Negative electrode for solid-state battery, solid-state battery and electric equipment

By using metal active materials as the negative electrode of solid-state batteries and utilizing their volume expansion characteristics to form a tight joint state, the energy density and reliability problems in the existing technology are solved, and solid-state batteries with high energy density and long life are achieved.

CN118738280APending Publication Date: 2024-10-01CHONGQING FUDI BATTERY RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310344212.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The graphite anode of existing solid-state batteries has a low energy density, and the volume expansion of the silicon-based anode during the charge and discharge process causes the material to break, making it difficult to meet the requirements for high energy density and reliability.

Method used

Metal active materials (such as aluminum, magnesium, tin, nickel, etc.) are used as negative electrode active materials, and the volume is expanded by embedding ions to form a tight joint state. Charge transmission is completed by relying on the ionic conductivity and electronic conductance of metal particles, reducing electrolyte materials. Increase the proportion of metal particles in the negative active material layer and reduce the thickness of the negative electrode to increase energy density.

Benefits of technology

A solid-state battery with high energy density and high reliability is achieved, which avoids material fragmentation caused by volume expansion and improves electrochemical performance and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738280A_ABST
    Figure CN118738280A_ABST
Patent Text Reader

Abstract

The invention provides a negative electrode, the negative electrode comprises a negative electrode active material layer, the negative electrode active material layer comprises metal particles and an electrolyte material, the material of the metal particles comprises at least one of aluminum, magnesium, tin, nickel, germanium, phosphorus, silver and lead, and the mass content of the electrolyte material in the negative electrode active material layer is less than 10%. Compared with the prior art, the negative electrode provided by the invention adopts less electrolyte material and mainly depends on the metal particles to complete charge transfer, so that the proportion of the metal particles in the negative electrode active material layer is increased, the thickness of the negative electrode in the solid-state battery is reduced, and the energy density of the solid-state battery is increased. The invention also provides a solid-state battery and electric equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a negative electrode for a solid-state battery, a solid-state battery, and an electrical device. Background Art

[0002] With the continuous development of science and technology, more and more devices need to be equipped with batteries to work, such as watches, mobile phones, computers, electric motorcycles, cars, etc., which puts higher requirements on the energy density of batteries. Solid-state batteries have high energy density in theory, but the energy density of graphite negative electrode materials commonly used in solid-state batteries is low, which is difficult to meet the requirements of high energy density. Although silicon-based negative electrode materials have a high theoretical specific capacity, they will undergo huge volume expansion during the charging and discharging process, resulting in the problem of broken negative electrode materials, affecting the use of batteries. Therefore, it is necessary to develop a battery with high energy density. Summary of the invention

[0003] In view of this, the present application provides a negative electrode for a solid-state battery, a solid-state battery and an electrical device, wherein the negative electrode and the solid-state battery have high energy density and good reliability.

[0004] In a first aspect, the present application provides a negative electrode for a solid-state battery, wherein the negative electrode comprises a negative electrode active material layer, wherein the negative electrode active material layer comprises a metal active material, wherein the material of the metal active material comprises at least one of aluminum, magnesium, tin, nickel, germanium, phosphorus, silver and lead, and the mass content of the solid electrolyte material in the negative electrode active material layer is less than 10%.

[0005] Optionally, the mass content of the electrolyte material in the negative electrode active material layer is 0.

[0006] Optionally, the material of the metal active material includes at least one of aluminum, tin, magnesium and nickel.

[0007] Optionally, before the solid-state battery is cycled for the first time, the metal active material comprises metal particles.

[0008] Furthermore, the average particle size of the metal particles is 0.5 μm-10 μm.

[0009] Optionally, the mass content of the metal active material in the negative electrode active material layer is greater than or equal to 80%.

[0010] Optionally, the negative electrode active material layer further includes a binder.

[0011] Furthermore, the mass content of the binder in the negative electrode active material layer is less than or equal to 10%.

[0012] Optionally, the negative electrode active material layer further includes a conductive agent.

[0013] Furthermore, the mass content of the conductive agent in the negative electrode active material layer is less than or equal to 5%.

[0014] Optionally, the negative electrode further includes a negative electrode current collector, and the negative electrode current collector and the negative electrode active material layer are stacked.

[0015] Furthermore, the material of the negative electrode current collector includes at least one of copper, aluminum, nickel, iron and cobalt, or stainless steel.

[0016] The negative electrode provided by the present application can embed ions during the charging process, so that the volume of the metal active material expands, and the metal active materials are in a tightly bonded state, relying on the ionic conductivity and electronic conductivity of the metal particles after the ions are embedded to complete the charge transfer inside the solid-state battery; at the same time, the negative electrode provided by the present application uses less electrolyte material, and mainly relies on metal particles to complete the charge transfer, which is beneficial to increase the proportion of metal particles in the negative electrode active material layer, reduce the thickness of the negative electrode in the solid-state battery, and further help to improve the energy density of the solid-state battery.

[0017] In a second aspect, the present application provides a solid-state battery, comprising a positive electrode, the negative electrode for the solid-state battery described in the first aspect, and a solid electrolyte layer arranged between the positive electrode and the negative electrode.

[0018] Optionally, the solid-state battery comprises a lithium-ion solid-state battery.

[0019] Furthermore, during the discharge process of the lithium-ion solid-state battery, the mass content of lithium in the negative electrode active material layer is less than 5%.

[0020] Optionally, the solid electrolyte layer includes a solid electrolyte, and the material of the solid electrolyte includes at least one of an inorganic solid electrolyte and an organic solid electrolyte.

[0021] Furthermore, the inorganic solid electrolyte includes at least one of an oxide solid electrolyte, a sulfide solid electrolyte and a selenide solid electrolyte.

[0022] Furthermore, the organic solid electrolyte includes a polymer solid electrolyte.

[0023] The solid-state battery provided in the present application has excellent energy density and high reliability during use, which is conducive to its widespread use.

[0024] In a third aspect, the present application provides an electrical device comprising the solid-state battery described in the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the embodiments or the prior art description. The specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0026] Figure 1 This is an electron microscope image of the solid-state battery provided in Example 1. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0028] The present application provides a negative electrode for a solid-state battery, including a negative electrode active material layer, the negative electrode active material layer including a metal active material, the material of the metal active material including at least one of aluminum, magnesium, tin, nickel, germanium, phosphorus, silver and lead, and the mass content of the electrolyte material in the negative electrode active material layer is less than 10%. When assembled into a battery, the negative electrode is often subjected to the tightening effect from the shell. The negative electrode provided by the present application can embed ions during the charging process, so that the volume of the metal active material expands, and the metal active materials are in a tightly bonded state, and the charge transfer inside the solid-state battery is completed by the ion conductivity and electronic conductivity of the metal active material after the ions are embedded; at the same time, the negative electrode provided by the present application uses less electrolyte material, and mainly relies on the metal active material to complete the charge transfer, which is conducive to increasing the proportion of metal active materials in the negative electrode active material layer, reducing the thickness of the negative electrode in the solid-state battery, and then It is beneficial to improve the energy density of the solid-state battery. The metal active material used in the negative electrode of the present application will expand and pulverize during the charge and discharge process of the liquid battery, thereby continuously consuming the electrolyte, affecting the use of the liquid battery, and thus limiting the use of these metal active materials in the battery; whereas in the present application, the metal active material is used in the negative electrode of the solid-state battery, and the volume expansion performance of the metal active material during the charging process is utilized to realize ion and charge transfer. At the same time, less solid electrolyte material is used in the negative electrode, and the charge transfer is mainly completed by the metal active material, which is beneficial to increase the proportion of the metal active material in the negative electrode active material layer, and further beneficial to improve the energy density of the solid-state battery. In addition, a stable interface can be formed between the solid electrolyte and the negative electrode during the charge and discharge process, and it will not continue to react with the electrolyte after swelling like in the liquid battery, thereby improving the reliability and service life of the solid-state battery.

[0029] In the present application, the mass content of the electrolyte material in the negative electrode active material layer is less than 10%. Specifically, the mass content of the electrolyte material in the negative electrode active material layer may be 0, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8% or 9%, etc. In one embodiment of the present application, the electrolyte material may include at least one of a sulfide solid electrolyte (such as LPSCl, LPS, etc.) and an oxide solid electrolyte (such as LLZO).

[0030] In one embodiment of the present application, the mass content of the electrolyte material in the negative electrode active material layer is 0. In this case, the negative electrode provided by the present application may not contain electrolyte materials, and only rely on the metal active material to generate ion conductivity after embedding ions during the charging process to achieve ion transmission, and the mass proportion of the metal active material in the negative electrode is increased, which is conducive to further improving the energy density of the solid-state battery.

[0031] In the present application, the material of the metal active material includes at least one of aluminum, magnesium, tin, nickel, germanium, phosphorus, silver and lead. The above-mentioned metal active material can embed ions during charging, expand in volume, and has a large specific capacity, which is beneficial to improving the electrochemical performance of solid-state batteries. In one embodiment of the present application, the material of the metal active material includes at least one of aluminum, tin, magnesium and nickel. The above-mentioned metal active material not only has a high specific capacity, but also has both high ionic conductivity and high electronic conductivity after lithium insertion.

[0032] In one embodiment of the present application, the negative electrode active material layer also includes lithium. During the charging process of the lithium-ion solid-state battery, the lithium of the positive electrode is embedded in the negative electrode metal active material. During the discharge process, the lithium embedded in the metal active material cannot be completely removed from the negative electrode, resulting in lithium loss. Therefore, the negative electrode active material layer contains lithium (i.e., pre-embedded lithium) to make up for the loss of lithium and increase the content of lithium during the charging and discharging process, thereby improving the coulombic efficiency of the solid-state battery. In one embodiment of the present application, before the first cycle of the battery, the mass content of lithium in the negative electrode active material layer is less than or equal to 10%. Specifically, the mass content of lithium in the negative electrode active material layer can be, but is not limited to, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc. In one embodiment, the mass content of lithium in the negative electrode active material layer can be 1%-5%. In another embodiment, the mass content of lithium in the negative electrode active material layer can be 5%-10%.

[0033] In one embodiment of the present application, before the first cycle of the solid-state battery, the metal active material includes metal particles. In one embodiment of the present application, before the first cycle of the solid-state battery, the metal active material is composed of metal particles. When the negative electrode of the solid-state battery is charged and lithium is inserted, the metal particles expand and squeeze each other. When the solid-state battery is charged to 100% SOC, the initial metal particle morphology in the negative electrode basically no longer exists, and the metal particles squeeze each other to form a whole; when the solid-state battery is discharged from 100% SOC to less than 100% SOC, the volume of the metal active material shrinks, and under the tightening action of the shell in the direction of the positive electrode-solid electrolyte layer-negative electrode stacking, the negative electrode active material layer still presents an integrated state in the direction of the positive electrode-solid electrolyte layer-negative electrode stacking, but the negative electrode active material layer will have gaps in the direction roughly perpendicular to the positive electrode-solid electrolyte layer-negative electrode stacking. In one embodiment of the present application, the average particle size of the metal particles is 0.5μm-10μm. The use of the above average particle size is conducive to more sufficient contact of the metal particles after charging and embedding ions, and is also conducive to the full embedding of ions by the metal particles, which helps to further improve the energy density of the solid-state battery. Specifically, the average particle size of the metal particles can be, but is not limited to, 0.5μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm or 10μm, etc. In one embodiment of the present application, the average particle size of the metal particles can be 1μm-3μm. In another embodiment of the present application, the average particle size of the metal particles can be 5μm-8μm.

[0034] In one embodiment of the present application, the mass content of the metal active material in the negative electrode active material layer is greater than or equal to 80%. The mass content of the metal active material in the negative electrode active material layer of the present application is high, which can significantly improve the electronic conductivity of the negative electrode and the electrochemical performance of the solid-state battery. Specifically, the mass content of the metal active material in the negative electrode active material layer is greater than or equal to 82%, 85%, 87%, 88%, 90%, 91%, 93%, 95%, 96%, 97% or 98%, etc. In one embodiment of the present application, the mass content of the metal active material in the negative electrode active material layer is 80%-100%. In another embodiment of the present application, the mass content of the metal active material in the negative electrode active material layer is 85%-95%. In another embodiment of the present application, the mass content of the metal active material in the negative electrode active material layer is 86%-92%.

[0035] In one embodiment of the present application, the thickness of the negative electrode active material layer is less than 20μm. This is beneficial to reduce the volume and weight of the solid-state battery, and at the same time can improve the energy density and first coulomb efficiency of the solid-state battery. Specifically, the thickness of the negative electrode active material layer can be but is not limited to 5μm, 7μm, 9μm, 10μm, 13μm, 15μm, 17μm or 18μm, etc. In one embodiment of the present application, the thickness of the negative electrode active material layer is 5μm-10μm. In another embodiment of the present application, the thickness of the negative electrode active material layer is 10μm-15μm.

[0036] In one embodiment of the present application, the negative electrode active material layer may also include at least one of a conductive agent and a binder. Specifically, the conductive agent may include but is not limited to at least one of conductive carbon black, carbon nanotubes, carbon fibers, carbon black and graphite; the binder may include but is not limited to at least one of polytetrafluoroethylene, polyvinylidene fluoride, sodium carboxymethyl cellulose, styrene-butadiene latex, and nitrile rubber. In one embodiment of the present application, the mass content of the conductive agent in the negative electrode active material layer is less than or equal to 5%. Specifically, the mass content of the conductive agent in the negative electrode active material layer may be but is not limited to 0.1%, 0.5%, 1%, 2%, 3%, 4% or 5%, etc. In one embodiment, the mass content of the conductive agent in the negative electrode active material layer may be 0.1%-5%. In another embodiment, the mass content of the conductive agent in the negative electrode active material layer may be 0.5%-3%. In one embodiment of the present application, the mass content of the binder in the negative electrode active material layer is less than or equal to 10%. Specifically, the mass content of the binder in the negative electrode active material layer may be, but is not limited to, 0.1%, 0.5%, 2%, 4%, 5%, 7%, 8% or 9%, etc. In one embodiment, the mass content of the binder in the negative electrode active material layer is 0.1%-10%. In another embodiment, the mass content of the binder in the negative electrode active material layer is 0.5%-5%. In one embodiment of the present application, the mass content of the solid electrolyte material in the negative electrode active material layer is 0. Due to the unstable nature of the solid electrolyte material, it is necessary to use a binder and a conductive agent suitable for the electrolyte material. When the negative electrode active material layer does not contain an electrolyte material, the difficulty of the preparation process of the negative electrode active material layer can be reduced.

[0037] In one embodiment of the present application, the negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector. In one embodiment of the present application, the negative electrode current collector is selected from a metal foil or an alloy foil. Among them, the metal foil includes copper, aluminum, nickel, iron or cobalt foil, and the alloy foil includes an alloy of at least one element of copper, aluminum, nickel, iron and cobalt or stainless steel. In one embodiment of the present application, the material of the negative electrode current collector includes at least one of copper, aluminum, nickel, iron and cobalt or stainless steel. In one embodiment of the present application, at least one of the binder and the conductive agent can be mixed with metal particles in an organic solvent (the mixing time can be but is not limited to 10min-30min) to form a mixed slurry, and the slurry is coated on the surface of the negative electrode current collector, and the negative electrode is obtained after drying. In another embodiment of the present application, at least one of the binder and the conductive agent can be mixed with metal particles and solid electrolyte materials in an organic solvent to form a mixed slurry, and the slurry is coated on the surface of the negative electrode current collector, and the negative electrode is obtained after drying. In another embodiment of the present application, the negative electrode is a negative electrode active material layer, and the negative electrode active material layer plays the role of a negative electrode current collector, which can further improve the energy density and simplify the preparation process of the negative electrode.

[0038] In one embodiment of the present application, the electronic conductivity of the negative electrode is greater than 10 -4 S / cm. The negative electrode provided in the present application has high electronic conductivity, which is beneficial to improving the electrochemical performance of solid-state batteries. In one embodiment of the present application, the mass content of metal particles in the negative electrode active material layer is greater than or equal to 80%, and the electronic conductivity of the negative electrode is greater than 10 -4 In one embodiment of the present application, the specific capacity of the negative electrode is greater than 1000 mAh / g, which is beneficial to improve the energy density of the solid-state battery, reduce the weight and volume of the solid-state battery, and facilitate its use.

[0039] The present application provides a solid-state battery, including a positive electrode, a negative electrode, and a solid electrolyte layer arranged between the positive electrode and the negative electrode in any of the above embodiments. The metal active material used in the negative electrode of the present application has a high specific capacity, and will expand and pulverize during the charging and discharging process of the liquid battery, thereby continuously consuming the electrolyte, affecting the use of the liquid battery, thereby limiting the use of these metal active materials in the battery; and in the present application, the metal active material is used in the negative electrode of the solid-state battery, and the volume expansion performance of the metal active material during the charging process is utilized to realize ion and charge transfer, and at the same time, less electrolyte material is used in the negative electrode, and the charge transfer is mainly completed by the metal active material, which is conducive to increasing the proportion of metal active materials in the negative electrode active material layer, and then It is conducive to improving the energy density of the solid-state battery, and a stable interface can be formed between the solid electrolyte and the negative electrode during the charging and discharging process, and it will not continue to react with the electrolyte after swelling in the liquid battery, thereby improving the reliability and service life of the solid-state battery.

[0040] In one embodiment of the present application, the solid-state battery includes a lithium-ion solid-state battery. Lithium-ion solid-state batteries have the advantages of high voltage, high energy density, excellent cycle performance, etc., and solid-state batteries also avoid the adverse consequences caused by leakage of liquid battery electrolytes, and are safer. The solid-state battery in the present application is an all-solid-state battery; of course, the solid-state battery can also be a sodium-ion solid-state battery, an aluminum-ion solid-state battery, etc. In the present application, the metal particles in the negative electrode do not have ionic conductivity before lithium insertion, and their volume expands after lithium insertion, thereby causing squeezing between the metal particles to achieve ion transmission.

[0041] In one embodiment of the present application, when the SOC (State of charge) of the lithium-ion solid-state battery is 0%, the mass content of lithium in the negative electrode active material layer is less than 5%. Specifically, the mass content of lithium in the negative electrode active material layer may be, but is not limited to, 1%, 2%, 2.5%, 3%, 4% or 4.5%, etc. The negative electrode active material layer provided in the present application has a small lithium content, but still enables the solid battery to achieve high energy density.

[0042] In one embodiment of the present application, the positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on the surface of the positive electrode current collector. In one embodiment of the present application, the positive electrode current collector is independently selected from a metal foil or an alloy foil. Among them, the metal foil includes copper, aluminum, nickel, iron, titanium, nickel, tungsten, gold, silver or cobalt foil, and the alloy foil includes an alloy of at least one element of copper, aluminum, nickel, iron, titanium, nickel, tungsten, gold, silver and cobalt or stainless steel. In one embodiment of the present application, the material of the positive electrode current collector includes at least one of copper, aluminum, nickel, iron, titanium, nickel, tungsten, gold, silver and cobalt or stainless steel. For example, the positive electrode current collector can be aluminum foil.

[0043] In one embodiment of the present application, the positive electrode active material layer includes a positive electrode active material. In one embodiment, the positive electrode active material may include at least one of an oxide type, a polyanion type, and a composite of the above materials. Specifically, the oxide type positive electrode active material may include a chemical formula of Li 1-a A b (Ni m M 1-m )X x O2Z zA material, wherein -0.1≤a≤0.1, A includes one or more of Na, K, Be, Mg, Ca, and B, 0≤b≤0.1, M includes one or more of Mn, Co, and Al, 0<m≤1, X includes one or more of Zr, V, Ti, Cr, Fe, Co, Ni, Zn, Nb, Mo, Os, W, and Y, 0≤x≤0.1, and Z includes one or more of F, Cl, Br, and I, 0≤z≤0.1; specifically, the oxide-type positive electrode active material may include, but is not limited to, LiNi m Co n Mn 1-m-n O2, 0<n<1 (such as LiNi 0.8 Co 0.1 Mn 0.1 O2, etc.), at least one of LiMn2O4, Li2CuO2, LiCoO2 or LiNiO2; the polyanionic positive electrode active material may include at least one of LiFePO4, Li3V2(PO4)3, Li3V3(PO4)3 or LiVPO4F. In one embodiment, the average particle size of the positive electrode active material may be 100nm-200μm. Specifically, the average particle size of the positive electrode active material may be, but is not limited to, 100nm, 500nm, 10μm, 60μm, 90μm, 110μm, 150μm, 175μm or 190μm, etc.

[0044] In one embodiment of the present application, the positive electrode active material layer may also include at least one of a conductive agent, a solid electrolyte material and a binder. Specifically, the conductive agent may include but is not limited to at least one of conductive carbon black, carbon nanotubes, carbon fibers and graphite; the solid electrolyte material may include but is not limited to at least one of a garnet-type solid electrolyte and a sulfur-based solid electrolyte; the binder may include but is not limited to at least one of a fluorine-containing resin, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, polyolefin, styrene-butadiene rubber and butadiene rubber. In one embodiment, the mass content of the conductive agent in the positive electrode active material layer may be 0.005%-10%. Specifically, the mass content of the conductive agent in the positive electrode active material layer may be but is not limited to 0.009%, 0.05%, 0.1%, 0.5%, 3%, 5%, 8% or 10%, etc. In one embodiment, the mass content of the solid electrolyte material in the positive electrode active material layer may be 0.1%-10%. Specifically, the mass content of the solid electrolyte material in the positive electrode active material layer may be, but is not limited to, 0.1%, 0.5%, 2%, 3%, 5%, 7%, 8% or 10%, etc. In one embodiment, the mass content of the binder in the positive electrode active material layer may be 0.01%-20%. Specifically, the mass content of the binder in the positive electrode active material layer may be, but is not limited to, 0.01%, 0.5%, 5%, 10%, 13%, 15%, 16% or 20%, etc.

[0045] In one embodiment of the present application, the solid electrolyte layer includes a solid electrolyte, and the material of the solid electrolyte includes at least one of an inorganic solid electrolyte and an organic solid electrolyte. In one embodiment, the inorganic solid electrolyte includes at least one of an oxide solid electrolyte, a sulfide solid electrolyte, and a selenide solid electrolyte. In one embodiment, the organic solid electrolyte includes a polymer solid electrolyte. Specifically, the sulfide solid electrolyte may include Li3PS4, Li7P3S 11 , Li 10 GeP2S 12 、Li6PS5Cl、Li7P2S8I、Li 10 SnP2S 12 and Li 3.25 Ge 0.25 P 0.75 At least one of S4. Sulfide solid electrolytes have higher ion conductivity than other types of solid electrolytes, which helps to improve the energy density of solid-state batteries. In one embodiment of the present application, the material of the solid electrolyte layer may also include a binder. Specifically, the binder may include but is not limited to at least one of fluorine-containing resin, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, polyolefin, styrene-butadiene rubber, and butadiene rubber.

[0046] In one embodiment of the present application, the first coulombic efficiency of the solid-state battery is greater than 85%, which is conducive to the use of the solid-state battery. Specifically, the first coulombic efficiency of the solid-state battery can be, but is not limited to, greater than 96%, 88%, 90%, 91%, 93% or 95%, etc. In one embodiment of the present application, the energy density of the solid-state battery is greater than 300Wh / kg. The solid-state battery provided in the present application has excellent energy density, which is conducive to the use of solid-state batteries.

[0047] In one embodiment of the present application, a slurry containing a solid electrolyte material can be coated on the surface of the negative electrode or the positive electrode, and then pressed and combined with the positive electrode or the negative electrode to obtain a solid-state battery. In one embodiment, pressing includes hot pressing and isostatic pressing. Specifically, the temperature of the hot pressing treatment may be, but is not limited to, about 100°C, and the hot pressing treatment time may be, but is not limited to, 0.5h-3h; the pressure of the isostatic pressing treatment may be, but is not limited to, above 100MPa, for example, the pressure is 100MPa-600MPa; the time of the isostatic pressing treatment may be, but is not limited to, 3min-10min.

[0048] The present application also provides an electrical device, including the solid-state battery provided in the present application. Specifically, the electrical device may refer to a vehicle, an electronic device, an energy storage system, etc., and the solid-state battery may be provided in the electrical device in the form of a single cell, a battery module, a battery pack, etc.

[0049] The effects of the technical solution of the present application are further illustrated below through specific embodiments.

[0050] Example 1

[0051] Under argon atmosphere, 98.5g of aluminum particles (average particle size of 6μm), 0.5g of conductive agent Super P, and 1g of binder PAA (polyacrylic acid) were added to 54g of xylene, and then stirred in a blender to form a stable and uniform negative electrode slurry. The negative electrode slurry was uniformly and intermittently coated on a copper foil (width 160mm, thickness 16μm), then dried at 373K, and pressed by a roller press to obtain a negative electrode, and the thickness of the negative electrode active material layer was less than 20μm.

[0052] Under an argon atmosphere, 98 g of Li6PS5Cl solid electrolyte material was placed in 167 g of a xylene solution containing 2 g of a butadiene rubber binder, and heated and stirred to obtain a stable and uniform slurry; the slurry was continuously coated on the negative electrode and then dried at 373 K to form a solid electrolyte layer with a thickness of 50 μm on the negative electrode.

[0053] Under an argon atmosphere, 80 g of NCM811 positive electrode active material, 20 g of Li6PS5Cl solid electrolyte material, 2 g of binder butadiene rubber, and 1 g of carbon fiber were added to 43 g of xylene solvent, and then stirred in a vacuum mixer to form a stable and uniform positive electrode mixed slurry; the positive electrode mixed slurry was uniformly and intermittently coated on an aluminum foil (width 160 mm, thickness 16 μm, surface roughness 1 μm), and then dried at 393 K. After being pressed by a roller press, a positive electrode material layer with a thickness of 100 μm was formed on the aluminum foil to obtain a positive electrode.

[0054] Under a protective atmosphere, the above-mentioned positive electrode and the negative electrode with a solid electrolyte layer were aligned and placed in a tablet press, the pole ears were fitted, hot pressed at 100°C for 1 hour, vacuum sealed with an aluminum-plastic film, and finally pressed at 500 MPa for 300 seconds in an isostatic press to obtain a solid-state battery.

[0055] Example 2

[0056] The method is substantially the same as Example 1, except that 93.6 g of aluminum metal particles, 0.5 g of conductive agent Super P, 1 g of binder PAA (polyacrylic acid), and 4.9 g of electrolyte material are added to 54 g of xylene to prepare negative electrode slurry.

[0057] Example 3

[0058] It is substantially the same as Example 1, except that the average particle size of the metal particles is 0.5 μm.

[0059] Example 4

[0060] It is substantially the same as Example 1, except that the average particle size of the metal particles is 20 μm.

[0061] Example 5

[0062] It is substantially the same as Example 1, except that the average particle size of the metal particles is 0.1 μm.

[0063] Example 6

[0064] It is substantially the same as Example 1, except that the negative electrode slurry contains only metal particles.

[0065] Example 7

[0066] It is substantially the same as Example 1, except that the material of the metal particles is an aluminum-lithium alloy, and the lithium content in the aluminum-lithium alloy is 10%.

[0067] Example 8

[0068] It is substantially the same as Example 1, except that the material of the metal particles is tin.

[0069] Example 9

[0070] It is substantially the same as Example 1, except that the material of the metal particles is magnesium.

[0071] Example 10

[0072] It is substantially the same as Example 1, except that the material of the metal particles is nickel.

[0073] Embodiment 11

[0074] It is substantially the same as Example 1, except that the material of the metal particles is lead.

[0075] Comparative Example 1

[0076] The method is substantially the same as Example 1, except that 78.8 g of graphite negative electrode, 0.5 g of conductive agent Super P, 1 g of binder PAA (polyacrylic acid), and 19.7 g of electrolyte material are added to 54 g of xylene to prepare negative electrode slurry.

[0077] Performance Testing

[0078] The electrochemical performance test was conducted on the batteries of each embodiment and the comparative example. The test method is as follows: 20 samples of all-solid-state lithium batteries prepared in each embodiment and comparative example were taken, and each battery was subjected to a charge-discharge cycle test at a rate of 0.1C on a LAND CT 2001C secondary battery performance test device at 298±1K: after being left for 10 minutes, the battery was first charged at a constant voltage to 4.25V / 0.05C (VS Li) and then cut off; after being left for 10 minutes, the battery was discharged at a constant current to 3V, which is one cycle, and the coulombic efficiency and the negative electrode specific capacity Q1 at the completion of the first discharge were recorded. The above steps were repeated at a rate of 0.5C, and the negative electrode specific capacity Q2 at 0.5C was recorded. The ratio of Q2 / Q1 was calculated and recorded as the 0.5C / 0.1C capacity retention rate. The test results are shown in Table 1.

[0079] Table 1 Performance test results

[0080]

[0081]

[0082] It can be seen that compared with the comparative example, the solid-state battery provided in the present application has a high energy density, and the first coulombic efficiency and capacity retention rate can be maintained at a high level, which is conducive to the use of solid-state batteries.

[0083] The solid-state battery (100% SOC) of Example 1 after the electrochemical performance test was disassembled, and the negative electrode and the solid electrolyte layer were detected using a scanning electron microscope. Figure 1 As shown; it can be seen that under the 100% SOC state of the solid-state battery, the initial metal particle morphology of the metal negative electrode after lithium insertion no longer exists, but after the particles expand, the metal particles squeeze each other to form a whole. The metal negative electrode itself has both ionic conductivity and electronic conductivity, and then relies on itself to transmit charge to ensure the use of the solid-state battery.

[0084] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A negative electrode for a solid-state battery, characterized in that: The negative electrode includes a negative electrode active material layer, the negative electrode active material layer includes a metal active material, the material of the metal active material includes at least one of aluminum, magnesium, tin, nickel, germanium, phosphorus, silver and lead, and the mass content of the solid electrolyte material in the negative electrode active material layer is less than 10%.

2. The negative electrode according to claim 1, characterized in that The mass content of the solid electrolyte material in the negative electrode active material layer is 0.

3. The negative electrode according to claim 1, characterized in that The material of the metal active material includes at least one of aluminum, tin, magnesium and nickel.

4. The negative electrode according to claim 1, characterized in that Before the solid-state battery is cycled for the first time, the metal active material includes metal particles.

5. The negative electrode according to claim 4, characterized in that The average particle size of the metal particles is 0.5 μm-10 μm.

6. The negative electrode according to any one of claims 1 to 5, characterized in that The mass content of the metal active material in the negative electrode active material layer is greater than or equal to 80%.

7. The negative electrode according to claim 1, characterized in that The negative electrode active material layer further includes a binder, and the mass content of the binder in the negative electrode active material layer is less than or equal to 10%.

8. The negative electrode according to claim 1, characterized in that The negative electrode active material layer further includes a conductive agent, and the mass content of the conductive agent in the negative electrode active material layer is less than or equal to 5%.

9. The negative electrode according to claim 1, characterized in that The negative electrode further comprises a negative electrode current collector, and the negative electrode current collector and the negative electrode active material layer are stacked; The material of the negative electrode current collector includes at least one of copper, aluminum, nickel, iron and cobalt, or stainless steel.

10. A solid-state battery, characterized in that: The invention comprises a positive electrode, a negative electrode for a solid-state battery according to any one of claims 1 to 9, and a solid electrolyte layer arranged between the positive electrode and the negative electrode.

11. The solid-state battery according to claim 10, characterized in that: The solid-state battery comprises a lithium-ion solid-state battery; When the SOC of the lithium-ion solid-state battery is 0%, the mass content of lithium element in the negative electrode active material layer is less than 5%.

12. The solid-state battery according to claim 10, characterized in that: The solid electrolyte layer includes a solid electrolyte, and the material of the solid electrolyte includes at least one of an inorganic solid electrolyte and an organic solid electrolyte; The inorganic solid electrolyte includes at least one of an oxide solid electrolyte, a sulfide solid electrolyte and a selenide solid electrolyte; The organic solid electrolyte includes a polymer solid electrolyte.