Negative electrode composite material, preparation method thereof, negative electrode and lithium ion secondary battery
By using negative electrode composite materials in lithium-ion secondary batteries, negative electrode active material particles containing silicon oxide and lithium silicate and a carbon coating layer, combined with carbon coating and washing treatments, the problem of high residual lithium content in the negative electrode material is solved. problem, significantly improving the Coulombic efficiency and cycle performance of lithium-ion secondary batteries.
Patent Information
- Application Number
- CN202310333248.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-01
AI Technical Summary
The residual lithium content of the negative electrode material in existing lithium-ion secondary batteries is too high, making it difficult to improve the processing performance of the slurry and effectively improve the first Coulombic efficiency and cycle performance of the lithium-ion secondary batteries.
A negative electrode composite material is used. The material includes negative electrode active material particles and Li2CO3 and LiOH on the surface of the negative electrode active material particles. The negative electrode active material particles include silicon oxide and lithium silicate. The carbon coating layer coats the surface of the particles. The carbon coating process, heat treatment and washing process form the negative electrode composite material.
Significantly reduce the amount of residual lithium, improve the processing performance of the slurry, improve the first Coulombic efficiency and cycle performance of lithium-ion secondary batteries, and avoid the jelly phenomenon of the slurry.
Smart Images

Figure CN118738307A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium ion secondary batteries, and in particular to a negative electrode composite material, a method for preparing the negative electrode composite material, and a negative electrode and a lithium ion secondary battery comprising the negative electrode composite material. Background Art
[0002] In recent years, with the continuous development of electronic technology, people's demand for battery devices used to support the energy supply of electronic devices has been increasing. Nowadays, batteries that can store more electricity and output high power are needed. Traditional lead-acid batteries and nickel-metal hydride batteries can no longer meet the needs of new electronic products such as mobile devices such as smart phones and fixed equipment such as power storage systems. Therefore, lithium-ion secondary batteries have attracted widespread attention. In the process of developing lithium-ion secondary batteries, their capacity and performance have been effectively improved. Lithium-ion secondary batteries have the advantages of high energy density, high operating voltage, long cycle life, and low environmental pollution. They have become a new green high-energy chemical power source with great development potential in the world today.
[0003] A lithium-ion secondary battery comprises a positive electrode, a negative electrode containing a negative electrode material, and an electrolyte. Various types of negative electrode materials have been developed, among which silicon-based negative electrode materials are one of the more promising negative electrode materials. The prior art discloses the use of pre-lithiation technology to improve the performance of silicon-based negative electrode materials and to control the amount of residual lithium in silicon-based negative electrode materials, but the upper and lower limits of the control of the amount of residual lithium in silicon-based negative electrode materials in the prior art are both relatively high, making it difficult to improve the processing performance of the slurry containing the negative electrode material and to effectively improve the first coulombic efficiency and cycle performance of the lithium-ion secondary battery. Therefore, it is necessary to develop a new negative electrode composite material, a method for preparing the negative electrode composite material, and a negative electrode and a lithium-ion secondary battery containing the negative electrode composite material. Summary of the invention
[0004] The main purpose of the present invention is to provide a negative electrode composite material, a method for preparing the negative electrode composite material, and a negative electrode and a lithium ion secondary battery containing the negative electrode composite material, so as to solve the problems in the prior art that the residual lithium content of the negative electrode material is too high, it is difficult to improve the processing performance of the slurry and it is difficult to effectively improve the first coulombic efficiency and cycle performance of the lithium ion secondary battery.
[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a negative electrode composite material, which includes negative electrode active material particles and Li2CO3 and LiOH on the surface of the negative electrode active material particles, the negative electrode active material particles include: particles containing silicon oxide and at least one lithium silicate selected from Li2SiO3 and Li2Si2O5; and a carbon coating layer coating at least a portion of the surface of the particles, based on the weight of the negative electrode active material particles, the content of Li2CO3 is greater than 0wt% and less than 0.01wt%, and the content of LiOH is greater than 0wt% and less than 0.01wt%.
[0006] Furthermore, in the above-mentioned negative electrode composite material, the silicon oxide is SiO x , where 0.5≤x≤1.6.
[0007] Further, in the above negative electrode composite material, the coating amount of the carbon coating layer is in the range of 1 wt % to 30 wt % based on the weight of the negative electrode active material particles.
[0008] Furthermore, in the above negative electrode composite material, the carbon coating layer covers the entire surface of the particles.
[0009] According to another aspect of the present invention, a method for preparing a negative electrode composite material is provided, the method comprising: carbon-coating a silicon oxide precursor with a carbon source to form a carbon-coated silicon oxide; mixing the carbon-coated silicon oxide with a lithium source to form a first mixture, performing a first heat treatment on the first mixture to form a calcined product, and then performing a second heat treatment on the calcined product to form a pre-lithium product; and washing the pre-lithium product to form a negative electrode composite material.
[0010] Furthermore, in the above-mentioned method for preparing a negative electrode composite material, the washing treatment includes mixing the pre-lithium product with water or an acid, preferably at a solid content of 2wt%-10wt% to form a second mixture, ultrasonically treating the second mixture, then dispersing it, followed by filtering it, and finally drying the filtered material.
[0011] Furthermore, in the above method for preparing a negative electrode composite material, the acid is selected from at least one of hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid and boric acid.
[0012] Further, in the above method for preparing a negative electrode composite material, a weight ratio of the lithium source to the carbon-coated silicon oxide is in the range of 5:95 to 15:85.
[0013] Further, in the above method for preparing a negative electrode composite material, the temperature for the first heat treatment is in the range of 500° C.-750° C., and the time for the first heat treatment is in the range of 2 h-5 h.
[0014] Further, in the above method for preparing a negative electrode composite material, the temperature for the second heat treatment is in the range of 925° C.-1050° C., and the time for the second heat treatment is in the range of 3 h-6 h.
[0015] Furthermore, in the above method for preparing a negative electrode composite material, the ultrasonic treatment is performed for a time in the range of 10 min to 30 min.
[0016] Furthermore, in the above method for preparing a negative electrode composite material, the dispersion time is in the range of 24h-72h.
[0017] Furthermore, in the above method for preparing a negative electrode composite material, the carbon source includes at least one of alkanes, alkenes and alkynes.
[0018] According to another aspect of the present invention, a negative electrode for a lithium ion secondary battery is provided. The negative electrode for a lithium ion secondary battery comprises the negative electrode composite material described above.
[0019] According to another aspect of the present invention, a lithium ion secondary battery is provided. The lithium ion secondary battery includes: a positive electrode, a negative electrode, and a separator. The negative electrode includes the negative electrode composite material described above.
[0020] The negative electrode composite material, the method for preparing the negative electrode composite material, and the negative electrode and lithium ion secondary battery containing the negative electrode composite material of the present invention can greatly reduce the amount of residual lithium, significantly improve the processing performance of the slurry, and improve the first coulombic efficiency and cycle performance of the lithium ion secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A photograph of the appearance of the negative electrode slurry in Comparative Example 4 is shown.
[0022] Figure 2 Li 1s XPS (X-ray photoelectron spectroscopy) spectra of the negative electrode composite materials in Examples 1-2, Comparative Examples 2 and 4 are shown. DETAILED DESCRIPTION
[0023] It should be noted that, in the absence of conflict, the various embodiments and features in the embodiments in this application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments. The following embodiments are merely exemplary and are not intended to limit the scope of protection of the present invention.
[0024] As described in the background art, in the prior art, the residual lithium content of the negative electrode material is too high, making it difficult to improve the processing performance of the slurry containing the negative electrode material and to effectively improve the first coulombic efficiency and cycle performance of the lithium-ion secondary battery. In view of the problems in the prior art, a typical embodiment of the present invention provides a negative electrode composite material, the negative electrode composite material includes negative electrode active material particles and Li2CO3 and LiOH on the surface of the negative electrode active material particles, the negative electrode active material particles include: particles containing silicon oxide and at least one lithium silicate selected from Li2SiO3 and Li2Si2O5; and a carbon coating layer coating at least a portion of the surface of the particles, based on the weight of the negative electrode active material particles, the content of Li2CO3 is greater than 0wt% and less than 0.01wt%, and the content of LiOH is greater than 0wt% and less than 0.01wt%.
[0025] A higher residual lithium value will affect the processing performance of the slurry containing the negative electrode composite material, resulting in the slurry being easily "jelly-like" in the process of preparing the slurry using the negative electrode composite material. After conducting a large number of experiments, the inventors of the present invention unexpectedly found that the present invention can achieve a great reduction in the amount of residual lithium and obtain a negative electrode composite material with an extremely low residual lithium amount. The negative electrode composite material of the present invention has an extremely low residual lithium amount, which can effectively avoid the slurry from "jellying" in the process of preparing the slurry using the negative electrode composite material, can significantly improve the processing performance of the slurry, and can improve the first coulombic efficiency and cycle performance of the lithium-ion secondary battery.
[0026] The silicon oxide of the present application may be silicon oxide conventionally used for negative electrode materials in the art. In some embodiments of the present invention, in the negative electrode composite material of the present invention, the silicon oxide may be SiO x , wherein 0.5≤x≤1.6, preferably 0.8≤x≤1.2, most preferably, x=1.0.
[0027] In some embodiments of the present invention, in the negative electrode composite material of the present invention, based on the weight of the negative electrode active material particles, the coating amount of the carbon coating layer is in the range of 1wt% to 30wt%, preferably, the coating amount of the carbon coating layer is in the range of 3wt% to 20wt%, and more preferably, the coating amount of the carbon coating layer is in the range of 5wt% to 10wt%. By controlling the coating amount of the carbon coating layer within the above range, a good balance can be obtained between the capacity of the material and the coating uniformity.
[0028] In some embodiments of the present invention, in the negative electrode composite material of the present invention, the carbon coating layer can cover the entire surface of the particles, thereby improving the conductivity of the negative electrode composite material, improving the first coulombic efficiency, more effectively reducing the amount of residual lithium, and improving the processing performance of the slurry.
[0029] In another typical embodiment of the present invention, a method for preparing a negative electrode composite material is provided, the method comprising: carbon-coating a silicon oxide precursor with a carbon source to form a carbon-coated silicon oxide; mixing the carbon-coated silicon oxide with a lithium source to form a first mixture, performing a first heat treatment on the first mixture to form a calcined product, and then performing a second heat treatment on the calcined product to form a pre-lithium product; and washing the pre-lithium product to form a negative electrode composite material.
[0030] The method for preparing the negative electrode composite material of the present invention can greatly reduce the amount of residual lithium, can effectively avoid the slurry from becoming "jelly" in the process of preparing the slurry using the negative electrode composite material, can significantly improve the processing performance of the slurry, can improve the first coulomb efficiency and cycle performance of the lithium ion secondary battery, and can inhibit the gas production of the slurry. The negative electrode composite material obtained by the above method according to the present invention has an extremely low amount of residual lithium, can significantly improve the processing performance of the slurry, can improve the first coulomb efficiency and cycle performance of the lithium ion secondary battery.
[0031] The silicon oxide precursor in the present invention, such as SiO x (wherein 0.5≤x≤1.6) can be prepared by conventional methods in the art. In some embodiments of the present invention, the silicon oxide precursor can be prepared by the following process: silicon powder and silicon dioxide of a certain particle size are mixed in a molar ratio of about 1.1:1, and then placed on a vibrator for about 12 hours to mix evenly, and about 1 kg of the above-mentioned substances mixed evenly are pressed into a block, and then the block is placed in a vacuum sublimation furnace and heated to a temperature of 1200°C-1500°C, and a block silicon oxide precursor is prepared by adjusting the vacuum degree to 0-30Pa, the heating time to 8h-10h, and the collection end temperature to 400°C-800°C, and the block silicon oxide precursor is placed in a crusher to be crushed to the millimeter level, and then the millimeter-level silicon oxide precursor is placed in an air flow mill for crushing, and powders of different particle sizes are separated by an air flow classifier, and finally the powders of different particle sizes are mixed with large and small particles, and finally the silicon oxide precursor of the desired particle size is obtained.
[0032] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, at a pressure of 50Pa-10000Pa and a temperature of 600°C-1000°C, chemical vapor deposition is performed on the surface of a silicon oxide precursor using at least one of alkanes, alkenes and alkynes as a carbon source to carbon-coat the silicon oxide precursor to form a carbon-coated silicon oxide. In some embodiments of the present invention, the carbon coating process can be performed in a rotary kiln, a fixed bed or a fluidized bed.
[0033] In some embodiments of the present invention, in the above-mentioned method for preparing a negative electrode composite material, the washing treatment includes mixing the pre-lithium product with water or acid, preferably at a solid content of 2wt%-10wt%, such as 2wt%-8wt% or 5wt%-10wt%, to form a second mixture, ultrasonically treating the second mixture, then dispersing it, then filtering it, and finally drying the filtered material. During the washing process, water can be used to dissolve alkaline substances such as Li2CO3 and LiOH, and acid can be used to neutralize the alkali generated on the surface of the pre-lithium product during washing; ultrasonic treatment can be used to wash the pre-lithium product more cleanly, ensuring a good washing effect, and improving the cycle performance of the lithium ion secondary battery. Through washing treatments such as water washing or acid washing, the amount of residual lithium can be greatly reduced, so that the amount of residual lithium in the negative electrode composite material is basically zero, which can effectively avoid the "jelly" of the slurry in the process of preparing the slurry using the negative electrode composite material, can significantly improve the processing performance of the slurry, and can further improve the first coulomb efficiency and cycle performance of the lithium ion secondary battery. By controlling the solid content within the above range, a sufficient amount of detergent for cleaning a unit mass of the pre-lithium product can be ensured, thereby ensuring a good cleaning effect.
[0034] In some embodiments of the present invention, the prepared pre-lithium product, such as pre-lithium SiO x The (0.5≤x≤1.6) material is mixed with water at a solid content of 2wt%-10wt% to form a second mixture, the second mixture is first ultrasonically treated for 10min-30min at room temperature, and then the second mixture is dispersed using a magnetic stirrer for 24h-72h, followed by suction filtration, and after suction filtration, pure water is poured on the material on the filter paper, and the material is washed twice in the form of suction filtration, and finally the filtered material is vacuum dried at 100℃-120℃ for 3-8 hours.
[0035] In some embodiments of the present invention, in the above-mentioned method for preparing a negative electrode composite material, in order to better neutralize the alkali generated on the surface of the pre-lithium product during washing, the acid is selected from at least one of hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid and boric acid.
[0036] In some embodiments of the present invention, the prepared pre-lithium product, such as pre-lithium SiO xThe (0.5≤x≤1.6) material is mixed with at least one of hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid and boric acid, such as citric acid with a concentration of 1 mol / L, at a solid content of 2wt%-10wt% to form a second mixture, the second mixture is first ultrasonically treated for 10min-30min at room temperature, and then the second mixture is dispersed for 24h-72h using a magnetic stirrer, followed by suction filtration, and after suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration, and finally the filtered material is vacuum dried at 100°C-120°C for 3-8 hours.
[0037] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the weight ratio of the lithium source to the carbon-coated silicon oxide is in the range of 5:95 to 15:85. By controlling the weight ratio of the lithium source to the carbon-coated silicon oxide within the above range, it is possible to ensure that the silicon oxide is fully pre-lithiated, the amount of residual lithium can be reduced, and the first coulombic efficiency and cycle performance of the lithium-ion secondary battery can be further improved. In some embodiments of the present invention, the lithium source may include any one of a lithium ingot, a lithium metal powder, and a lithium foil.
[0038] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the temperature of the first heat treatment is in the range of 500°C-750°C, and the time of the first heat treatment is in the range of 2h-5h. By controlling the temperature and time of the first heat treatment within the above range, it is beneficial to the lithium diffusion of the solid phase reaction, can ensure sufficient pre-lithiation of silicon oxide, can reduce the amount of residual lithium, and can further improve the first coulombic efficiency and cycle performance of the lithium ion secondary battery.
[0039] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the temperature for the second heat treatment is in the range of 925°C-1050°C, and the time for the second heat treatment is in the range of 3h-6h. By controlling the temperature for the second heat treatment within the above range, it is beneficial to the decomposition of Li2CO3 and LiOH (decomposition temperature is 924°C), and the decomposition product Li2O of Li2CO3 and LiOH begins to sublime above 1000°C, which is beneficial to greatly reduce the amount of residual lithium. By controlling the temperature and time for the second heat treatment within the above range, it can be ensured that the silicon oxide is fully pre-lithified, the amount of residual lithium can be greatly reduced, and the first coulombic efficiency and cycle performance of the lithium-ion secondary battery can be further improved.
[0040] In some embodiments of the present invention, under the protection of an inert atmosphere of argon, a lithium source and a carbon-coated silicon oxide are ground and mixed in a weight ratio of 5:95 to 15:85 to form a first mixture, and then the first mixture is placed in a rotary kiln, and calcined at 500°C-750°C for 2h-5h in an argon atmosphere to allow the carbon-coated silicon oxide to fully react with the lithium metal, and then heat treated at 925°C-1050°C for 3h-6h to obtain a pre-lithium product.
[0041] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the ultrasonic treatment time is in the range of 10 min-30 min. By controlling the ultrasonic treatment time in the above range, it is beneficial to clean the residual lithium in the pores, and the pre-lithium product can be washed more cleanly to ensure a good washing effect, while avoiding damage to the particles of the pre-lithium product and avoiding affecting the particle size distribution.
[0042] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, the time for dispersing can be controlled within the range of 24h-72h, mainly from the perspective of energy consumption, time cost and washing effect. If the time for dispersing is too short, it may not be washed cleanly, and if the time for dispersing is too long, the energy consumption and time cost are high. By controlling the time for dispersing within the above range, not only a good washing effect can be ensured, but also energy consumption and time cost can be reduced.
[0043] In some embodiments of the present invention, in the above method for preparing a negative electrode composite material, in order to better carbon-coat at least a portion of the surface of silicon oxide and obtain a good coating effect, the carbon source includes at least one of alkanes, alkenes and alkynes.
[0044] In another typical embodiment of the present invention, a negative electrode of a lithium ion secondary battery is provided, and the negative electrode of the lithium ion secondary battery comprises the negative electrode composite material described above. Since the negative electrode of the lithium ion secondary battery of the present invention comprises the negative electrode composite material described above, the amount of residual lithium can be reduced to a great extent, the processing performance of the slurry can be significantly improved, and the first coulombic efficiency and cycle performance of the lithium ion secondary battery can be improved.
[0045] The negative electrode sheet of the present invention can be fabricated by conventional methods in the art. For example, the negative composite material, conductive agent, and binder of the present invention can be dispersed in water as a solvent to form a uniform negative electrode slurry. The negative electrode slurry is coated on a negative electrode current collector and dried to obtain the negative electrode sheet. The conductive agent can be conductive carbon black, conductive graphite, vapor-grown carbon fiber, carbon nanotube, or any combination thereof. The binder can be one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyimide (PI), etc., and preferably the polyacrylic acid (PAA) binder.
[0046] In yet another typical embodiment of the present invention, a lithium-ion secondary battery is provided. The lithium-ion secondary battery includes a positive electrode, a negative electrode, and a separator. The negative electrode contains the negative composite material described above. Since the lithium-ion secondary battery of the present invention contains the negative composite material described above, the amount of residual lithium can be greatly reduced, the processing performance of the slurry can be significantly improved, and the first Coulombic efficiency and cycle performance of the lithium-ion secondary battery can be enhanced.
[0047] The positive electrode of the present invention includes a positive electrode current collector and a positive electrode active material layer containing a positive electrode active material. The positive electrode active material layer is formed on both surfaces of the positive electrode current collector. A metal foil such as aluminum foil, nickel foil, or stainless steel foil can be used as the positive electrode current collector.
[0048] The positive electrode active material layer contains one or more positive electrode materials capable of intercalating and deintercalating lithium ions as the positive electrode active material, and may contain additional materials such as a positive electrode binder and / or a positive electrode conductive agent when necessary.
[0049] Preferably, the positive electrode material is a lithium-containing compound. Examples of such lithium-containing compounds include lithium-transition metal composite oxides, lithium-transition metal phosphate compounds, and the like. The lithium-transition metal composite oxide is an oxide containing Li and one or more transition metal elements as constituent elements, and the lithium-transition metal phosphate compound is a phosphate compound containing Li and one or more transition metal elements as constituent elements. The transition metal elements are advantageously one or more of Co, Ni, Mn, Fe, etc.
[0050] Examples of the lithium-transition metal composite oxide can include, for example, LiCoO2 and LiNiO2, etc. Examples of the lithium-transition metal phosphate compound can include, for example, LiFePO4 and LiFe 1-u Mn u PO4(0 < u < 1), etc.
[0051] The negative electrode of the present invention includes a negative electrode current collector and a negative electrode active material layer containing a negative electrode composite material. The negative electrode active material layer is formed on both surfaces of the negative electrode current collector. Metal foil such as copper (Cu) foil, carbon-coated copper foil, nickel foil or stainless steel foil can be used as the negative electrode current collector.
[0052] The separator of the present invention is used to separate the positive electrode and the negative electrode in the battery, and to allow lithium ions to pass therethrough while preventing a current short circuit caused by contact between the positive electrode and the negative electrode. The separator is, for example, a porous film formed of a synthetic resin or ceramic, and may be a laminated film in which two or more porous films are laminated. Examples of synthetic resins include, for example, polytetrafluoroethylene, polypropylene, polyethylene, and the like.
[0053] In an embodiment of the present invention, when the lithium ion secondary battery is charged, for example, lithium ions are extracted from the positive electrode and embedded in the negative electrode through the electrolyte impregnated in the separator. When the lithium ion secondary battery is discharged, for example, lithium ions are extracted from the negative electrode and embedded in the positive electrode through the electrolyte impregnated in the separator.
[0054] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0055] Example 1
[0056] Preparation of negative electrode composite materials
[0057] At a pressure of 50 Pa and a temperature of 920 ° C, methane was used as a carbon source in 20 g of silicon oxide precursor SiO x The surface of the (x=1) material is subjected to chemical vapor deposition to deposit the silicon oxide precursor SiO x (x=1) material was subjected to carbon coating treatment to form 21 g of carbon-coated SiO x (x=1) material.
[0058] Under the protection of inert atmosphere argon, lithium ingots were mixed with carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 10:90 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 550°C for 3 h under an argon atmosphere to form a carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 925 °C for 3 h to obtain pre-lithium SiO x Material.
[0059] The prepared pre-lithium SiO xThe material and 1 mol / L hydrochloric acid at a solid content of 8 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 20 minutes at room temperature, and then dispersed for 48 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.
[0060] Preparation of negative electrode
[0061] Weigh 4 g of the negative electrode composite material prepared by the above process, and fully stir and mix the negative electrode composite material with conductive carbon black Super-P as a conductive agent and polyacrylic acid PAA as a binder in an appropriate amount of deionized water in a mass ratio of 82:8:10, and form a uniform negative electrode slurry by adjusting the solid content to 42 wt%, and then coat the negative electrode slurry on the surface of copper foil as a negative electrode collector, and obtain a negative electrode sheet after drying.
[0062] Battery Assembly
[0063] The prepared negative electrode sheet, separator, lithium sheet, gasket and battery shell are stacked in sequence and injected with 100 μl of electrolyte, and then sealed with a sealing machine to assemble the required half-cell.
[0064] Example 2
[0065] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 15:85 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600°C for 4 hours under an argon atmosphere to make the carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 1000 °C for 4 h to obtain pre-lithium SiO x Material;
[0066] The prepared pre-lithium SiO x The material and hydrochloric acid with a concentration of 1 mol / L are taken into a beaker with a solid content of 5 wt% and mixed to form a second mixture. The second mixture is first ultrasonically treated for 15 minutes at room temperature, and then dispersed for 36 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.
[0067] Example 3
[0068] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 500°C for 2 h in an argon atmosphere to make the carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 1050 °C for 6 h to obtain pre-lithium SiO x Material;
[0069] The prepared pre-lithium SiO x The material and hydrochloric acid with a concentration of 1 mol / L are taken into a beaker with a solid content of 2 wt% and mixed to form a second mixture. The second mixture is first ultrasonically treated for 30 minutes at room temperature, and then dispersed for 72 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.
[0070] Example 4
[0071] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 15:85 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750°C for 5 h under an argon atmosphere to form a carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 1025 °C for 4 h to obtain pre-lithium SiO x Material;
[0072] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 10 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 10 minutes at room temperature, and then dispersed for 24 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.
[0073] Example 5
[0074] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO xThe (x=1) materials were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 650°C for 2 h under an argon atmosphere to form a carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 1050 °C for 6 h to obtain pre-lithium SiO x Material;
[0075] The prepared pre-lithium SiO x The material and pure water are taken into a beaker with a solid content of 2wt% and mixed to form a second mixture. The second mixture is first ultrasonically treated for 30 minutes at room temperature, and then dispersed for 72 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.
[0076] Comparative Example 1
[0077] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 15:85 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750°C for 5 h under an argon atmosphere to form a carbon-coated SiO x The material fully reacts with lithium metal and then heat-treated at 775 °C for 4 h to obtain pre-lithium SiO x Material;
[0078] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 10 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is first ultrasonically treated for 10 minutes at room temperature, and then dispersed for 24 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120° C. for 8 hours to obtain a negative electrode composite material.
[0079] Comparative Example 2
[0080] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 2:98 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400°C for 2 h under an argon atmosphere to make the carbon-coated SiO xThe material fully reacts with lithium metal and then heat-treated at 950 °C for 7 h to obtain pre-lithium SiO x Material;
[0081] The prepared pre-lithium SiO x The material and hydrochloric acid with a concentration of 1 mol / L are taken into a beaker with a solid content of 20 wt% and mixed to form a second mixture. The second mixture is first ultrasonically treated for 10 minutes at room temperature, and then dispersed for 8 hours using a magnetic stirrer, followed by suction filtration. After suction filtration, pure water is poured on the material on the filter paper, and washed twice in the form of suction filtration. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.
[0082] Comparative Example 3
[0083] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 15:85 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600°C for 4 hours under an argon atmosphere to make the carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 1000 °C for 4 h to obtain pre-lithium SiO x Material;
[0084] The prepared pre-lithium SiO x The material and 1 mol / L hydrochloric acid at a solid content of 5 wt% are taken into a beaker and mixed to form a second mixture. The second mixture is dispersed for 36 hours using a magnetic stirrer at room temperature, and then filtered. After filtering, pure water is poured on the material on the filter paper, and washed twice in the form of filtering. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.
[0085] Comparative Example 4
[0086] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 10:90 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 550°C for 3 h under an argon atmosphere to form a carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 925 °C for 3 h to obtain pre-lithium SiO x Material;
[0087] No pre-lithiation of SiO xThe material is washed and the pre-lithium SiO x The material is used as a negative electrode composite material.
[0088] Comparative Example 5
[0089] The half-cell was prepared in the same manner as in Example 1, except that the lithium ingot and the carbon-coated SiO x The (x=1) materials were ground and mixed in a weight ratio of 30:70 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600°C for 5 h in an argon atmosphere to make the carbon-coated SiO x The material reacts fully with lithium metal and then heat-treated at 820 °C for 2 h to obtain pre-lithium SiO x Material;
[0090] The prepared pre-lithium SiO x The material and pure water are taken into a beaker with a solid content of 5wt% and mixed to form a second mixture. The second mixture is dispersed at room temperature for 48 hours using a magnetic stirrer, and then filtered. After filtering, pure water is poured on the material on the filter paper, and washed twice in the form of filtering. Finally, the filtered material is vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.
[0091] Material property testing
[0092] The negative electrode composite materials in Examples 1-5 and Comparative Examples 1-5 were tested to obtain the results of the content of Li 2 CO 3 and the content of LiOH.
[0093] Neutralization titration method: The negative electrode composite material and pure water are measured in a mass ratio of 1:9 into a beaker and mixed. The negative electrode composite material is dispersed for 1 hour using a magnetic stirrer at room temperature, and the dispersion is allowed to stand for 1 hour. The dispersion is filtered. The obtained 10 mL filtrate is automatically titrated with 0.2 M hydrochloric acid using an acid-base automatic titrator, and the first endpoint (a mL) and the second endpoint (b mL) are obtained.
[0094] Li2CO3 content = [pure water amount (g) / filtrate amount (g)] × 2 × (b / 1000) × (hydrochloric acid titration equivalent concentration × coefficient) × (1 / 2) × (Li2CO3 molar mass) × [100 (%) / sample amount (g)]
[0095] LiOH content = [amount of pure water (g) / amount of filtrate (g)] × [(ab) / 1000] × (equivalent concentration of hydrochloric acid titration × coefficient) × (1 / 2) × (molar mass of LiOH) × [100 (%) / sample amount (g)].
[0096] Battery performance test
[0097] The half-cells in Examples 1-5 and Comparative Examples 1-5 were subjected to charge and discharge tests at a voltage between 0V and 1.5V at 25°C. The half-cells in the above-mentioned Examples and Comparative Examples were first subjected to a cycle test at 25°C with a charge and discharge current of 0.1C for one time (the charge and discharge voltage range was 0V-1.5V) to determine the initial discharge capacity and initial coulombic efficiency of the battery. The battery was then subjected to a charge and discharge cycle test 50 times with a current of 1C (the charge and discharge cut-off voltage was 0V-1.5V) to determine the capacity retention rate of the battery after 50 cycles. Initial coulombic efficiency (%) = initial discharge capacity / initial charge capacity × 100%. The experimental results are shown in Tables 1 and Figure 1-2 Shown in.
[0098] Table 1 Material properties and electrochemical performance test results
[0099]
[0100] It can be seen from the above test results that the above embodiments of the present invention achieve the following technical effects:
[0101] By comparing the results of Examples 1-5 with Comparative Examples 1-5, it can be seen that the batteries in Examples 1-5, in which the content of Li2CO3 based on the weight of the negative electrode active material particles and the content of LiOH are not within the scope of the present invention, have a higher first coulombic efficiency and a higher discharge capacity retention rate after 50 cycles, compared with Comparative Examples 1-5 in which the content of Li2CO3 based on the weight of the negative electrode active material particles and the content of LiOH are not within the scope of the present invention.
[0102] Figure 2 The Li 1s XPS (X-ray photoelectron spectroscopy) spectra of the negative electrode composite materials in Examples 1-2, Comparative Examples 2 and Comparative Examples 4 are shown. The XPS spectra show the comparison of the amount of lithium carbonate Li2CO3 as one of the residual lithium components in the negative electrode composite materials of Examples 1-2, Comparative Examples 2 and Comparative Examples 4. Figure 2 It can be seen that there is no Li2CO3 peak in the XPS spectrum of the negative electrode composite material in Example 1-2. This indicates that the amount of Li2CO3 in the negative electrode composite material of Example 1-2 does not meet the amount required by the XPS test.
[0103] By comparing the results of Example 1 with those of Comparative Example 4, it can be seen that by xBy washing the material, a negative electrode composite material with extremely low Li2CO3 content and extremely low LiOH content can be obtained, which can greatly reduce the amount of residual lithium, significantly improve the processing performance of the slurry, and improve the battery's first discharge capacity, first coulomb efficiency and discharge capacity retention rate after 50 cycles. Figure 1 The following is a photograph of the appearance of the negative electrode slurry in Comparative Example 4. Figure 1 It can be seen that since the negative electrode composite material in Comparative Example 4 has a high amount of residual lithium, the negative electrode slurry has become jelly-like.
[0104] By comparing the results of Example 2 with those of Comparative Example 3, it can be seen that when the washing treatment includes ultrasonic treatment of the second mixture, a negative electrode composite material having an extremely low Li2CO3 content and an extremely low LiOH content can be obtained, the amount of residual lithium can be reduced, the processing performance of the slurry can be significantly improved, and the battery's first discharge capacity, first coulombic efficiency and discharge capacity retention rate after 50 cycles can be improved.
[0105] By comparing the results of Example 4 with those of Comparative Example 1, it can be seen that when the temperature of the second heat treatment is in the range of 925°C-1050°C, a negative electrode composite material with extremely low Li2CO3 content and extremely low LiOH content can be obtained, the amount of residual lithium can be reduced, the processing performance of the slurry can be significantly improved, and the battery's first discharge capacity, first coulombic efficiency and discharge capacity retention rate after 50 cycles can be improved.
[0106] It can be seen from the above battery performance test results that the negative electrode composite material of the present invention, the method for preparing the negative electrode composite material, and the negative electrode and lithium ion secondary battery containing the negative electrode composite material can greatly reduce the amount of residual lithium, significantly improve the processing performance of the slurry, and improve the first coulombic efficiency and cycle performance of the lithium ion secondary battery.
[0107] The above description is only the preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A negative electrode composite material, characterized in that: The negative electrode composite material comprises negative electrode active material particles and Li2CO3 and LiOH on the surface of the negative electrode active material particles, and the negative electrode active material particles comprise: Particles comprising silicon oxide and at least one lithium silicate selected from Li2SiO3 and Li2Si2O5; and a carbon coating layer covering at least a portion of the surface of the particle, Based on the weight of the negative electrode active material particles, the content of Li 2 CO 3 is greater than 0 wt % and less than 0.01 wt %, and the content of LiOH is greater than 0 wt % and less than 0.01 wt %.
2. The negative electrode composite material according to claim 1, characterized in that: The silicon oxide is SiO x , where 0.5≤x≤1.
6.
3. The negative electrode composite material according to claim 1 or 2, characterized in that: The coating amount of the carbon coating layer is in a range of 1 wt % to 30 wt % based on the weight of the negative electrode active material particles.
4. The negative electrode composite material according to claim 1 or 2, characterized in that: The carbon coating layer covers the entire surface of the particle.
5. A method for preparing a negative electrode composite material, characterized in that: The method comprises: Performing carbon coating treatment on a silicon oxide precursor using a carbon source to form carbon-coated silicon oxide; mixing the carbon-coated silicon oxide with a lithium source to form a first mixture, subjecting the first mixture to a first heat treatment to form a calcined product, and then subjecting the calcined product to a second heat treatment to form a pre-lithium product; and The pre-lithium product is washed to form the negative electrode composite material.
6. The method for preparing a negative electrode composite material according to claim 5, characterized in that: The washing treatment includes mixing the pre-lithium product with water or acid, preferably at a solid content of 2wt%-10wt%, to form a second mixture, ultrasonically treating the second mixture, then dispersing it, then filtering it, and finally drying the filtered material.
7. The method for preparing a negative electrode composite material according to claim 6, characterized in that: The acid is selected from at least one of hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid and boric acid.
8. The method for preparing a negative electrode composite material according to claim 5, characterized in that: A weight ratio of the lithium source to the carbon-coated silicon oxide is in a range of 5:95 to 15:
85.
9. The method for preparing a negative electrode composite material according to claim 5, characterized in that: The temperature for performing the first heat treatment is in the range of 500° C.-750° C., and the time for performing the first heat treatment is in the range of 2 h-5 h.
10. The method for preparing a negative electrode composite material according to claim 5, characterized in that: The temperature for performing the second heat treatment is in the range of 925° C.-1050° C., and the time for performing the second heat treatment is in the range of 3 h-6 h.
11. The method for preparing a negative electrode composite material according to claim 6, characterized in that: The ultrasonic treatment is performed for a period of 10 min to 30 min.
12. The method for preparing a negative electrode composite material according to claim 6, characterized in that: The dispersion is carried out for a period of time ranging from 24h to 72h.
13. The method for preparing a negative electrode composite material according to claim 5, characterized in that: The carbon source includes at least one of alkanes, alkenes and alkynes.
14. A negative electrode for a lithium ion secondary battery, characterized in that: The negative electrode of the lithium ion secondary battery comprises the negative electrode composite material according to any one of claims 1 to 4.
15. A lithium ion secondary battery, characterized in that: The lithium-ion secondary battery comprises: positive electrode, The negative electrode, and Diaphragm, Characterized in that the negative electrode comprises the negative electrode composite material according to any one of claims 1 to 4.