Battery pole piece, battery and electric equipment

By adopting a double-layer active material design in the battery electrodes and using carbon black and graphene of different shapes and sizes to construct an ion and electron transfer network, the problem of low ion diffusion and electron conduction rates in traditional battery electrodes is solved and significantly improved Battery performance.

CN118738282APending Publication Date: 2024-10-01BYD CO LTD +1

Patent Information

Application Number
CN202410652580.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The single-layer coating of traditional battery pole pieces results in low ion diffusion rate away from the current collector and low electron conduction rate close to the current collector, which cannot effectively meet battery performance requirements.

Method used

A double-layer active material design is adopted, in which the first active material layer is close to the current collector and includes carbon black and graphene of different shapes and sizes as conductive agents. The second active material layer is far away from the current collector and also uses carbon black and graphene as conductive agents. , different ion transfer channels and electron transfer networks are constructed through conductive agents of different shapes and sizes.

Benefits of technology

The double-layer design optimizes the transmission efficiency of electrons and ions in the active material layer, improving battery performance, including improving electronic conductivity, ion diffusion rate and battery capacity retention rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738282A_ABST
    Figure CN118738282A_ABST
Patent Text Reader

Abstract

The battery pole piece comprises a current collector, a first active material layer and a second active material layer, the first active material layer is arranged on the current collector, the second active material layer is arranged on one side, opposite to the current collector, of the first active material layer, the first active material layer comprises a first conductive agent, and the second active material layer comprises a second conductive agent. The first active material layer comprises a first conductive agent, the first conductive agent comprises carbon black and / or graphene, the second active material layer comprises a second conductive agent, the second conductive agent comprises carbon black and / or graphene, the first conductive agent has a first shape size, the second conductive agent has a second shape size, and the first shape size is different from the second shape size. Through the arrangement, the conductive agents with different shapes and sizes construct different ion transfer channels and electron transfer networks in the active material layers, so that different ion transfer rates and electron conduction rates are realized in the two active material layers, and the transmission efficiency of electrons and ions in the active material layers can be optimized through the double-layer design; the battery performance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a battery electrode, a battery and an electrical device. Background Art

[0002] The traditional electrode design has only one layer of active material coating, which limits the requirements of the electrode to meet different functional requirements in different environments. The single-layer coating will result in a low ion diffusion rate in the coating far away from the current collector; the electron conduction rate in the coating close to the current collector is low, and the diffusion of ions and the conduction of electrons in the entire electrode cannot be adapted to each other, thus affecting the battery performance. Summary of the invention

[0003] The purpose of the present application is to provide a battery pole piece, a battery and an electrical device to solve the problems of low ion diffusion rate of the coating far from the current collector and low electron conduction rate of the coating close to the current collector in a single-layer coating.

[0004] To achieve the purpose of this application, this application provides the following technical solutions:

[0005] In a first aspect, the present invention provides a battery pole piece, comprising: a current collector, a first active material layer and a second active material layer, wherein the first active material layer is arranged on the current collector, the first active material layer includes a first conductive agent, and the first conductive agent includes carbon black and / or graphene; the second active material layer is arranged on a side of the first active material layer facing away from the current collector, the second active material layer includes a second conductive agent, and the second conductive agent includes carbon black and / or graphene; the first conductive agent has a first shape and size, the second conductive agent has a second shape and size, and the first shape and size are different from the second shape and size.

[0006] In one embodiment, when the first conductive agent and the second conductive agent both include carbon black, the carbon black particle size Dv50 in the first active material layer is smaller than the carbon black particle size Dv50 in the second active material layer; when the first conductive agent and the second conductive agent both include graphene, the flake diameter of the graphene in the first active material layer is larger than the flake diameter of the graphene in the second active material layer.

[0007] In one embodiment, when the first conductive agent includes carbon black, the particle size Dv50 of carbon black in the first active material layer is 6.3nm-14.8nm; when the second conductive agent includes carbon black, the particle size Dv50 of carbon black in the second active material layer is 22nm-111nm; when the first conductive agent includes graphene, the graphene sheet diameter in the first active material layer is 2μm-10μm; when the second conductive agent includes graphene, the graphene sheet diameter in the second active material layer is 0.1μm-1.5μm.

[0008] In one embodiment, the first conductive agent and the second conductive agent further include carbon nanotubes.

[0009] In one embodiment, the aspect ratio of the carbon nanotubes in the first active material layer is greater than the aspect ratio of the carbon nanotubes in the second active material layer.

[0010] In one embodiment, the aspect ratio of the carbon nanotubes in the first active material layer is 500-800; and / or the aspect ratio of the carbon nanotubes in the second active material layer is 200-590.

[0011] In one embodiment, the first active material layer includes first active material particles, and the second active material layer includes second active material particles; a particle size Dv50 of the first active material particles is smaller than a particle size Dv50 of the second active material particles.

[0012] In one embodiment, the particle size Dv50 of the first active material particles is 0.01 μm-0.8 μm; and / or the particle size Dv50 of the second active material particles is 0.7 μm-1.5 μm.

[0013] In a second aspect, the present invention provides a battery, comprising an electrolyte and a battery pole piece as described in any one of the first aspects, wherein the battery pole piece is immersed in the electrolyte.

[0014] In a third aspect, the present invention provides an electrical device, comprising the battery and an electrical device as described in the second aspect, wherein the battery supplies power to the electrical device.

[0015] The present invention provides a battery pole piece, including a current collector, a first active material layer and a second active material layer, wherein the first active material layer is arranged on the current collector, and the second active material layer is arranged on the side of the first active material layer facing away from the current collector, the first active material layer includes a first conductive agent, and the first conductive agent includes carbon black and / or graphene, and the second active material layer includes a second conductive agent, and the second conductive agent includes carbon black and / or graphene, and the first conductive agent has a first shape and size, and the second conductive agent has a second shape and size, and the first shape and size are different from the second shape and size. Through the above arrangement, conductive agents of different shapes and sizes construct different ion transfer channels and electron transfer networks in the active material layer, thereby achieving different ion transfer rates and electron conduction rates in the two active material layers, and the double-layer design can optimize the transmission efficiency of electrons and ions in the active material layer, thereby improving battery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0017] Figure 1 is a schematic diagram of a double-layer active material layer of an embodiment;

[0018] Figure 2 The present invention is a schematic diagram of a method for manufacturing a pole piece according to an embodiment.

[0019] Description of reference numerals:

[0020] 1-first active material layer; 2-second active material layer; 3-current collector. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0022] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there can be a central component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there can be a central component at the same time.

[0023] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in this application and in the specification are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more of the related listed items.

[0024] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0025] Glossary of terms and specific test methods in the present invention:

[0026] Dv50: refers to the volume distribution of granular materials, in which 50% of the particles have a volume less than or equal to the Dv50 value, while the other 50% of the particles have a volume greater than or equal to the Dv50 value.

[0027] Sheet diameter: refers to the width or lateral dimension of sheet material.

[0028] Aspect Ratio: refers to the ratio of the length of a tubular material to its diameter.

[0029] Particle size Dv50 of carbon black: tested by scanning electron microscopy (SEM). The image of carbon black is taken using SEM and the particle size Dv50 of carbon black is measured by image analysis.

[0030] Graphene sheet aspect ratio: The graphene sheet aspect ratio is measured by scanning electron microscopy (SEM) testing, using SEM to take images of graphene and measuring the graphene sheet aspect ratio by image analysis.

[0031] Aspect ratio of carbon nanotubes: The aspect ratio of carbon nanotubes was measured by scanning electron microscopy (SEM). The images of carbon nanotubes were taken using SEM and the aspect ratio of carbon nanotubes was measured by image analysis.

[0032] Particle size Dv50 of active material particles: tested by scanning electron microscopy (SEM), using SEM to take images of active material particles, and measuring the particle size Dv50 of active material particles by image analysis.

[0033] In one embodiment, the present invention provides a battery pole piece, which includes a current collector, a first active material layer and a second active material layer, the first active material layer is arranged on the current collector, the first active material layer includes a first conductive agent, and the first conductive agent includes carbon black and / or graphene; the second active material layer is arranged on the side of the first active material layer facing away from the current collector, the second active material layer includes a second conductive agent, and the second conductive agent includes carbon black and / or graphene; the first conductive agent has a first shape and size, the second conductive agent has a second shape and size, and the first shape and size are different from the second shape and size.

[0034] Please refer to Figure 1, the first active material layer 1 is closer to the current collector 3, and the second active material layer 2 is far away from the current collector 3; the second active material layer 2 mainly plays the role of diffusing lithium ions in the electrolyte in the solid phase active material layer, while the first active material layer 1 needs to enable electrons to be transferred to the current collector 3 more effectively. Different ion transfer channels and electron transfer networks in the active material layer can achieve different ion transfer rates and electron conduction rates in the active material layer; the first shape size of the first conductive agent is different from the second shape size of the second conductive agent, and the shape size can be but not limited to the particle size, aspect ratio and sheet diameter of the conductive agent. Through the different shape sizes of the conductive agent, different ion transfer channels and electron transfer networks are constructed in the first active material layer and the second active material layer, thereby achieving different ion transfer rates and electron conduction rates in the first active material layer and the second active material layer. The double-layer design can optimize the transmission efficiency of electrons and ions in the active material layer and improve battery performance.

[0035] Specifically, the first shape and size of the first conductive agent are different from the second shape and size of the second conductive agent. It can be that when the first conductive agent and the second conductive agent are both carbon black, the shape of the carbon black particles is the same, and the carbon black particle size Dv50 in the first active material layer is smaller than or larger than the carbon black particle size Dv50 in the second active material layer. When the first conductive agent and the second conductive agent are both graphene, the shape of the graphene sheets is the same, and the sheet diameter of the graphene in the first active material layer is larger than or smaller than the sheet diameter of the graphene in the second active material layer. When the first conductive agent is carbon black and the second conductive agent is graphene, there is no comparability between the sizes of different shapes, and it is only necessary that the first shape and size are different from the shape of the second conductive agent. Therefore, it can be understood that the shape and size of the conductive agent shown in the present invention can be the shape of the conductive agent, or the size of the conductive agent, and it cannot be considered that the shape and size of the first conductive agent are different from the shape and size of the second conductive agent.

[0036] Carbon black and / or graphene are added to the first active material layer 1 and the second active material layer 2; carbon black can provide a large number of electron transmission channels due to its high specific surface area; graphene can form a stable conductive network due to its two-dimensional planar structure. These materials can effectively improve the conductivity of the electrode and increase the contact area between the active material and the electrolyte, thereby improving the capacity and energy density of the battery.

[0037] Both carbon black and graphene have high electrical conductivity, but they have different shapes and sizes. Carbon black usually exists in the form of smaller particles, while graphene is a two-dimensional material composed of a single layer or a few layers of carbon atoms. In the active material layer, carbon black and graphene together form a three-dimensional conductive network. Carbon black fills the gaps between graphene layers, increasing the density and continuity of the entire network, while graphene provides highly conductive channels, allowing electrons to be quickly transported throughout the network. The synergistic effect of carbon black and graphene improves the efficiency of electron transmission in the active material layer. The small particles of carbon black can form more contact points with the active material particles, reducing the contact resistance of electron transmission. The high conductivity and large specific surface area of ​​graphene provide more transmission channels for electrons, allowing electrons to move quickly inside the active material and between the current collector. The layered structure of graphene provides a diffusion path for ions, which helps the transmission of ions inside the electrode. The presence of carbon black increases the porosity of the electrode and provides more space for ion migration.

[0038] Carbon nanotubes can also be added to the first active material layer 1 and the second active material layer 2. Carbon nanotubes can serve as bridges to connect carbon black and graphene to form a more complete three-dimensional conductive network. Carbon nanotubes have a high aspect ratio and can span a long distance, thereby improving the connectivity of the entire conductive network and facilitating the rapid transmission of electrons throughout the electrode. The high conductivity and unique tubular structure of carbon nanotubes provide additional transmission paths for electrons, which can shorten the transmission distance of electrons and reduce resistance. At the same time, the presence of carbon nanotubes can further improve the conductivity of the electrode, especially under high-rate charge and discharge conditions. The large specific surface area and tubular structure of carbon nanotubes provide more channels for the diffusion of ions, which facilitates the transmission of ions inside the electrode. In addition, carbon nanotubes can reduce the blockage of pores inside the electrode and maintain the fluidity of the electrolyte, thereby improving the transmission efficiency of ions. The synergistic effect of the three can optimize the charge and discharge performance of the electrode and improve the capacity retention rate and cycle stability of the battery. The presence of carbon nanotubes can provide more active sites and increase the contact area between the electrode and the electrolyte, thereby improving the capacity and energy density of the battery.

[0039] When the materials in the first conductive agent and the second conductive agent are the same. The first conductive agent and the second conductive agent both include carbon black, and carbon black with different particle sizes can provide different ion transfer channels and electron transfer networks, thereby achieving different ion transfer rates and electron conduction rates in the first active material layer and the second active material layer. The first conductive agent and the second conductive agent both include graphene, and graphene with different sheet diameters can provide different ion transfer channels and electron transfer networks, thereby achieving different ion transfer rates and electron conduction rates in the first active material layer and the second active material layer.

[0040] When the materials in the first conductive agent and the second conductive agent are different. The first conductive agent includes carbon black, and the second conductive agent includes graphene. The carbon black in the first conductive agent and the graphene in the second conductive agent provide different ion transfer channels and electron transfer networks due to different shapes, thereby achieving different ion transfer rates and electron conduction rates in the first active material layer and the second active material layer. The first conductive agent includes graphene, and the second conductive agent includes carbon black. The graphene in the first conductive agent and the carbon black in the second conductive agent provide different ion transfer channels and electron transfer networks due to different shapes, thereby achieving different ion transfer rates and electron conduction rates in the first active material layer and the second active material layer.

[0041] The present invention provides a battery pole piece, including a current collector, a first active material layer and a second active material layer, wherein the first active material layer is arranged on the current collector, and the second active material layer is arranged on the side of the first active material layer facing away from the current collector, the first active material layer includes a first conductive agent, and the first conductive agent includes carbon black and / or graphene, and the second active material layer includes a second conductive agent, and the second conductive agent includes carbon black and / or graphene, and the first conductive agent has a first shape and size, and the second conductive agent has a second shape and size, and the first shape and size are different from the second shape and size. Through the above arrangement, conductive agents of different shapes and sizes construct different ion transfer channels and electron transfer networks in the active material layer, thereby achieving different ion transfer rates and electron conduction rates in the two active material layers, and the double-layer design can optimize the transmission efficiency of electrons and ions in the active material layer, thereby improving battery performance.

[0042] In one embodiment, when both the first conductive agent and the second conductive agent include carbon black, the carbon black particle size Dv50 in the first active material layer is smaller than the carbon black particle size Dv50 in the second active material layer.

[0043] The first active material layer 1 needs to have a high electron conduction rate. A smaller carbon black particle size Dv50 has a higher specific surface area and can provide more electron transport channels, thereby enhancing the electron conduction efficiency. A larger carbon black particle size Dv50 in the second active material layer 2 helps to form more ion transport channels, thereby improving the ion diffusion efficiency.

[0044] In one embodiment, the carbon black particle size Dv50 of the first active material layer is 6.3nm-14.8nm; and / or, the carbon black particle size Dv50 of the second active material layer is 22nm-111nm. Optionally, the carbon black particle size Dv50 of the first active material layer can be, but is not limited to, 6.3nm, 7.8nm, 9.3nm, 10.8nm, 12.3nm, 13.8nm, 14.8nm.

[0045] The carbon black particle size Dv50 of the first active material layer is within this range, which can provide a high specific surface area. The unit mass of carbon black has more surfaces available for reaction, which will not cause pores to form inside the pole piece, increase the density of the pole piece, thereby increasing the contact area between the active material and the electrolyte, improving the ion transmission efficiency and the rate of electrochemical reaction; it can form a more effective conductive network. It can improve the electronic conductivity of the electrode, reduce the transmission resistance of electrons inside the electrode, and thus improve the power output of the battery; carbon black particles can provide mechanical support for the active material, prevent the electrode piece from generating stress during the charge and discharge process, enhance the structural stability of the pole piece, and reduce the mechanical stress caused by the volume expansion and contraction of the battery during the charge and discharge process.

[0046] Optionally, the particle size Dv50 of the carbon black of the second active material layer can be, but is not limited to, 22 nm, 33 nm, 44 nm, 55 nm, 66 nm, 77 nm, 88 nm, 99 nm, 100 nm, 111 nm. The reason why the particle size Dv50 of the carbon black of the second active material layer is set within this range is the same as the reason for setting the particle size of the carbon black of the first active material layer, so it is not repeated here.

[0047] In one embodiment, when both the first conductive agent and the second conductive agent include graphene, the sheet diameter of the graphene in the first active material layer is greater than the sheet diameter of the graphene in the second active material layer.

[0048] The use of graphene with a large flake diameter in the first active material layer 1 helps to improve the electron transfer efficiency and mechanical stability, while the use of graphene with a small flake diameter in the second active material layer 2 helps to increase the electrochemical reaction interface area and improve the ion diffusion efficiency.

[0049] In one embodiment, the graphene sheet diameter of the first active material layer is 2 μm-10 μm; and / or, the graphene sheet diameter of the second active material layer is 0.1 μm-1.5 μm. Optionally, the graphene sheet diameter of the first active material layer can be, but is not limited to, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm.

[0050] When the graphene sheet diameter of the first active material layer is within this range, a continuous and efficient conductive network can be formed in the electrode, reducing internal resistance, thereby increasing the electron transmission speed and the overall conductivity of the electrode; providing better mechanical support, increasing the mechanical strength and deformation resistance of the electrode, reducing the volume change of the active material, and improving the long-term cycle stability of the battery; the graphene sheets can form stably arranged connection points inside the electrode, forming a tight conductive network, providing a large number of active sites for electrochemical reactions, and increasing the capacity of the battery.

[0051] Optionally, the graphene sheet diameter of the second active material layer can be, but is not limited to, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm. The reason why the sheet diameter of the graphene of the second active material layer is set within this range is the same as the reason for setting the sheet diameter of the graphene of the first active material layer, so it will not be repeated.

[0052] In one embodiment, the first conductive agent and the second conductive agent further include carbon nanotubes, and the aspect ratio of the carbon nanotubes in the first active material layer is greater than that of the carbon nanotubes in the second active material layer.

[0053] Carbon nanotubes with a larger aspect ratio can form a more effective electron transport network and provide a fast electron conduction path. Therefore, the use of carbon nanotubes with a larger aspect ratio in the first active material layer 1 can enhance the electron transport capacity. Graphene with a larger sheet diameter can form a more continuous and efficient electron transport network, which helps to improve the electron conduction speed and the overall conductivity of the electrode.

[0054] In one embodiment, the aspect ratio of the carbon nanotubes in the first active material layer is 500-800; and / or, the aspect ratio of the carbon nanotubes in the second active material layer is 200-590. Optionally, the aspect ratio of the carbon nanotubes in the first active material layer can be, but is not limited to, 500, 550, 600, 650, 700, 750, 800.

[0055] The aspect ratio of the carbon nanotubes in the first active material layer is within this range, which can provide a longer continuous conductive path, form an efficient conductive network, and facilitate the transmission of electrons in the active material layer; provide support for the electrode material, enhance the mechanical stability of the electrode, reduce the stress caused by volume change during the charge and discharge process, thereby improving the cycle stability of the battery; increase the contact area between the active material and the electrolyte, and increase the number of electrochemical active sites; form a porous structure to enhance the transmission of ions in the electrode; form fewer agglomerates, and improve the uniformity and consistency of the active material.

[0056] Optionally, the aspect ratio of the carbon nanotubes in the second active material layer may be, but is not limited to, 200, 250, 300, 350, 400, 450, 500, 550, or 590. The reason why the aspect ratio of the carbon nanotubes in the second active material layer is set within this range is the same as the reason why the aspect ratio of the carbon nanotubes in the first active material layer is set, so it will not be repeated.

[0057] In one embodiment, the first active material layer includes first active material particles, and the second active material layer includes second active material particles; the particle size Dv50 of the first active material particles is smaller than the particle size Dv50 of the second active material particles.

[0058] The first active material particles and the second active material particles can be lithium iron phosphate active material particles, ternary active material particles, lithium manganate active material particles and lithium cobaltate active material particles; the first active material particles and the second active material particles can also be graphite active material particles and lithium titanate active material particles. The particle size Dv50 of the first active material particles is smaller than the particle size Dv50 of the second active material particles. The contact area between the first active material particles with small particle size increases, which can form a more compact conductive network, reduce the path length of electron transmission, and improve the electronic conductivity. The electronic conductivity of the first active material layer close to the current collector is greater than the electronic conductivity of the second active material layer far away from the current collector; the ability of the current collector side to exchange electrons is improved, the impedance of the battery is reduced, and the battery performance is improved.

[0059] In one embodiment, the particle size Dv50 of the first active material particles is 0.01 μm-0.8 μm; and / or the particle size Dv50 of the second active material particles is 0.7 μm-1.5 μm. Optionally, the particle size Dv50 of the first active material particles can be, but is not limited to, 0.01 μm, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm.

[0060] When the particle size D50 of the first active material particles is within this range, the first active material particles have good dispersibility, prevent agglomeration, and form a uniformly dispersed distribution, so that the electrolyte can better penetrate into the electrode material, forming a more compact conductive network, thereby improving the ion and electron transmission efficiency and improving the battery performance; it can provide a suitable specific surface area, improve the electrochemical reaction rate of the electrode and the capacity of the battery. The carbon nanotubes have a high aspect ratio and can span a long distance, thereby improving the connectivity of the entire conductive network, and through the synergistic effect with the first active material particles, the electrons are quickly transmitted throughout the electrode. Carbon black provides a high specific surface area, and the unit mass of carbon black has more surfaces available for reaction, which increases the contact area between the first active material particles and the electrolyte, thereby improving the ion transmission efficiency and the rate of the electrochemical reaction; it can form a more effective conductive network. The large sheet diameter of graphene can form a continuous and efficient conductive network for the first active material particles in the pole piece, which can improve the transmission speed of electrons and the overall conductivity of the electrode.

[0061] Optionally, the particle size Dv50 of the second active material particles can be, but is not limited to, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm. The reason why the particle size Dv50 of the second active material particles is set within this range is the same as the reason why the particle size Dv50 of the first active material particles is set, so it will not be repeated.

[0062] In one embodiment, the present invention provides a method for manufacturing a battery electrode. Figure 2 , and its preparation method comprises the following steps:

[0063] S1, disposing a first active material layer on a current collector.

[0064] S2, disposing a second active material layer on the first active material layer.

[0065] Specifically, in step S1, the first active material layer includes carbon black and / or graphene. In step S2, the second active material layer includes carbon black and / or graphene. The carbon black and / or graphene in the first active material layer has a first shape and size, and the carbon black and / or graphene in the second active material layer has a second shape and size, and the first shape and size are different from the second shape and size.

[0066] In one embodiment, the present invention provides a battery, comprising an electrolyte and a battery electrode as in any one of the above embodiments, or an electrode electrode prepared by the method for making a battery electrode in any of the above embodiments, wherein the battery electrode is immersed in the electrolyte.

[0067] In this battery, the electrode includes a first active material layer with high electronic conductivity and a second active material layer with high ion conductivity; through layered design, the first active material layer close to the current collector can quickly transmit electrons, and the second active material layer close to the electrolyte can quickly transmit ions; optimize the conduction of electrons and ions, thereby improving battery performance.

[0068] In one embodiment, the present invention provides an electrical device, including a battery and an electrical device as described in the above embodiment, wherein the battery supplies power to the electrical device. The electrical device may be, but is not limited to, an electrical energy storage device, an electric car, a smart phone, and a laptop computer.

[0069] The present application is further described below with reference to embodiments.

[0070] Example 1

[0071] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0072] Among them, the first active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the first active material layer is 7.94nm; the aspect ratio of the carbon nanotubes in the first active material layer is 702; the diameter of the graphene sheet in the first active material layer is 6.3μm. The second active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the second active material layer is 50.5nm, the aspect ratio of the carbon nanotubes in the second active material layer is 320, and the diameter of the graphene sheet in the second active material layer is 0.47μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm, and the particle size Dv50 of the second active material particles is 1.1μm.

[0073] The method for making the positive electrode sheet of this embodiment is as follows:

[0074] (1) The first active material particles, a binder, N-methyl-2-pyrrolidone solvent (NMP) and a conductive agent (carbon black, carbon nanotubes and graphene) are mixed to prepare slurry A.

[0075] (2) The second active material particles, a binder, an N-methyl-2-pyrrolidone solvent (NMP) and a conductive agent (carbon black, carbon nanotubes and graphene) are mixed to prepare slurry B.

[0076] (3) The slurry A obtained in step (1) is coated on an aluminum foil and baked to obtain a first active material layer.

[0077] (4) The slurry B obtained in step (2) is coated on the first active material layer obtained in step (3), and baked to obtain a second active material layer.

[0078] (5) Baking and rolling to prepare the positive electrode sheet.

[0079] Example 2

[0080] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0081] Among them, the first active material layer includes carbon black and graphene; the particle size Dv50 of the carbon black in the first active material layer is 7.94nm; the diameter of the graphene sheet in the first active material layer is 6.3μm. The second active material layer includes carbon black and graphene; the particle size Dv50 of the carbon black in the second active material layer is 50.5nm, and the diameter of the graphene sheet in the second active material layer is 0.47μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm, and the particle size Dv50 of the second active material particles is 1.1μm.

[0082] The difference between Example 2 and Example 1 is that in Example 2, no carbon nanotubes are added.

[0083] The method for manufacturing the positive electrode sheet in Example 2 is the same as that in Example 1.

[0084] Example 3

[0085] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0086] Among them, the first active material layer includes carbon nanotubes and graphene; the aspect ratio of the carbon nanotubes in the first active material layer is 702; the diameter of the graphene sheets in the first active material layer is 6.3μm. The second active material layer includes carbon nanotubes and graphene; the aspect ratio of the carbon nanotubes in the second active material layer is 320, and the diameter of the graphene sheets in the second active material layer is 0.47μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm, and the particle size Dv50 of the second active material particles is 1.1μm.

[0087] The difference between Example 3 and Example 1 is that in Example 3, no carbon black is added.

[0088] The method for manufacturing the positive electrode sheet in Example 3 is the same as that in Example 1.

[0089] Example 4

[0090] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0091] Among them, the first active material layer includes carbon black and carbon nanotubes; the particle size Dv50 of the carbon black in the first active material layer is 7.94nm; the aspect ratio of the carbon nanotubes in the first active material layer is 702. The second active material layer includes carbon black and carbon nanotubes; the particle size Dv50 of the carbon black in the second active material layer is 50.5nm, and the aspect ratio of the carbon nanotubes in the second active material layer is 320. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm, and the particle size Dv50 of the second active material particles is 1.1μm.

[0092] The difference between Example 4 and Example 1 is that no graphene is added in Example 4.

[0093] The method for making the positive electrode sheet in Example 4 is the same as that in Example 1.

[0094] Example 5

[0095] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0096] The first active material layer includes carbon black; the particle size Dv50 of the carbon black in the first active material layer is 7.94 nm. The second active material layer includes carbon black; the particle size Dv50 of the carbon black in the second active material layer is 50.5 nm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38 μm, and the particle size Dv50 of the second active material particles is 1.1 μm.

[0097] The difference between Example 5 and Example 1 is that in Example 5, only carbon black is added.

[0098] The method for making the positive electrode sheet in Example 5 is the same as that in Example 1.

[0099] Example 6

[0100] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0101] The first active material layer includes graphene, and the diameter of the graphene sheet of the first active material layer is 6.3 μm. The second active material layer includes graphene, and the diameter of the graphene sheet of the second active material layer is 0.47 μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38 μm, and the particle size Dv50 of the second active material particles is 1.1 μm.

[0102] The difference between Example 6 and Example 1 is that in Example 6, only graphene is added.

[0103] The method for manufacturing the positive electrode sheet in Example 6 is the same as that in Example 1.

[0104] Example 7

[0105] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0106] Among them, the first active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the first active material layer is 6.3nm; the aspect ratio of the carbon nanotubes in the first active material layer is 702; the diameter of the graphene sheet in the first active material layer is 6.3μm. The second active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the second active material layer is 22nm, the aspect ratio of the carbon nanotubes in the second active material layer is 320, and the diameter of the graphene sheet in the second active material layer is 0.47μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm, and the particle size Dv50 of the second active material particles is 1.1μm.

[0107] The difference between Example 7 and Example 1 is that in Example 7, the particle sizes of carbon black in the first active material layer and the second active material layer are changed.

[0108] The method for making the positive electrode sheet in Example 7 is the same as that in Example 1.

[0109] Example 8

[0110] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0111] Among them, the first active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the first active material layer is 14.8nm; the aspect ratio of the carbon nanotubes in the first active material layer is 702; the diameter of the graphene sheet in the first active material layer is 6.3μm. The second active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the second active material layer is 111nm, the aspect ratio of the carbon nanotubes in the second active material layer is 320, and the diameter of the graphene sheet in the second active material layer is 0.47μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm, and the particle size Dv50 of the second active material particles is 1.1μm.

[0112] The difference between Example 8 and Example 1 is that in Example 8, the particle sizes of carbon black in the first active material layer and the second active material layer are changed.

[0113] The method for making the positive electrode sheet in Example 8 is the same as that in Example 1.

[0114] Example 9

[0115] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0116] Among them, the first active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the first active material layer is 7.94nm; the aspect ratio of the carbon nanotubes in the first active material layer is 702; the diameter of the graphene sheet in the first active material layer is 2μm. The second active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the second active material layer is 50.5nm, the aspect ratio of the carbon nanotubes in the second active material layer is 320, and the diameter of the graphene sheet in the second active material layer is 0.1μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm, and the particle size Dv50 of the second active material particles is 1.1μm.

[0117] The difference between Example 9 and Example 1 is that in Example 9, the diameters of the graphene sheets in the first active material layer and the second active material layer are changed.

[0118] The method for making the positive electrode sheet in Example 9 is the same as that in Example 1.

[0119] Example 10

[0120] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0121] Among them, the first active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the first active material layer is 7.94nm; the aspect ratio of the carbon nanotubes in the first active material layer is 702; the diameter of the graphene sheet in the first active material layer is 10μm. The second active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the second active material layer is 50.5nm, the aspect ratio of the carbon nanotubes in the second active material layer is 320, and the diameter of the graphene sheet in the second active material layer is 1.5μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm, and the particle size Dv50 of the second active material particles is 1.1μm.

[0122] The difference between Example 10 and Example 1 is that in Example 10, the diameters of the graphene sheets in the first active material layer and the second active material layer are changed.

[0123] The method for manufacturing the positive electrode sheet in Example 10 is the same as that in Example 1.

[0124] Embodiment 11

[0125] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0126] Among them, the first active material layer includes carbon black, carbon nanotubes and graphene; the particle size D50 of the carbon black in the first active material layer is 7.94nm; the aspect ratio of the carbon nanotubes in the first active material layer is 500; the diameter of the graphene sheet in the first active material layer is 6.3μm. The second active material layer includes carbon black, carbon nanotubes and graphene; the particle size D50 of the carbon black in the second active material layer is 50.5nm, the aspect ratio of the carbon nanotubes in the second active material layer is 200, and the diameter of the graphene sheet in the second active material layer is 0.47μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size D50 of the first active material particles is 0.38μm, and the particle size D50 of the second active material particles is 1.1μm.

[0127] The difference between Example 11 and Example 1 is that in Example 11, the aspect ratio of the carbon nanotubes in the first active material layer and the second active material layer is changed.

[0128] The method for making the positive electrode sheet in Example 11 is the same as that in Example 1.

[0129] Example 12

[0130] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0131] Among them, the first active material layer includes carbon black, carbon nanotubes and graphene; the particle size D50 of the carbon black in the first active material layer is 7.94nm; the aspect ratio of the carbon nanotubes in the first active material layer is 800; the diameter of the graphene sheet in the first active material layer is 6.3μm. The second active material layer includes carbon black, carbon nanotubes and graphene; the particle size D50 of the carbon black in the second active material layer is 50.5nm, the aspect ratio of the carbon nanotubes in the second active material layer is 590, and the diameter of the graphene sheet in the second active material layer is 0.47μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size D50 of the first active material particles is 0.38μm, and the particle size D50 of the second active material particles is 1.1μm.

[0132] The difference between Example 12 and Example 1 is that in Example 12, the aspect ratio of the carbon nanotubes in the first active material layer and the second active material layer is changed.

[0133] The method for preparing the positive electrode sheet in Example 12 is the same as that in Example 1.

[0134] Embodiment 13

[0135] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0136] Among them, the first active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the first active material layer is 7.94nm; the aspect ratio of the carbon nanotubes in the first active material layer is 702; the diameter of the graphene sheet in the first active material layer is 6.3μm. The second active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the second active material layer is 50.5nm, the aspect ratio of the carbon nanotubes in the second active material layer is 320, and the diameter of the graphene sheet in the second active material layer is 0.47μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.8μm, and the particle size Dv50 of the second active material particles is 1.1μm.

[0137] The difference between Example 13 and Example 1 is that in Example 13, the particle size Dv50 of the first active material particles is changed.

[0138] The method for preparing the positive electrode sheet in Example 13 is the same as that in Example 1.

[0139] Embodiment 14

[0140] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0141] Among them, the first active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the first active material layer is 7.94nm; the aspect ratio of the carbon nanotubes in the first active material layer is 702; the diameter of the graphene sheet in the first active material layer is 6.3μm. The second active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the second active material layer is 50.5nm, the aspect ratio of the carbon nanotubes in the second active material layer is 320, and the diameter of the graphene sheet in the second active material layer is 0.47μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm, and the particle size Dv50 of the second active material particles is 0.7μm.

[0142] The difference between Example 14 and Example 1 is that in Example 14, the particle size Dv50 of the second active material particles is changed.

[0143] The method for preparing the positive electrode sheet in Example 14 is the same as that in Example 1.

[0144] Comparative Example 1

[0145] This embodiment provides a positive electrode sheet, which includes a current collector and a first active material layer; the first active material layer is disposed on the current collector.

[0146] The first active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the first active material layer is 7.94nm; the aspect ratio of the carbon nanotubes in the first active material layer is 702; the diameter of the graphene sheet in the first active material layer is 6.3μm. The first active material particles in the first active material layer are lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm.

[0147] The difference between Comparative Example 1 and Example 1 is that in Comparative Example 1, only a single active material layer is provided.

[0148] The method for preparing the positive electrode sheet in Comparative Example 1 is the same as that in Example 1.

[0149] Comparative Example 2

[0150] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the second active material layer is arranged on the current collector, and the first active material layer is arranged on the second active material layer.

[0151] Among them, the first active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the first active material layer is 7.94nm; the aspect ratio of the carbon nanotubes in the first active material layer is 702; the diameter of the graphene sheet in the first active material layer is 6.3μm. The second active material layer includes carbon black, carbon nanotubes and graphene; the particle size Dv50 of the carbon black in the second active material layer is 7.94nm, the aspect ratio of the carbon nanotubes in the second active material layer is 702, and the diameter of the graphene sheet in the second active material layer is 6.3μm. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38μm, and the particle size Dv50 of the second active material particles is 1.1μm.

[0152] The difference between Comparative Example 2 and Example 1 is that the first shape and size of the first conductive agent in Comparative Example 2 are the same as the second shape and size of the second conductive agent.

[0153] The method for preparing the positive electrode sheet in Comparative Example 2 is the same as that in Example 1.

[0154] Comparative Example 3

[0155] This embodiment provides a positive electrode sheet, which includes a current collector, a first active material layer and a second active material layer; the first active material layer is arranged on the current collector, and the second active material layer is arranged on the first active material layer.

[0156] The first active material layer and the second active material layer are both conductive graphite. The first active material particles in the first active material layer and the second active material particles in the second active material layer are both lithium iron phosphate particles. The particle size Dv50 of the first active material particles is 0.38 μm, and the particle size Dv50 of the second active material particles is 1.1 μm.

[0157] The difference between Comparative Example 3 and Example 1 is that the first active material layer and the second active material layer in Comparative Example 3 do not include any one of carbon black and graphene.

[0158] The method for preparing the positive electrode sheet in Comparative Example 3 is the same as that in Example 1.

[0159] The positive electrode sheets and negative electrode sheets provided in Examples 1-14 and Comparative Examples 1-3 are assembled to form soft-pack batteries, wherein the negative electrode sheets are graphite negative electrode sheets.

[0160] Test method:

[0161] (1) Longitudinal resistivity of the electrode

[0162] The electrode is pressed against the electrode with a uniform and stable pressure in the electrode longitudinal resistivity test instrument, and a constant current is passed through the electrode longitudinally to measure the voltage drop and obtain the resistivity.

[0163] (2) Electrode liquid phase diffusion impedance

[0164] Take the above battery electrodes and electrolyte and assemble them into a battery cell. Set the parameters of the EIS test on the electrochemical workstation. Apply a small amplitude sine wave potential perturbation or current perturbation and measure the response of the battery. Use the collected data to construct Nyquist and Bode plots, and then select or design an equivalent circuit model to fit the experimental data to determine the parameter value of the liquid phase diffusion impedance.

[0165] (3) Mixed material capacity

[0166] The above battery was charged at 0.1C constant current to an upper limit voltage of 4.2V, then charged at constant voltage until the current dropped to 0.03C, left for 5 minutes, and discharged at 0.1C constant current to a lower limit cut-off voltage of 2.0V. The charge and discharge current values ​​were changed to complete the test of 0.2C and 0.5C current values.

[0167] Gram capacity = actual battery capacity / (pole mass - current collector mass)

[0168] (4) DCIR test:

[0169] The battery was discharged at 1 / 3C constant current to 2.0V at room temperature, and charged at 1 / 3C constant current to 50% SOC. It was discharged at 1.5C constant current for 30s at 25℃ and -10℃ respectively, and the voltage before and after discharge was recorded. The discharge DCIR (mΩ) was calculated as (pre-discharge voltage - post-discharge voltage) / discharge current * 1000.

[0170] The results are shown in Table 1.

[0171] Table 1

[0172]

[0173]

[0174] By comparing Examples 1-14 with Comparative Examples 1-3, in Table 1, the electrode longitudinal resistivity, electrode liquid phase diffusion impedance, mixed material gram capacity and DCIR of Examples 1-14 are all better than those of Comparative Examples 1-3. Examples 1-14 are provided with a double-layer active material layer, and the first active material layer has high electronic conductivity, the second active material layer has high ion conductivity, and at least one of carbon black and graphene is added; the carbon black particle size Dv50 in the first active material layer is smaller than the carbon black particle size Dv50 in the second active material layer; the graphene sheet diameter in the first active material layer is larger than the graphene sheet diameter in the second active material layer, which optimizes the ion transport channel and the conductive network in the electrode, thereby improving the performance of the electrode and the battery.

[0175] By comparing Example 1 with Examples 2-6, in Table 1, the electrode longitudinal resistivity, electrode liquid phase diffusion impedance, mixed material gram capacity and DCIR of Example 1 are all better than those of Examples 2-6; Example 1 optimizes the ion transport channels and conductive network in the electrode by adding carbon black, carbon nanotubes and graphene through the combined action of carbon black, carbon nanotubes and graphene, thereby improving the performance.

[0176] By comparing Example 1 with Examples 7-14, in Table 1, the electrode longitudinal resistivity, electrode liquid phase diffusion impedance, mixed material gram capacity and DCIR of Example 1 are all better than those of Examples 7-14; the carbon black particle size Dv50 in the first active material layer of Example 1 is smaller than the carbon black particle size Dv50 in the second active material layer; the aspect ratio of the carbon nanotubes in the first active material layer is greater than the aspect ratio of the carbon nanotubes in the second active material layer; the sheet diameter of the graphene in the first active material layer is greater than the sheet diameter of the graphene in the second active material layer, which optimizes the ion transport channel and the conductive network in the electrode, provides better electron and ion transport performance, and thus improves the performance of the electrode and the battery.

[0177] In the description of the embodiments of the present application, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.

[0178] What is disclosed above is only a preferred embodiment of the present application, and it certainly cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiment and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.

Claims

1. A battery pole piece, characterized in that: include: current collector; A first active material layer, disposed on the current collector, wherein the first active material layer comprises a first conductive agent, and the first conductive agent comprises carbon black and / or graphene; A second active material layer, disposed on a side of the first active material layer facing away from the current collector, the second active material layer comprising a second conductive agent, and the second conductive agent comprising carbon black and / or graphene; The first conductive agent has a first shape and size, and the second conductive agent has a second shape and size, and the first shape and size are different from the second shape and size.

2. The battery electrode according to claim 1, characterized in that: When both the first conductive agent and the second conductive agent include carbon black, the carbon black particle size Dv50 in the first active material layer is smaller than the carbon black particle size Dv50 in the second active material layer; When both the first conductive agent and the second conductive agent include graphene, a sheet diameter of the graphene in the first active material layer is larger than a sheet diameter of the graphene in the second active material layer.

3. The battery pole piece according to claim 1, characterized in that: When the first conductive agent includes carbon black, the carbon black particle size Dv50 in the first active material layer is 6.3 nm-14.8 nm; When the second conductive agent includes carbon black, the particle size Dv50 of the carbon black in the second active material layer is 22 nm-111 nm; When the first conductive agent includes graphene, the diameter of the graphene sheets in the first active material layer is 2 μm-10 μm; When the second conductive agent includes graphene, the diameter of the graphene sheets in the second active material layer is 0.1 μm-1.5 μm.

4. The battery pole piece according to claim 1, characterized in that: The first conductive agent and the second conductive agent further include carbon nanotubes.

5. The battery pole piece according to claim 4, characterized in that: The aspect ratio of the carbon nanotubes in the first active material layer is greater than the aspect ratio of the carbon nanotubes in the second active material layer.

6. The battery pole piece according to claim 4, characterized in that: The aspect ratio of the carbon nanotubes in the first active material layer is 500-800; and / or The aspect ratio of the carbon nanotubes in the second active material layer is 200-590.

7. The battery pole piece according to claim 1, characterized in that: The first active material layer includes first active material particles, and the second active material layer includes second active material particles; a particle size Dv50 of the first active material particles is smaller than a particle size Dv50 of the second active material particles.

8. The battery pole piece according to claim 7, characterized in that: The particle size Dv50 of the first active material particles is 0.01 μm-0.8 μm; and / or The particle size Dv50 of the second active material particles is 0.7 μm to 1.5 μm.

9. A battery, characterized in that: It comprises an electrolyte and a battery pole piece as described in any one of claims 1 to 8, wherein the battery pole piece is immersed in the electrolyte.

10. An electrical device, characterized in that: The invention comprises the battery as claimed in claim 9 and an electrical device, wherein the battery supplies power to the electrical device.

Citation Information

Patent Citations

  • Multilayer coated pole piece, secondary battery, battery module, battery pack, and electric device

    CN115842092A

  • Electrochemical device pole piece, preparation method thereof and electrochemical device

    CN116682933A

  • Lithium battery negative plate as well as preparation method and application thereof

    CN117117079A

  • Positive plate and secondary battery

    CN218004914U

  • Lithium ion secondary battery

    JP2012064537A

Cited By

  • Battery electrode sheet, battery, and electric device

    WO2025241698A1