Negative electrode composite material, preparation method thereof, negative electrode and lithium ion secondary battery

By using negative electrode composite materials in lithium-ion secondary batteries, including silicon oxide, Li2SiO3 and Li2Si2O5 particles and carbon coating layers, combined with specific processing methods, the problem of high residual lithium content in the negative electrode material is solved and the battery performance is improved. Coulombic efficiency and cycle performance.

CN118738306APending Publication Date: 2024-10-01MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310332070.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The residual lithium content of negative electrode materials in existing lithium-ion secondary batteries is too high, making it difficult to improve the processing performance of the slurry and effectively improve the first Coulombic efficiency and cycle performance of lithium-ion secondary batteries.

Method used

A negative electrode composite material is used, which includes negative active material particles and Li2CO3 and LiOH on the surface. The negative active material particles include silicon oxide, Li2SiO3 and Li2Si2O5, and are coated with a carbon coating layer to control the contents of Li2CO3 and LiOH as well as the interaction between Li2Si2O5 and Li2Si2O5. The weight ratio of Li2SiO3, combined with carbon coating treatment, heat treatment and washing treatment to prepare negative electrode composite materials.

Benefits of technology

Effectively reduce the amount of residual lithium, improve the processing performance of the slurry, and improve the first Coulomb efficiency and cycle performance of lithium-ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738306A_ABST
    Figure CN118738306A_ABST
Patent Text Reader

Abstract

The invention provides a negative electrode composite material, a preparation method thereof, a negative electrode and a lithium ion secondary battery. The negative electrode composite material includes negative electrode active material particles, and Li2CO3 and LiOH on the surfaces of the negative electrode active material particles. The negative electrode active material particles include: particles including a silicon oxide, Li2SiO3, and Li2Si2O5; and a carbon coating layer that coats at least a part of the surface of the particles, the content of Li2CO3 being greater than 0.01 wt% and less than 1 wt%, the content of LiOH being greater than 0.001 wt% and less than 0.1 wt%, based on the weight of the negative electrode active material particles, and the weight ratio of Li2Si2O5 to Li2SiO3 being in the range of 1.00 to 10.00. According to the negative electrode composite material, the preparation method thereof, the negative electrode and the lithium ion secondary battery, the amount of residual lithium can be effectively reduced, the processing performance of slurry is improved, and the first coulombic efficiency and the cycle performance of the lithium ion secondary battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium ion secondary batteries, and in particular to a negative electrode composite material, a method for preparing the negative electrode composite material, and a negative electrode and a lithium ion secondary battery comprising the negative electrode composite material. Background Art

[0002] In recent years, with the continuous development of electronic technology, people's demand for battery devices used to support the energy supply of electronic devices has been increasing. Nowadays, batteries that can store more electricity and output high power are needed. Traditional lead-acid batteries and nickel-metal hydride batteries can no longer meet the needs of new electronic products such as mobile devices such as smart phones and fixed equipment such as power storage systems. Therefore, lithium-ion secondary batteries have attracted widespread attention. In the process of developing lithium-ion secondary batteries, their capacity and performance have been effectively improved. Lithium-ion secondary batteries have the advantages of high energy density, high operating voltage, long cycle life, and low environmental pollution. They have become a new green high-energy chemical power source with great development potential in the world today.

[0003] A lithium-ion secondary battery comprises a positive electrode, a negative electrode containing a negative electrode material, and an electrolyte. Various types of negative electrode materials have been developed, among which silicon-based negative electrode materials are one of the more promising negative electrode materials. The prior art discloses the use of pre-lithiation technology to improve the performance of silicon-based negative electrode materials and to control the amount of residual lithium in silicon-based negative electrode materials, but the upper and lower limits of the control of the amount of residual lithium in silicon-based negative electrode materials in the prior art are both relatively high, making it difficult to improve the processing performance of the slurry containing the negative electrode material and to effectively improve the first coulombic efficiency and cycle performance of the lithium-ion secondary battery. Therefore, it is necessary to develop a new negative electrode composite material, a method for preparing the negative electrode composite material, and a negative electrode and a lithium-ion secondary battery containing the negative electrode composite material. Summary of the invention

[0004] The main purpose of the present invention is to provide a negative electrode composite material, a method for preparing the negative electrode composite material, and a negative electrode and a lithium ion secondary battery containing the negative electrode composite material, so as to solve the problems in the prior art that the residual lithium content of the negative electrode material is too high, it is difficult to improve the processing performance of the slurry and it is difficult to effectively improve the first coulombic efficiency and cycle performance of the lithium ion secondary battery.

[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a negative electrode composite material, which includes negative electrode active material particles and Li2CO3 and LiOH on the surface of the negative electrode active material particles, the negative electrode active material particles include: particles containing silicon oxide, Li2SiO3 and Li2Si2O5; and a carbon coating layer coating at least a portion of the surface of the particles, based on the weight of the negative electrode active material particles, the content of Li2CO3 is greater than 0.01wt% and less than 1wt%, the content of LiOH is greater than 0.001wt% and less than 0.1wt%, and the weight ratio of Li2Si2O5 to Li2SiO3 is Li2Si2O5 / Li2SiO3 in the range of 1.00 to 10.00.

[0006] Furthermore, in the above negative electrode composite material, the content of Li2SiO3 is greater than 1.0 wt% and less than 48.0 wt% based on the weight of the negative electrode active material particles.

[0007] Furthermore, in the above negative electrode composite material, Li2SiO3 is distributed in the particle in a gradually decreasing trend from a position close to the surface of the particle toward the center of the particle, and Li2Si2O5 is distributed at a position closer to the center of the particle than Li2SiO3.

[0008] Furthermore, in the above negative electrode composite material, the carbon coating layer covers the entire surface of the particles.

[0009] Furthermore, in the above-mentioned negative electrode composite material, the silicon oxide is SiO x , where 0.5≤x≤1.6.

[0010] Furthermore, in the above negative electrode composite material, the silicon in the silicon oxide exists in the form of crystalline silicon, and the size of the crystalline silicon is in the range of 5.0 nm to 12.0 nm.

[0011] Furthermore, in the above negative electrode composite material, the intensity ratio of the D peak to the G peak in the Raman spectrum of the negative electrode composite material is D / I G Greater than 0.8 and less than 2.0, preferably, greater than 1.5 and less than 1.8.

[0012] Further, in the above negative electrode composite material, the coating amount of the carbon coating layer is in the range of 1 wt % to 30 wt % based on the weight of the negative electrode active material particles.

[0013] According to another aspect of the present invention, a method for preparing a negative electrode composite material is provided, the method comprising: carbon-coating a silicon oxide precursor with a carbon source to form a carbon-coated silicon oxide; mixing the carbon-coated silicon oxide with a lithium source to form a first mixture, performing a first heat treatment on the first mixture to form a calcined product, and then performing a second heat treatment on the calcined product to form a pre-lithium product; and washing the pre-lithium product to form a negative electrode composite material.

[0014] Furthermore, in the above-mentioned method for preparing a negative electrode composite material, the washing treatment includes mixing the pre-lithium product with water, alcohol or acid, preferably with a solid content of 5wt%-20wt% to form a second mixture, ultrasonically treating the second mixture, then dispersing it, followed by filtering it, and finally drying the filtered material.

[0015] Furthermore, in the above method for preparing a negative electrode composite material, the acid is selected from at least one of hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid and boric acid.

[0016] Further, in the above method for preparing a negative electrode composite material, a weight ratio of the lithium source to the carbon-coated silicon oxide is in the range of 5:95 to 40:60.

[0017] Further, in the above method for preparing a negative electrode composite material, the temperature for the first heat treatment is in the range of 400° C.-750° C., and the time for the first heat treatment is in the range of 1 h-5 h.

[0018] Further, in the above method for preparing a negative electrode composite material, the temperature of the second heat treatment is in the range of greater than or equal to 800° C. and less than 925° C., and the time of the second heat treatment is in the range of 1 h-6 h.

[0019] Furthermore, in the above method for preparing a negative electrode composite material, the ultrasonic treatment is performed for a time in the range of 1 min to 30 min.

[0020] Furthermore, in the above method for preparing a negative electrode composite material, the dispersion time is in the range of 8h-48h.

[0021] Furthermore, in the above method for preparing a negative electrode composite material, the carbon source includes at least one of alkanes, alkenes and alkynes.

[0022] Furthermore, in the above method for preparing a negative electrode composite material, the alcohol is selected from at least one of ethanol, isopropanol and butanol.

[0023] According to another aspect of the present invention, a negative electrode for a lithium ion secondary battery is provided. The negative electrode for a lithium ion secondary battery comprises the negative electrode composite material described above.

[0024] According to another aspect of the present invention, a lithium ion secondary battery is provided. The lithium ion secondary battery includes: a positive electrode, a negative electrode, and a separator. The negative electrode includes the negative electrode composite material described above.

[0025] The negative electrode composite material, the method for preparing the negative electrode composite material, and the negative electrode and lithium ion secondary battery containing the negative electrode composite material of the present invention can effectively reduce the amount of residual lithium, improve the processing performance of the slurry, and improve the first coulombic efficiency and cycle performance of the lithium ion secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A schematic structural diagram of a negative electrode composite material according to one embodiment of the present invention is shown.

[0027] Figure 2 A graph showing the relationship between the size of crystalline silicon in the negative electrode composite materials and the weight ratio of Li2Si2O5 to Li2SiO3 (Li2Si2O5 / Li2SiO3) of Examples 1-10 and Comparative Examples 1-3, 5, 7 and 9 is shown, wherein the ordinate is the size of crystalline silicon in the negative electrode composite materials and the abscissa is the weight ratio of Li2Si2O5 to Li2SiO3 (Li2Si2O5 / Li2SiO3).

[0028] Figure 3 The discharge capacity retention rate (%) after 50 cycles of Examples 1-8 and Comparative Examples 1, 3, 4, 6, 8 and 9 and the intensity ratio of the D peak to the G peak in the Raman spectrum of the negative electrode composite material are shown. D / I G , wherein the ordinate is the discharge capacity retention rate (%) after 50 cycles, and the abscissa is the intensity ratio of the D peak to the G peak in the Raman spectrum of the negative electrode composite material. D / I G .

[0029] Figure 4 The Li 1s XPS (X-ray photoelectron spectroscopy) spectra of Example 2 at different etching depths are shown.

[0030] Figure 5 The Li 1s XPS (X-ray photoelectron spectroscopy) spectra of Comparative Example 1 at different etching depths are shown. DETAILED DESCRIPTION

[0031] It should be noted that, in the absence of conflict, the various embodiments and features in the embodiments in this application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments. The following embodiments are merely exemplary and are not intended to limit the scope of protection of the present invention.

[0032] As described in the background art, in the prior art, the residual lithium content of the negative electrode material is too high, it is difficult to improve the processing performance of the slurry containing the negative electrode material and it is difficult to effectively improve the first coulombic efficiency and cycle performance of the lithium ion secondary battery. In view of the problems in the prior art, a typical embodiment of the present invention provides a negative electrode composite material, the negative electrode composite material includes negative electrode active material particles and Li2CO3 and LiOH on the surface of the negative electrode active material particles, the negative electrode active material particles include: particles containing silicon oxide, Li2SiO3 and Li2Si2O5; and a carbon coating layer covering at least a portion of the surface of the particles, based on the weight of the negative electrode active material particles, the content of Li2CO3 is greater than 0.01wt% and less than 1wt%, the content of LiOH is greater than 0.001wt% and less than 0.1wt%, and the weight ratio of Li2Si2O5 to Li2SiO3 is Li2Si2O5 / Li2SiO3 in the range of 1.00 to 10.00.

[0033] A higher residual lithium value will affect the processing performance of the slurry containing the negative electrode composite material, resulting in the slurry being easily "jelly" in the process of preparing the slurry using the negative electrode composite material. In the prior art, it is not realized that the distribution of lithium-containing compounds and the weight ratio of Li2Si2O5 to Li2SiO3 Li2Si2O5 / Li2SiO3 on the control of residual lithium. After conducting a large number of experiments, the inventors of the present invention unexpectedly found that by designing the distribution of lithium-containing compounds in the negative electrode composite material and by regulating the weight ratio of Li2Si2O5 to Li2SiO3 Li2Si2O5 / Li2SiO3, not only the size of crystalline silicon can be regulated, but also the control and optimization of residual lithium can be facilitated, the amount of residual lithium can be effectively reduced, and the slurry can be prevented from "jellying" in the process of preparing the slurry using the negative electrode composite material, the processing performance of the slurry can be improved, and the first coulomb efficiency and cycle performance of the lithium ion secondary battery can be improved. Therefore, the negative electrode composite material of the present invention has a significantly reduced amount of residual lithium, can improve the processing performance of the slurry, and can improve the first coulomb efficiency and cycle performance of the lithium ion secondary battery.

[0034] In some embodiments of the present invention, in the negative electrode composite material of the present invention, the content of Li2SiO3 is greater than 1.0wt% and less than 48.0wt% based on the weight of the negative electrode active material particles. The control of the amount of water-soluble Li2SiO3 in the prior art is not clear, and there is no in-depth study on the effect of the amount of water-soluble Li2SiO3 on the electrochemical performance. The inventors of the present invention unexpectedly found that by controlling the content of Li2SiO3 within the above range, it is possible to ensure that a fully pre-lithium negative electrode composite material is obtained, and the first coulombic efficiency and cycle performance of the lithium ion secondary battery can be improved.

[0035] In some embodiments of the present invention, in the negative electrode composite material of the present invention, Li2SiO3 is distributed in a gradually decreasing trend from a position close to the surface of the particle to the center of the particle, and Li2Si2O5 is distributed at a position closer to the center of the particle than Li2SiO3. The distribution of the water-soluble Li2SiO3 and the water-insoluble Li2Si2O5 in the negative electrode composite material is conducive to the control and optimization of residual lithium, can effectively reduce the amount of residual lithium, improve the processing performance of the slurry, and improve the first coulomb efficiency and cycle performance of the lithium-ion secondary battery. Figure 1 A schematic structural diagram of a negative electrode composite material according to one embodiment of the present invention is shown.

[0036] In some embodiments of the present invention, in the negative electrode composite material of the present invention, the carbon coating layer can cover the entire surface of the particles, thereby improving the conductivity of the negative electrode composite material, improving the first coulombic efficiency, more effectively reducing the amount of residual lithium, and improving the processing performance of the slurry.

[0037] The silicon oxide of the present application may be silicon oxide conventionally used for negative electrode materials in the art. In some embodiments of the present invention, in the negative electrode composite material of the present invention, the silicon oxide may be SiO x , wherein 0.5≤x≤1.6, preferably 0.8≤x≤1.2, most preferably, x=1.0.

[0038] In some embodiments of the present invention, in the negative electrode composite material of the present invention, the silicon in the silicon oxide exists in the form of crystalline silicon, and the size of the crystalline silicon is in the range of 5.0nm to 12.0nm, preferably, the size of the crystalline silicon is in the range of 5.0nm to 11.5nm. By controlling the size of the crystalline silicon within the above range, it is possible to ensure that the volume expansion of the negative electrode composite material is small, and better cycle performance can be obtained, and a good balance can be obtained between reducing the residual lithium content of the negative electrode composite material and improving the cycle performance of the lithium ion secondary battery.

[0039] In some embodiments of the present invention, in the negative electrode composite material of the present invention, the intensity ratio of the D peak to the G peak in the Raman spectrum of the negative electrode composite material is 1 D / I G The intensity ratio of the D peak to the G peak in the Raman spectrum of the negative electrode composite material is greater than 0.8 and less than 2.0, preferably, greater than 1.5 and less than 1.8. D / I G Controlling within the above range can make the conductivity of the carbon coating layer better and enable the lithium-ion secondary battery to obtain better cycle performance. The D band (~1350cm -1 ) and G band (~1580cm -1 )'s peak intensity I D and I G The Raman equipment model used is, for example, Renishaw Qontor, and the wave number range used is, for example, 100-1800cm -1 The laser wavelength used is, for example, 532 nm.

[0040] In some embodiments of the present invention, in the negative electrode composite material of the present invention, based on the weight of the negative electrode active material particles, the coating amount of the carbon coating layer is in the range of 1wt% to 30wt%, preferably, the coating amount of the carbon coating layer is in the range of 3wt% to 20wt%, and more preferably, the coating amount of the carbon coating layer is in the range of 5wt% to 10wt%. By controlling the coating amount of the carbon coating layer within the above range, a good balance can be obtained between the capacity of the material and the coating uniformity.

[0041] In another typical embodiment of the present invention, a method for preparing a negative electrode composite material is provided, the method comprising: carbon-coating a silicon oxide precursor with a carbon source to form a carbon-coated silicon oxide; mixing the carbon-coated silicon oxide with a lithium source to form a first mixture, performing a first heat treatment on the first mixture to form a calcined product, and then performing a second heat treatment on the calcined product to form a pre-lithium product; and washing the pre-lithium product to form a negative electrode composite material.

[0042] The method for preparing the negative electrode composite material of the present invention is conducive to the control and optimization of residual lithium, can effectively reduce the amount of residual lithium, can avoid the slurry from becoming "jelly" in the process of preparing the slurry using the negative electrode composite material, can improve the processing performance of the slurry, can improve the first coulomb efficiency and cycle performance of the lithium ion secondary battery, and can inhibit the gas production of the slurry. The negative electrode composite material obtained by the above method according to the present invention has a significantly reduced amount of residual lithium, can improve the processing performance of the slurry, can improve the first coulomb efficiency and cycle performance of the lithium ion secondary battery.

[0043] The silicon oxide precursor in the present invention, such as SiO x (wherein 0.5≤x≤1.6) can be prepared by conventional methods in the art. In some embodiments of the present invention, the silicon oxide precursor can be prepared by the following process: silicon powder and silicon dioxide of a certain particle size are mixed in a molar ratio of about 1.1:1, and then placed on a vibrator for about 12 hours to mix evenly, and about 1 kg of the above-mentioned substances mixed evenly are pressed into a block, and then the block is placed in a vacuum sublimation furnace and heated to a temperature of 1200°C-1500°C, and a block silicon oxide precursor is prepared by adjusting the vacuum degree to 0-30Pa, the heating time to 8h-10h, and the collection end temperature to 400°C-800°C, and the block silicon oxide precursor is placed in a crusher to be crushed to the millimeter level, and then the millimeter-level silicon oxide precursor is placed in an air flow mill for crushing, and powders of different particle sizes are separated by an air flow classifier, and finally the powders of different particle sizes are mixed with large and small particles, and finally the silicon oxide precursor of the desired particle size is obtained.

[0044] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, at a pressure of 50Pa-10000Pa and a temperature of 600°C-1000°C, chemical vapor deposition is performed on the surface of a silicon oxide precursor using at least one of alkanes, alkenes and alkynes as a carbon source to carbon-coat the silicon oxide precursor to form a carbon-coated silicon oxide. In some embodiments of the present invention, the carbon coating process can be performed in a rotary kiln, a fixed bed or a fluidized bed.

[0045] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the washing treatment includes mixing the pre-lithium product with water, alcohol or acid, preferably with a solid content of 5wt%-20wt%, such as 5wt%-10wt%, 10wt%-15wt% or 15wt%-20wt% to form a second mixture, ultrasonically treating the second mixture, then dispersing it, then filtering it, and finally drying the filtered material. During the washing process, water can be used to dissolve alkaline substances such as Li2CO3, LiOH and Li2SiO3, alcohol can be used to slightly dissolve LiOH, and acid can be used to neutralize the alkali generated on the surface of the pre-lithium product during washing; ultrasonic treatment can be used to wash the pre-lithium product more cleanly, ensuring a good washing effect, and improving the cycle performance of the lithium ion secondary battery. Through the washing treatment, the amount of residual lithium can be effectively reduced, the "jelly" of the slurry can be avoided in the process of preparing the slurry using the negative electrode composite material, the processing performance of the slurry can be improved, and the first coulomb efficiency and cycle performance of the lithium ion secondary battery can be further improved. Since Li2Si2O5 is insoluble in water, while Li2SiO3 is soluble in water, the weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, can also be regulated by washing treatment.

[0046] In some embodiments of the present invention, the prepared pre-lithium product, such as pre-lithium SiO x The (0.5≤x≤1.6) material is mixed with water at a solid content of 5wt%-20wt% to form a second mixture, the second mixture is firstly ultrasonically treated for 1min-30min at room temperature, and then the second mixture is dispersed for 8h-48h using a magnetic stirrer, followed by suction filtration, and after suction filtration, pure water is poured on the material on the filter paper, and the material is washed twice in the form of suction filtration, and finally the filtered material is vacuum dried at 100℃-120℃ for 3-8 hours.

[0047] In some embodiments of the present invention, in the above-mentioned method for preparing a negative electrode composite material, in order to better neutralize the alkali generated on the surface of the pre-lithium product during washing, the acid is selected from at least one of hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid and boric acid.

[0048] In some embodiments of the present invention, the prepared pre-lithium product, such as pre-lithium SiO xThe (0.5≤x≤1.6) material is mixed with at least one of hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid and boric acid, for example, citric acid with a concentration of 1 mol / L, with a solid content of 5wt%-20wt% to form a second mixture, the second mixture is firstly ultrasonically treated for 1min-30min at room temperature, and then the second mixture is dispersed for 8h-48h using a magnetic stirrer, followed by suction filtration, after which pure water is poured on the material on the filter paper, and the material is washed twice by suction filtration, and finally the filtered material is vacuum dried at 100°C-120°C for 3-8 hours.

[0049] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the weight ratio of the lithium source to the carbon-coated silicon oxide is in the range of 5:95 to 40:60. By controlling the weight ratio of the lithium source to the carbon-coated silicon oxide within the above range, it is possible to ensure that the silicon oxide is fully pre-lithiated, the amount of residual lithium can be reduced, and the first coulombic efficiency and cycle performance of the lithium-ion secondary battery can be further improved. In some embodiments of the present invention, the lithium source may include any one of a lithium ingot, a lithium metal powder, and a lithium foil.

[0050] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the temperature of the first heat treatment is in the range of 400°C-750°C, and the time of the first heat treatment is in the range of 1h-5h. By controlling the temperature and time of the first heat treatment within the above range, it is possible to ensure that the silicon oxide is fully pre-lithiated, the amount of residual lithium can be reduced, and the first coulombic efficiency and cycle performance of the lithium-ion secondary battery can be further improved.

[0051] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the temperature of the second heat treatment is greater than or equal to 800°C and less than 925°C, and the time of the second heat treatment is in the range of 1h-6h. By controlling the temperature and time of the second heat treatment within the above range, it is possible to ensure that the silicon oxide is fully pre-lithiated, the size of the crystalline silicon is prevented from being too large, the amount of residual lithium can be effectively reduced, and the first coulombic efficiency and cycle performance of the lithium-ion secondary battery can be further improved.

[0052] In some embodiments of the present invention, under the protection of an inert atmosphere of argon, a lithium source and a carbon-coated silicon oxide are ground and mixed in a weight ratio of 5:95 to 40:60 to form a first mixture, and then the first mixture is placed in a rotary kiln, and calcined at 400°C-750°C for 1h-5h in an argon atmosphere to allow the carbon-coated silicon oxide to fully react with the lithium metal, and then heat-treated at 800°C-924°C for 1h-6h to regulate the pre-lithiation depth and the amount of lithium-containing silicate to obtain a pre-lithiation product.

[0053] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the ultrasonic treatment time is in the range of 1 min-30 min. By controlling the ultrasonic treatment time within the above range, the pre-lithium product can be washed more cleanly, ensuring a good washing effect, and at the same time avoiding damage to the particles of the pre-lithium product.

[0054] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the time for dispersing can be controlled within the range of 8h-48h, mainly from the perspective of energy consumption, time cost and washing effect. If the time for dispersing is too short, it may not be washed cleanly, and if the time for dispersing is too long, the energy consumption and time cost are high. By controlling the time for dispersing within the above range, not only a good washing effect can be ensured, but also energy consumption and time cost can be reduced.

[0055] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, in order to better carbon-coat at least a portion of the surface of silicon oxide and obtain a good coating effect, the carbon source includes at least one of alkanes, alkenes and alkynes.

[0056] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the alcohol can be selected from at least one of ethanol, isopropanol and butanol, so that a better washing effect can be obtained. The alcohol is preferably ethanol, which can slightly dissolve LiOH. In the case of using ethanol for cleaning, since ethanol is easy to volatilize, it is beneficial to dry in subsequent steps. Ethanol generally contains water, and the water contained in ethanol can dissolve alkaline substances such as Li2CO3, LiOH and Li2SiO3. As ethanol, 75% concentration of ethanol is generally used.

[0057] In some embodiments of the present invention, the prepared pre-lithium product, such as pre-lithium SiO x The (0.5≤x≤1.6) material is mixed with at least one of ethanol, isopropanol and butanol at a solid content of 5wt%-20wt% to form a second mixture, the second mixture is firstly ultrasonically treated for 1min-30min at room temperature, and then the second mixture is dispersed for 8h-48h using a magnetic stirrer, followed by suction filtration, and after suction filtration, pure water is poured on the material on the filter paper, and the filtered material is washed twice in the form of suction filtration, and finally the filtered material is vacuum dried at 100℃-120℃ for 3-8 hours.

[0058] In another typical embodiment of the present invention, a negative electrode of a lithium ion secondary battery is provided, and the negative electrode of the lithium ion secondary battery comprises the negative electrode composite material described above. Since the negative electrode of the lithium ion secondary battery of the present invention comprises the negative electrode composite material described above, the amount of residual lithium can be effectively reduced, the processing performance of the slurry can be improved, and the first coulombic efficiency and cycle performance of the lithium ion secondary battery can be improved.

[0059] The negative electrode sheet of the present invention can be made according to conventional methods in the art. For example, the negative electrode composite material, the conductive agent and the binder of the present invention can be dispersed in water as a solvent to form a uniform negative electrode slurry, and the negative electrode slurry is coated on the negative electrode collector, and after drying, the negative electrode sheet is obtained. The conductive agent can be conductive carbon black, conductive graphite, vapor-grown carbon fiber, carbon nanotubes or any combination thereof. The binder can be one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA) and polyimide (PI), etc., preferably a polyacrylic acid (PAA) binder.

[0060] In another typical embodiment of the present invention, a lithium ion secondary battery is provided, the lithium ion secondary battery comprising: a positive electrode, a negative electrode, and a separator, the negative electrode comprising the negative electrode composite material described above. Since the lithium ion secondary battery of the present invention comprises the negative electrode composite material described above, the amount of residual lithium can be effectively reduced, the processing performance of the slurry can be improved, and the first coulombic efficiency and cycle performance of the lithium ion secondary battery can be improved.

[0061] The positive electrode of the present invention includes a positive electrode collector and a positive electrode active material layer containing a positive electrode active material. The positive electrode active material layer is formed on both surfaces of the positive electrode collector. A metal foil such as aluminum foil, nickel foil or stainless steel foil can be used as the positive electrode collector.

[0062] The positive electrode active material layer contains one or more positive electrode materials capable of inserting and extracting lithium ions as positive electrode active materials, and may contain additional materials such as a positive electrode binder and / or a positive electrode conductor as necessary.

[0063] Preferably, the positive electrode material is a lithium-containing compound. Examples of such lithium-containing compounds include lithium-transition metal composite oxides, lithium-transition metal phosphate compounds, and the like. Lithium-transition metal composite oxides are oxides containing Li and one or more transition metal elements as constituent elements, and lithium-transition metal phosphate compounds are phosphate compounds containing Li and one or more transition metal elements as constituent elements. The transition metal element is advantageously one or more of Co, Ni, Mn, and Fe, and the like.

[0064] Examples of lithium-transition metal composite oxides can include, for example, LiCoO2 and LiNiO2. Examples of lithium-transition metal phosphate compounds can include, for example, LiFePO4 and LiFe 1-u Mn u PO4(0 < u < 1), etc.

[0065] The negative electrode of the present invention includes a negative electrode current collector and a negative electrode active material layer containing a negative electrode composite material. The negative electrode active material layer is formed on both surfaces of the negative electrode current collector. A metal foil such as copper (Cu) foil, carbon-coated copper foil, nickel foil, or stainless steel foil can be used as the negative electrode current collector.

[0066] The separator of the present invention is used to separate the positive electrode and the negative electrode in the battery and allow lithium ions to pass through it while preventing a current short circuit caused by contact between the positive electrode and the negative electrode. The separator is, for example, a porous membrane formed of a synthetic resin or ceramic, and can be a laminated membrane in which two or more porous membranes are laminated. Examples of synthetic resins include, for example, polytetrafluoroethylene, polypropylene, and polyethylene.

[0067] In an embodiment of the present invention, when charging a lithium-ion secondary battery, for example, lithium ions are released from the positive electrode and embedded in the negative electrode through the electrolyte impregnated in the separator. When discharging the lithium-ion secondary battery, for example, lithium ions are released from the negative electrode and embedded in the positive electrode through the electrolyte impregnated in the separator.

[0068] The following further describes the present application in detail with specific examples, and these examples should not be construed as limiting the scope claimed by the present application.

[0069] Example 1

[0070] Preparation of Negative Electrode Composite Material

[0071] Under a pressure of 50 Pa and at a temperature of 920 °C, using methane as a carbon source, chemical vapor deposition was carried out on the surface of 20 g of silicon oxide precursor SiO x (x = 1) material to perform carbon coating treatment on the silicon oxide precursor SiO x (x = 1) material to form 21 g of carbon-coated SiO x (x = 1) material.

[0072] Under the protection of an inert atmosphere of argon, lithium ingot and carbon-coated SiO x (x = 1) material were ground and mixed at a weight ratio of 20:80 to form a first mixture, and then the first mixture was placed in a rotary furnace and calcined at 500 °C for 3 h under an argon atmosphere to allow the carbon-coated SiO x material to fully react with lithium metal, and then heat-treated at 850 °C for 3 h to obtain pre-lithiated SiOx Material.

[0073] The prepared pre-lithium SiO x The material and hydrochloric acid with a concentration of 1 mol / L are taken into a beaker with a solid content of 5 wt% and mixed to form a second mixture. The second mixture is first ultrasonically treated for 30 minutes at room temperature, and then dispersed for 48 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.

[0074] Preparation of negative electrode

[0075] Weigh 4 g of the negative electrode composite material prepared by the above process, and fully stir and mix the negative electrode composite material with conductive carbon black Super-P as a conductive agent and polyacrylic acid PAA as a binder in an appropriate amount of deionized water in a mass ratio of 82:8:10, and form a uniform negative electrode slurry by adjusting the solid content to 42 wt%, and then coat the negative electrode slurry on the surface of copper foil as a negative electrode collector, and obtain a negative electrode sheet after drying.

[0076] Battery Assembly

[0077] The prepared negative electrode sheet, separator, lithium sheet, gasket and battery shell are stacked in sequence and injected with 100 μl of electrolyte, and then sealed with a sealing machine to assemble the required half-cell.

[0078] Example 2

[0079] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 15:85 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 450°C for 3 h under an argon atmosphere to form a carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 900 °C for 4 h to obtain pre-lithium SiO x Material;

[0080] The prepared pre-lithium SiO x The material and hydrochloric acid with a concentration of 1 mol / L are taken into a beaker with a solid content of 5 wt% and mixed to form a second mixture. The second mixture is first ultrasonically treated for 10 minutes at room temperature, and then dispersed for 48 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.

[0081] Example 3

[0082] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 10:90 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600°C for 2 h in an argon atmosphere to make the carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 920 °C for 5 h to obtain pre-lithium SiO x Material;

[0083] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 15 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 5 minutes at room temperature, and then dispersed for 16 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.

[0084] Example 4

[0085] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400°C for 1 h under an argon atmosphere to make the carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 924 °C for 6 h to obtain pre-lithium SiO x Material;

[0086] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 20 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 1 min at room temperature, and then dispersed for 8 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and the material is washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.

[0087] Example 5

[0088] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 25:75 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600°C for 4 hours under an argon atmosphere to make the carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 850 °C for 2 h to obtain pre-lithium SiO x Material;

[0089] The prepared pre-lithium SiO x The material and hydrochloric acid with a concentration of 1 mol / L are taken into a beaker with a solid content of 5 wt% and mixed to form a second mixture. The second mixture is first ultrasonically treated for 20 minutes at room temperature, and then dispersed for 36 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.

[0090] Example 6

[0091] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 30:70 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600°C for 5 h in an argon atmosphere to make the carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 820 °C for 2 h to obtain pre-lithium SiO x Material;

[0092] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 10 wt% are taken into a beaker and mixed to form a second mixture, the second mixture is first ultrasonically treated for 30 minutes at room temperature, and then the second mixture is dispersed for 40 hours using a magnetic stirrer, followed by suction filtration, and after suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration, and finally the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.

[0093] Example 7

[0094] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO xThe (x=1) materials were ground and mixed in a weight ratio of 40:60 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750°C for 5 h under an argon atmosphere to form a carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 800 °C for 1 h to obtain pre-lithium SiO x Material;

[0095] The prepared pre-lithium SiO x The material and hydrochloric acid with a concentration of 1 mol / L are taken into a beaker with a solid content of 5 wt% and mixed to form a second mixture. The second mixture is first ultrasonically treated for 30 minutes at room temperature, and then dispersed for 48 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.

[0096] Example 8

[0097] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 20:80 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 550°C for 4 hours under an argon atmosphere to form a carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 900 °C for 5 h to obtain pre-lithium SiO x Material;

[0098] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 10 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 10 minutes at room temperature, and then dispersed for 24 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.

[0099] Example 9

[0100] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 30:70 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600°C for 5 h in an argon atmosphere to make the carbon-coated SiO xThe material reacts fully with lithium metal and then heat-treated at 820 °C for 2 h to obtain pre-lithium SiO x Material;

[0101] The prepared pre-lithium SiO x The material and 75% ethanol at a solid content of 5wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 30 minutes at room temperature, and then dispersed for 40 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.

[0102] Example 10

[0103] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 30:70 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600°C for 5 h in an argon atmosphere to make the carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 820 °C for 2 h to obtain pre-lithium SiO x Material;

[0104] The prepared pre-lithium SiO x The material and pure water are taken into a beaker with a solid content of 5wt% and mixed to form a second mixture. The second mixture is first ultrasonically treated for 30 minutes at room temperature, and then dispersed for 48 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.

[0105] Comparative Example 1

[0106] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 50:50 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750°C for 5 h under an argon atmosphere to form a carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 800 °C for 1 h to obtain pre-lithium SiO x Material;

[0107] The prepared pre-lithium SiO xThe material and hydrochloric acid with a concentration of 1 mol / L are taken into a beaker with a solid content of 5 wt% and mixed to form a second mixture. The second mixture is first ultrasonically treated for 30 minutes at room temperature, and then dispersed for 48 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.

[0108] Comparative Example 2

[0109] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 40:60 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750°C for 5 h under an argon atmosphere to form a carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 800 °C for 1 h to obtain pre-lithium SiO x Material;

[0110] No pre-lithiation of SiO x The material is washed and the pre-lithium SiO x The material is used as a negative electrode composite material.

[0111] Comparative Example 3

[0112] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400°C for 1 h under an argon atmosphere to make the carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 1000 °C for 6 h to obtain pre-lithium SiO x Material;

[0113] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 20 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 1 min at room temperature, and then dispersed for 8 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and the material is washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.

[0114] Comparative Example 4

[0115] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 350°C for 1 h under an argon atmosphere to form a carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 924 °C for 6 h to obtain pre-lithium SiO x Material;

[0116] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 20 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 1 min at room temperature, and then dispersed for 8 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and the material is washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.

[0117] Comparative Example 5

[0118] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 30:70 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600°C for 5 h in an argon atmosphere to make the carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 820 °C for 2 h to obtain pre-lithium SiO x Material;

[0119] The prepared pre-lithium SiO x The material and pure water are taken into a beaker with a solid content of 5wt% and mixed to form a second mixture. The second mixture is dispersed at room temperature for 48 hours using a magnetic stirrer, and then filtered. After filtering, pure water is poured on the material on the filter paper, and washed twice in the form of filtering. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.

[0120] Comparative Example 6

[0121] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO xThe (x=1) materials were ground and mixed in a weight ratio of 2:98 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400°C for 1 h under an argon atmosphere to make the carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 924 °C for 6 h to obtain pre-lithium SiO x Material;

[0122] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 20 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 1 min at room temperature, and then dispersed for 8 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and the material is washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.

[0123] Comparative Example 7

[0124] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 40:60 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750°C for 5 h under an argon atmosphere to form a carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 800 °C for 1 h to obtain pre-lithium SiO x Material;

[0125] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 5 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 40 minutes at room temperature, and then dispersed for 48 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.

[0126] Comparative Example 8

[0127] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400°C for 0.5 h in an argon atmosphere to make the carbon-coated SiO xThe material fully reacts with lithium metal and then heat-treated at 924 °C for 6 h to obtain pre-lithium SiO x Material;

[0128] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 20 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 1 min at room temperature, and then dispersed for 8 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and the material is washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.

[0129] Comparative Example 9

[0130] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400°C for 1 h under an argon atmosphere to make the carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 924 °C for 7 h to obtain pre-lithium SiO x Material;

[0131] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 20 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 1 min at room temperature, and then dispersed for 8 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and the material is washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.

[0132] Material property testing

[0133] The negative electrode composite materials in Examples 1-10 and Comparative Examples 1-9 were tested to obtain I D / I G , the results of the content of Li2CO3, the content of LiOH, the content of Li2SiO3, the weight ratio of Li2Si2O5 and Li2SiO3 Li2Si2O5 / Li2SiO3 and the size of crystalline silicon.

[0134] The mass fractions of Li2Si2O5 and Li2SiO3 were calculated by XRD (Druker Advanced D8) test results, thereby obtaining the weight ratio of Li2Si2O5 and Li2SiO3, Li2Si2O5 / Li2SiO3.

[0135] The content of Li2SiO3 was calculated from the XRD pattern.

[0136] The size of the crystalline silicon was calculated from the XRD (Druker Advanced D8) test results (calculated using the Scherrer formula using the half-width of the crystalline silicon peak on the XRD spectrum).

[0137] XRD test conditions: 10-80°, 1° / min.

[0138] Neutralization titration method: The negative electrode composite material and pure water are measured in a mass ratio of 1:9 into a beaker and mixed. The negative electrode composite material is dispersed for 1 hour using a magnetic stirrer at room temperature, and the dispersion is allowed to stand for 1 hour. The dispersion is filtered. The obtained 10 mL filtrate is automatically titrated with 0.2 M hydrochloric acid using an acid-base automatic titrator, and the first endpoint (a mL) and the second endpoint (b mL) are obtained.

[0139] Li2CO3 content = [pure water amount (g) / filtrate amount (g)] × 2 × (b / 1000) × (hydrochloric acid titration equivalent concentration × coefficient) × (1 / 2) × (Li2CO3 molar mass) × [100 (%) / sample amount (g)]

[0140] LiOH content = [amount of pure water (g) / amount of filtrate (g)] × [(ab) / 1000] × (equivalent concentration of hydrochloric acid titration × coefficient) × (1 / 2) × (molar mass of LiOH) × [100 (%) / sample amount (g)].

[0141] Battery performance test

[0142] The half-cells in Examples 1-10 and Comparative Examples 1-9 were subjected to charge and discharge tests at a voltage between 0V and 1.5V at 25°C. The half-cells in the above-mentioned Examples and Comparative Examples were first subjected to a cycle test at 25°C with a charge and discharge current of 0.1C for one time (the charge and discharge voltage range was 0V-1.5V) to determine the initial discharge capacity and initial coulombic efficiency of the battery. The battery was then subjected to a charge and discharge cycle test 50 times with a current of 1C (the charge and discharge cut-off voltage was 0V-1.5V) to determine the capacity retention rate of the battery after 50 cycles. Initial coulombic efficiency (%) = initial discharge capacity / initial charge capacity × 100%. The experimental results are shown in Tables 1 and Figure 2-5 Shown in.

[0143] from Figure 2 It can be seen that the relationship between the size of crystalline silicon in the negative electrode composite material and the weight ratio of Li2Si2O5 to Li2SiO3 is linear. Figure 3 It can be seen that when the intensity ratio of the D peak to the G peak in the Raman spectrum of the negative electrode composite material is D / I G When it is greater than 0.8 and less than 2.0, preferably greater than 1.5 and less than 1.8, better cycle performance can be obtained. Figure 4 and Figure 5 In the diagram, the direction from bottom to top is from the surface to the inside. Figure 4 and Figure 5 It can be seen that the water-soluble Li2CO3 and LiOH are basically on the surface of the particles (Li2CO3 and LiOH in Example 2 are very small, so the signal on the surface XPS spectrum is very weak), and Li2SiO3 is distributed in the particles from the position close to the surface of the particles to the center of the particles with a gradually decreasing trend. Other water-insoluble lithium silicates (Li2Si2O5) are distributed closer to the center of the particles than Li2SiO3.

[0144] Table 1 Material properties and electrochemical performance test results

[0145]

[0146] It can be seen from the above test results that the above embodiments of the present invention achieve the following technical effects:

[0147] By comparing the results of Examples 1-10 with Comparative Examples 1-9, it can be seen that the batteries in Examples 1-10 in which the content of Li2CO3 based on the weight of the negative electrode active material particles, the content of LiOH and the weight ratio of Li2Si2O5 to Li2SiO3 Li2Si2O5 / Li2SiO3 are not completely within the scope of the present invention, in which the content of Li2CO3 based on the weight of the negative electrode active material particles is greater than 0.01wt% and less than 1wt%, the content of LiOH is greater than 0.001wt% and less than 0.1wt% and the weight ratio of Li2Si2O5 to Li2SiO3 Li2Si2O5 / Li2SiO3 is in the range of 1.00 to 10.00 have higher first coulombic efficiency and higher discharge capacity retention rate after 50 cycles.

[0148] By comparing the results of Examples 1-10 with those of Comparative Example 9, it can be seen that the batteries in Examples 1-10, in which the weight ratio Li2Si2O5 to Li2SiO3 based on the weight of the negative electrode active material particles Li2Si2O5 / Li2SiO3 is in the range of 1.00 to 10.00 and the content of Li2SiO3 is greater than 1.0wt% and less than 48.0wt%, have higher first coulombic efficiency and higher discharge capacity retention after 50 cycles, compared with Comparative Example 9 in which both the weight ratio Li2Si2O5 to Li2SiO3 based on the weight of the negative electrode active material particles Li2Si2O5 / Li2SiO3 and the content of Li2SiO3 are not within the scope of the present invention.

[0149] According to the results of Example 6, Example 9 and Example 10, it can be seen that the negative electrode composite material of the present invention can be obtained by the preparation method of the present invention including acid washing, alcohol washing or water washing treatment, which can effectively reduce the amount of residual lithium, improve the processing performance of the slurry, and improve the first coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles.

[0150] By comparing the results of Example 7 with those of Comparative Example 1, it can be seen that when the weight ratio of the lithium source to the carbon-coated silicon oxide is in the range of 5:95 to 40:60, a negative electrode composite material having a suitable Li2CO3 content, a suitable LiOH content, a suitable Li2SiO3 content and a suitable weight ratio of Li2Si2O5 to Li2SiO3 Li2Si2O5 / Li2SiO3 can be obtained, which can effectively reduce the amount of residual lithium, improve the processing performance of the slurry, and improve the battery's first coulombic efficiency and the discharge capacity retention rate after 50 cycles.

[0151] By comparing the results of Example 7 with those of Comparative Example 2, it can be seen that by x By washing the material, a negative electrode composite material having a suitable Li2CO3 content, a suitable LiOH content, a suitable Li2SiO3 content and a suitable weight ratio of Li2Si2O5 to Li2SiO3 (Li2Si2O5 / Li2SiO3) can be obtained, which can effectively reduce the amount of residual lithium, improve the processing performance of the slurry, and improve the battery's first coulombic efficiency and the discharge capacity retention rate after 50 cycles.

[0152] By comparing the results of Example 4 with those of Comparative Example 3, it can be seen that when the temperature of the second heat treatment is within the range of greater than or equal to 800°C and less than 925°C, a negative electrode composite material having a suitable LiOH content, a suitable Li2SiO3 content and a suitable weight ratio of Li2Si2O5 to Li2SiO3 Li2Si2O5 / Li2SiO3 can be obtained, the size of the crystalline silicon can be controlled to avoid the crystalline silicon being too large, the amount of residual lithium can be effectively reduced, the processing performance of the slurry can be improved, and the first coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles can be improved.

[0153] By comparing the results of Example 4 with those of Comparative Example 4, it can be seen that when the temperature of the first heat treatment is within the range of 400°C-750°C, a negative electrode composite material having a suitable Li2CO3 content, a suitable LiOH content, a suitable Li2SiO3 content and a suitable weight ratio of Li2Si2O5 to Li2SiO3 (Li2Si2O5 / Li2SiO3) can be obtained, which can ensure a good pre-lithium effect, and can improve the first coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles. When the temperature of the first heat treatment is too low, the pre-lithium may not be pre-entered, and the first coulombic efficiency of the battery may be reduced.

[0154] By comparing the results of Example 10 with those of Comparative Example 5, it can be seen that when the washing treatment includes ultrasonic treatment of the second mixture, a negative electrode composite material having a suitable LiOH content, a suitable Li2SiO3 content and a suitable weight ratio of Li2Si2O5 to Li2SiO3 Li2Si2O5 / Li2SiO3 can be obtained, which can improve the battery's first coulombic efficiency and the discharge capacity retention rate after 50 cycles.

[0155] By comparing the results of Example 4 with those of Comparative Example 6, it can be seen that when the weight ratio of the lithium source to the carbon-coated silicon oxide is in the range of 5:95 to 40:60, a negative electrode composite material having a suitable Li2CO3 content, a suitable LiOH content, a suitable Li2SiO3 content, and a suitable weight ratio of Li2Si2O5 to Li2SiO3 (Li2Si2O5 / Li2SiO3) can be obtained, which can ensure a good pre-lithium effect, and can improve the first coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles. When the weight ratio of the lithium source to the carbon-coated silicon oxide is too low, pre-lithium may not be able to be pre-entered, lithium silicate may not be obtained, and the first coulombic efficiency of the battery may be reduced.

[0156] By comparing the results of Example 7 with those of Comparative Example 7, it can be seen that when the ultrasonic treatment time is in the range of 1 min-30 min, a negative electrode composite material having a suitable weight ratio of Li2Si2O5 to Li2SiO3 (Li2Si2O5 / Li2SiO3) can be obtained, particle fragmentation can be avoided, and the battery's first coulombic efficiency and the discharge capacity retention rate after 50 cycles can be improved.

[0157] By comparing the results of Example 4 with those of Comparative Example 8, it can be seen that when the time for the first heat treatment is in the range of 1h-5h, a negative electrode composite material having a suitable Li2CO3 content, a suitable LiOH content, a suitable Li2SiO3 content and a suitable weight ratio of Li2Si2O5 to Li2SiO3 Li2Si2O5 / Li2SiO3 can be obtained, which can ensure a good pre-lithium effect and can improve the battery's first coulombic efficiency and the discharge capacity retention rate after 50 cycles.

[0158] By comparing the results of Example 4 with those of Comparative Example 9, it can be seen that when the time for the second heat treatment is in the range of 1h-6h, a negative electrode composite material having a suitable Li2SiO3 content and a suitable weight ratio of Li2Si2O5 to Li2SiO3 (Li2Si2O5 / Li2SiO3) can be obtained, the size of the crystalline silicon can be controlled to avoid the crystalline silicon being too large, and the first coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles can be improved.

[0159] It can be seen from the above battery performance test results that the negative electrode composite material of the present invention, the method for preparing the negative electrode composite material, and the negative electrode and lithium ion secondary battery containing the negative electrode composite material can effectively reduce the amount of residual lithium, improve the processing performance of the slurry, and improve the first coulombic efficiency and cycle performance of the lithium ion secondary battery.

[0160] The above description is only the preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A negative electrode composite material, It is characterized in that The negative electrode composite material includes negative electrode active material particles and Li 2 CO 3 and LiOH, the negative electrode active material particles comprising: Contains silicon oxide, Li 2 SiO 3 and Li 2 Si 2 O 5 particles; and a carbon coating layer covering at least a portion of the surface of the particle, Based on the weight of the negative electrode active material particles, Li 2 CO 3 The content of LiOH is greater than 0.01wt% and less than 1wt%, the content of LiOH is greater than 0.001wt% and less than 0.1wt%, and Li 2 Si 2 O 5 With Li 2 SiO 3 Weight ratio Li 2 Si 2 O 5 / Li 2 SiO 3 In the range of 1.00 to 10.

00.

2. The negative electrode composite material according to claim 1, It is characterized in that Based on the weight of the negative electrode active material particles, Li 2 SiO 3 The content of is greater than 1.0wt% and less than 48.0wt%.

3. The negative electrode composite material according to claim 1 or 2, It is characterized in that Li 2 SiO 3 The Li is distributed in the particle in a gradually decreasing trend from a position close to the surface of the particle toward the center of the particle, and Li 2 Si 2 O 5 Distributed in Li 2 SiO 3 at a position closer to the center of the particle.

4. The negative electrode composite material according to claim 1 or 2, It is characterized in that The carbon coating layer covers the entire surface of the particle.

5. The negative electrode composite material according to claim 1 or 2, It is characterized in that The silicon oxide is SiO x , where 0.5≤x≤1.

6.

6. The negative electrode composite material according to claim 1 or 2, It is characterized in that The silicon in the silicon oxide exists in the form of crystalline silicon, and the size of the crystalline silicon is in the range of 5.0 nm to 12.0 nm.

7. The negative electrode composite material according to claim 1 or 2, It is characterized in that The intensity ratio of the D peak to the G peak in the Raman spectrum of the negative electrode composite material is D / I G Greater than 0.8 and less than 2.0, preferably, greater than 1.5 and less than 1.

8.

8. The negative electrode composite material according to claim 1 or 2, It is characterized in that The coating amount of the carbon coating layer is in a range of 1 wt % to 30 wt % based on the weight of the negative electrode active material particles.

9. A method for preparing a negative electrode composite material, It is characterized in that The method comprises: Performing carbon coating treatment on a silicon oxide precursor using a carbon source to form carbon-coated silicon oxide; mixing the carbon-coated silicon oxide with a lithium source to form a first mixture, subjecting the first mixture to a first heat treatment to form a calcined product, and then subjecting the calcined product to a second heat treatment to form a pre-lithium product; and The pre-lithium product is washed to form the negative electrode composite material.

10. The method for preparing a negative electrode composite material according to claim 9, It is characterized in that The washing treatment includes mixing the pre-lithium product with water, alcohol or acid, preferably at a solid content of 5wt%-20wt%, to form a second mixture, ultrasonically treating the second mixture, then dispersing it, then filtering it, and finally drying the filtered material.

11. The method for preparing a negative electrode composite material according to claim 10, It is characterized in that The acid is selected from at least one of hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid and boric acid.

12. The method for preparing a negative electrode composite material according to claim 9, It is characterized in that A weight ratio of the lithium source to the carbon-coated silicon oxide is in a range of 5:95 to 40:

60.

13. The method for preparing a negative electrode composite material according to claim 9, It is characterized in that The temperature for performing the first heat treatment is in the range of 400° C.-750° C., and the time for performing the first heat treatment is in the range of 1 h-5 h.

14. The method for preparing a negative electrode composite material according to claim 9, It is characterized in that The temperature of the second heat treatment is in the range of greater than or equal to 800° C. and less than 925° C., and the time of the second heat treatment is in the range of 1 h to 6 h.

15. The method for preparing a negative electrode composite material according to claim 10, It is characterized in that The ultrasonic treatment is performed for a time ranging from 1 min to 30 min.

16. The method for preparing a negative electrode composite material according to claim 10, It is characterized in that The dispersion is carried out for a period of time ranging from 8 h to 48 h.

17. The method for preparing a negative electrode composite material according to claim 9, It is characterized in that The carbon source includes at least one of alkanes, alkenes and alkynes.

18. The method for preparing a negative electrode composite material according to claim 10, It is characterized in that The alcohol is selected from at least one of ethanol, isopropanol and butanol.

19. A negative electrode for a lithium ion secondary battery, It is characterized in that The negative electrode of the lithium ion secondary battery comprises the negative electrode composite material according to any one of claims 1 to 8.

20. A lithium ion secondary battery, It is characterized in that The lithium-ion secondary battery comprises: positive electrode, The negative electrode, and Diaphragm, Characterized in that the negative electrode comprises the negative electrode composite material according to any one of claims 1 to 8.