0060] Furthermore, the light transmittance of the liquid silicone is 92%-95%, and the materials of the liquid silicone include divinyl-terminated polydimethylsiloxane, polydimethylsiloxane, hydrogen-containing polysiloxane, inhibitor, platinum-containing catalyst and silane coupling agent.
[0061] Furthermore, the mass percentage of polydimethylsiloxane is 80%-85%, the mass percentage of hydrogen-containing polysiloxane is 8-13%, the mass percentage of inhibitor is 2%-5%, the mass percentage of silane coupling agent is 1-2%, and the mass percentage of catalyst is 4ppm-8ppm.
[0062] The viscosity of liquid silicone is an important factor affecting its bonding effect. If the viscosity of liquid silicone is too high, it will lose fluidity, while if the viscosity is too low, it will be easily squeezed out by lamination. The viscosity of liquid silicone is changed by adjusting the molecular weights of divinyl-terminated polydimethylsiloxane, polydimethylsiloxane and hydrogen-containing polysiloxane. In this embodiment, the molecular weight of divinyl-terminated polydimethylsiloxane is 186-800000, and a combination of high molecular weight vinyl siloxane and low molecular weight vinyl siloxane is used; the molecular weight of polydimethylsiloxane is 162-1000000; the molecular weight of hydrogen-containing polysiloxane is 134-10000.
[0063] Furthermore, the liquid silicone can be applied to the surface of the front glass 21 and the back glass 22 by brushing, spraying or scraping.
[0064] Furthermore, in the process of applying liquid silicone to the surface of the front glass 21 and the surface of the back glass 22, bubbles in the liquid silicone applied to the surface of the front glass 21 and the surface of the back glass 22 are removed by ultrasonic vibration. Alternatively, after applying liquid silicone to the surface of the front glass 21 and the surface of the back glass 22, bubbles in the liquid silicone applied to the surface of the front glass 21 and the surface of the back glass 22 are removed by vacuuming and letting it stand.
[0065] As a preferred embodiment, before placing the back glass 22 on the battery cell group 23, transparent edge sealing glue is applied to the edge of the surface of the front glass 21 not covered by the battery cell group 23, and the transparent edge sealing glue is a transparent POE adhesive film or a transparent butyl adhesive.
[0066] As another preferred embodiment, before debubbling and laminating the primary laminate, transparent butyl adhesive is added into the gap between the front glass 21 and the back glass 22 by hot injection molding.
[0067] Furthermore, the degassing and lamination process of the primary laminate is roughly as follows: the primary laminate is placed in a laminator, the air in the primary laminate is extracted by vacuuming so that there are no bubbles in the primary laminate, and then heated and laminated to combine the back glass 22, the battery cell group 23 and the back glass 22 into a whole, and after lamination, it is taken out and cooled to obtain a laminate 2.
[0068] Preferably, before the laminate 2 is installed in the frame 1 , the process further includes pasting photovoltaic waterproof tapes 32 on four sides of the laminate 2 .
[0069] The photovoltaic waterproof tape 32 can extend from the side of the laminate 2 to the top surface of the front glass 21 and the bottom surface of the back glass 22, so that after the laminate 2 is framed, the photovoltaic waterproof tape 32 can be located between the front glass 21 and the frame 1 and between the glass surface glass 22 and the frame 1, thereby preventing the frame 1 from directly pressing on the glass and playing a certain pressure buffering role.
[0070] The photovoltaic waterproof tape 32 can be made of butyl waterproof tape, which includes an anti-oxidation coating, metal aluminum foil, precision non-woven fabric and butyl rubber.
[0071] Furthermore, before the laminate 2 is installed in the frame 1, an EL test is performed on the laminate 2 to detect the quality of the laminate 2. The EL test is performed by adding current to the laminate 2 and observing whether there is light emission through a photovoltaic EL dedicated camera to detect potential defects or flaws. When the laminate 2 has defects, the laminate 2 is no longer framed.
[0072] Furthermore, after framing, the process also includes installing a junction box.
[0073] Embodiment 3
[0074] The present invention also provides a process for preparing a photovoltaic module, which can be used to prepare the photovoltaic module in implementation one.
[0075] The preparation process of photovoltaic modules includes the following steps:
[0076] Apply liquid silicone to the surface of the front glass 21 and the back glass 22 respectively;
[0077] Welding multiple battery cells into a whole to form a battery cell group 23;
[0078] The battery cell group 23 is placed on the surface of the front glass 21 with liquid silicone applied thereto, and then the back glass 22 is placed on the battery cell group 23 to form a primary laminate;
[0079] Degassing and laminating the primary laminate to form a laminate 2;
[0080] The laminate 2 is mounted in the frame 1 .
[0081] Furthermore, the light transmittance of the liquid silicone is 92%-95%, and the materials of the liquid silicone include divinyl-terminated polydimethylsiloxane, polydimethylsiloxane, hydrogen-containing polysiloxane, inhibitor, platinum-containing catalyst and silane coupling agent.
[0082] Furthermore, the mass percentage of polydimethylsiloxane is 80%-85%, the mass percentage of hydrogen-containing polysiloxane is 8-13%, the mass percentage of inhibitor is 2%-5%, the mass percentage of silane coupling agent is 1-2%, and the mass percentage of catalyst is 4ppm-8ppm.
[0083] The viscosity of liquid silicone is an important factor affecting its bonding effect. If the viscosity of liquid silicone is too high, it will lose fluidity, and if the viscosity is too low, it will be easily squeezed out by lamination. The viscosity of liquid silicone is changed by regulating the molecular weights of divinyl-terminated polydimethylsiloxane, polydimethylsiloxane and hydrogen-containing polysiloxane. In this embodiment, the molecular weight of divinyl-terminated polydimethylsiloxane is 186-800000, and a combination of high molecular weight vinyl siloxane and low molecular weight vinyl siloxane is used; the molecular weight of polydimethylsiloxane is 162-1000000; the molecular weight of hydrogen-containing polysiloxane is 134-10000.
[0084] Furthermore, the liquid silicone can be applied to the surface of the front glass 21 and the back glass 22 by brushing, spraying or scraping.
[0085] Furthermore, in the process of applying liquid silicone to the surface of the front glass 21 and the surface of the back glass 22, bubbles in the liquid silicone applied to the surface of the front glass 21 and the surface of the back glass 22 are removed by ultrasonic vibration. Alternatively, after applying liquid silicone to the surface of the front glass 21 and the surface of the back glass 22, bubbles in the liquid silicone applied to the surface of the front glass 21 and the surface of the back glass 22 are removed by vacuuming and letting it stand.
[0086] Furthermore, before the laminate 2 is framed, the process also includes pasting photovoltaic waterproof tapes 32 on four sides of the laminate 2 .
[0087] The photovoltaic waterproof tape 32 can extend from the side of the laminate 2 to the top surface of the front glass 21 and the bottom surface of the back glass 22, so that after the laminate 2 is framed, the photovoltaic waterproof tape 32 can be located between the front glass 21 and the frame 1 and between the glass surface glass 22 and the frame 1, thereby preventing the frame 1 from directly pressing on the glass and playing a certain pressure buffering role.
[0088] The photovoltaic waterproof tape 32 can be made of butyl waterproof tape, which includes an anti-oxidation coating, metal aluminum foil, precision non-woven fabric and butyl rubber.
[0089] Furthermore, before the laminate 2 is installed in the frame 1, an EL test is performed on the laminate 2 to detect the quality of the laminate 2. The EL test is performed by adding current to the laminate 2 and observing whether there is light emission through a photovoltaic EL dedicated camera to detect potential defects or flaws. When the laminate 2 has defects, the laminate 2 is no longer framed.
[0090] Furthermore, before the laminate 2 is installed in the frame 1, an EL test is performed on the laminate 2 to detect the quality of the laminate 2. The EL test is performed by adding current to the laminate 2 and observing whether there is light emission through a photovoltaic EL dedicated camera to detect potential defects or flaws. When the laminate 2 has defects, the laminate 2 is no longer framed.
[0091] Furthermore, after framing, the process also includes installing a junction box.
[0092] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to the above embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the above embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A photovoltaic module, comprising a frame and a laminated member arranged in the frame, characterized in that: The laminate comprises: Front glass; A rear glass, arranged opposite to the front glass; A battery cell group, formed by welding a plurality of battery cells, wherein the battery cell group is arranged between the front glass and the back glass; Packaging glue, bonding the battery cell group to the front glass and the back glass respectively, wherein the packaging glue is liquid silicone; The photovoltaic assembly further comprises a waterproof edge sealing structure for sealing the gap between the front glass and the back glass, and the waterproof edge sealing structure is a transparent edge sealing adhesive and / or a photovoltaic waterproof tape.
2. The photovoltaic module according to claim 1, characterized in that: The materials of the liquid silicone include divinyl-terminated polydimethylsiloxane, polydimethylsiloxane, hydrogen-containing polysiloxane, an inhibitor, a platinum-containing catalyst and a silane coupling agent.
3. The photovoltaic module according to claim 1 or 2, characterized in that: The transparent edge sealing adhesive is arranged between the front glass and the back glass and surrounds the four sides of the battery cell group; The transparent edge sealing adhesive is made of transparent POE adhesive film or transparent butyl adhesive.
4. The photovoltaic module according to claim 1 or 2, characterized in that: The photovoltaic waterproof tape is adhered to four sides of the laminate.
5. A process for preparing a photovoltaic module, characterized in that: The method for preparing a photovoltaic module according to any one of claims 1 to 4 comprises the following steps: Apply liquid silicone to the front glass and back glass surfaces respectively; Welding multiple battery cells into a whole to form a battery cell group; Placing the cell group on the front glass surface with liquid silicone applied, and then placing the back glass on top of the cell group to form a primary laminate; Degassing and laminating the primary laminate to form a laminate; Install the laminate inside the frame.
6. The process for preparing a photovoltaic module according to claim 5, characterized in that: Before placing the back glass on the battery cell group, it also includes applying transparent edge sealing glue on the edge of the front glass surface not covered by the battery cell group. The transparent edge sealing glue is a transparent POE adhesive film or a transparent butyl adhesive.
7. The process for preparing a photovoltaic module according to claim 5, characterized in that: Prior to debubbling and laminating the primary laminate, transparent butyl adhesive is added into the gap between the front and back glass by hot injection molding.
8. The process for preparing a photovoltaic module according to claim 5, characterized in that: Before framing the laminate, it also includes applying photovoltaic waterproofing tape to the four sides of the laminate.
9. The process for preparing a photovoltaic module according to claim 5, characterized in that: In the process of applying liquid silicone to the front glass surface and the back glass surface, simultaneously using ultrasonic vibration to remove bubbles in the liquid silicone applied to the front glass surface and the back glass surface; or After the liquid silicone is applied to the front glass surface and the back glass surface, bubbles in the liquid silicone applied to the front glass surface and the back glass surface are removed by vacuuming and letting the liquid silicone stand.
10. The process for preparing a photovoltaic module according to claim 5, characterized in that: The liquid silicone is applied to the front glass and the back glass surfaces by brushing, spraying or scraping.
Citation Information
Cited By
Photovoltaic module and manufacturing method
CN119364869A
A method for manufacturing a photovoltaic module
CN119364869B
Photovoltaic module and preparation method thereof
CN119789542A
A photovoltaic module and a method for manufacturing the same
CN119789542B
Photovoltaic module and preparation method thereof
CN120936109A