Negative electrode material, electrochemical device, and electronic device

By using a negative electrode material that combines a carbon layer and a silicon layer in a lithium-ion battery, combined with the optimization of carbon nanomaterials, the problem of easy breakage of the negative electrode material is solved, and the cycle stability and power performance of the lithium-ion battery are significantly improved.

CN118738308APending Publication Date: 2024-10-01ENVISION DYNAMICS TECH (JIANGSU) CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310335059.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing lithium-ion battery anode materials are easily broken during the production and long-term cycling process of lithium-ion batteries, resulting in poor cycle performance.

Method used

Using a negative electrode material that combines a carbon layer and a silicon layer, by controlling the range of the crushing coefficient Y ≤ 40% and the pore utilization rate R, combined with the use of carbon nanomaterials, a negative electrode plate with excellent cycle stability and power performance is formed.

Benefits of technology

Significantly improves the cycle stability and power performance of lithium-ion batteries and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of secondary batteries, and particularly relates to a negative electrode material, an electrochemical device and an electronic device. The negative electrode material comprises: a carbon layer; the silicon layer is positioned on at least part of the surface of the carbon layer. The negative electrode material meets the following relations: Y is less than or equal to 40%; y is the crushing coefficient of the negative electrode material, and Y meets the following relation: Y = (D2-D1) / D2 * 100%; in the formula, D2 is the particle size corresponding to 10% of the accumulated particle size distribution number of the negative electrode material before powder pressing treatment, the unit is [mu] m, D1 is the particle size corresponding to 10% of the accumulated particle size distribution number of the negative electrode material after powder pressing treatment, and the unit is [mu] m. The crushing coefficient Y of the negative electrode material is limited in a specific range (the crushing coefficient Y is less than or equal to 40%), so that the cycle performance and the power performance of an electrochemical device made of a negative electrode piece formed by the negative electrode material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to negative electrode materials, electrochemical devices and electronic devices. Background Art

[0002] Compared with lead-acid batteries and nickel-metal hydride batteries, lithium-ion batteries have higher specific capacity, and they also have the advantages of high output voltage, high energy density, good safety, long cycle life, and environmental protection. Therefore, lithium-ion batteries gradually replace lead-acid batteries and nickel-metal hydride batteries and become the first choice for electric vehicle batteries. In recent years, the rapid development of small energy storage for electronic equipment, electric vehicle power batteries, and large-scale energy storage for power grids has put forward higher requirements for the energy density and cycle life of lithium-ion batteries.

[0003] Generally, lithium-ion batteries are mainly composed of positive electrodes, separators, electrolytes and negative electrodes. Among them, the positive electrode material, which accounts for about 40% of the battery cell cost, and the negative electrode material, which accounts for about 30% of the battery cell cost, have a crucial impact on the performance of lithium-ion batteries. In practical applications, carbon materials such as graphite are generally used as negative electrode materials. However, the specific capacity of graphite negative electrode materials is relatively low. Studies have shown that silicon is currently the negative electrode material with the largest theoretical specific capacity. Its theoretical specific capacity is much higher than that of graphite. In addition, silicon has a low lithium insertion potential and low cost. Silicon is expected to replace graphite as one of the next generation of lithium-ion battery negative electrode materials.

[0004] However, during the lithium insertion and extraction process, the short Si-Si covalent bond is replaced by the longer Li-Si bond, which causes a huge volume expansion. The series of problems caused by the volume expansion of silicon during lithium insertion and extraction and its low conductivity characteristics limit its large-scale practical application.

[0005] At present, the above-mentioned volume expansion and low conductivity problems are generally solved by depositing silicon on the surface of a porous carbon substrate. However, the negative electrode plates made of the composite materials obtained in this way are easily broken during the lithium-ion battery manufacturing process and long-cycle processes, resulting in poor cycle performance of the lithium-ion battery. Summary of the invention

[0006] The present invention provides negative electrode materials, electrochemical devices and electronic devices to solve the technical problem that negative electrode plates made of composite materials obtained by the above-mentioned existing methods are easily broken during the lithium ion battery manufacturing process and long cycle process, resulting in poor cycle performance of lithium ion batteries.

[0007] In order to solve the above technical problems, in a first aspect, the present application provides a negative electrode material, the negative electrode material comprising: a carbon layer; and a silicon layer located on at least a portion of the surface of the carbon layer, the negative electrode material satisfies the following relationship:

[0008] Y≤40%;

[0009] Y is the crushing coefficient of the negative electrode material, wherein Y satisfies the following relationship:

[0010] Y = (D2 - D1) / D2 × 100%;

[0011] Wherein, D2 is the particle size corresponding to 10% of the cumulative particle size distribution number of the negative electrode material before powder pressing treatment, in μm, and D1 is the particle size corresponding to 10% of the cumulative particle size distribution number of the negative electrode material after powder pressing treatment, in μm.

[0012] In the present invention, the electrochemical device made of the negative electrode sheet formed by the negative electrode material having the above-mentioned specific selected technical characteristics (the crushing coefficient Y satisfies the following formula: Y≤40%) has excellent cycle stability and excellent power performance.

[0013] In the present invention, if the crushing coefficient Y>40%, the electrochemical device made of the negative electrode sheet formed by the negative electrode material has poor cycle stability and poor power performance.

[0014] In some embodiments, the negative electrode material satisfies the following relationship:

[0015] Y≤25%.

[0016] In some embodiments, the negative electrode material satisfies the following relationship:

[0017] Y≤10%.

[0018] In some embodiments, the powder pressing treatment includes: increasing the pressure to 150 MPa at a pressure increasing rate of 3 MPa / min, and then maintaining the pressure at 150 MPa for 20 minutes.

[0019] In some embodiments, the negative electrode material satisfies the following relationship:

[0020] 30%≤R≤70%;

[0021] Wherein, R is the porosity utilization rate of the negative electrode material, and R satisfies the following relationship:

[0022] R=[m×P / 2.21] / [1-m×n / 2.25]×100%;

[0023] Wherein, m is the true density of the negative electrode material, in g / cm 3 , n and P are the mass percentages of carbon and silicon in the negative electrode material, respectively, in wt%.

[0024] In some embodiments, the negative electrode material satisfies the following relationship:

[0025] 30%≤R≤60%.

[0026] In some embodiments, the carbon layer further includes carbon-containing nanomaterials, and the carbon-containing nanomaterials include carbon nanofibers (CNF for short in English), carbon nanotubes (CNT for short in English), or a mixture of the two.

[0027] In some embodiments, the carbon nanofibers have a diameter of 5-30 nm, preferably 5-25 nm.

[0028] In some embodiments, the diameter of the carbon nanotubes is 5-30 nm, preferably 5-25 nm.

[0029] In some embodiments, the aspect ratio of the carbon nanofibers is 10:1-100:1, preferably 10:1-50:1.

[0030] In some embodiments, the aspect ratio of the carbon nanotubes is 10:1-100:1, preferably 10:1-50:1.

[0031] In some embodiments, based on the mass of the carbon layer, the mass of the carbon-containing nanomaterial is 0.05 wt %-2 wt %, preferably 1 wt %-5 wt %.

[0032] In some embodiments, the silicon layer includes a silicon substrate, and the silicon substrate is silicon, silicon oxide, or a mixture of the two.

[0033] In a second aspect, the present invention further provides an electrochemical device, comprising a negative electrode plate, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector, wherein the negative electrode active material layer comprises the negative electrode material as described above.

[0034] In a third aspect, the present application provides an electronic device comprising the electrochemical device as described above. DETAILED DESCRIPTION

[0035] The present invention is further described below through specific examples, but it should be pointed out that the specific material ratios, process conditions and results described in the embodiments of the present invention are only used to illustrate the present invention and cannot be used to limit the scope of protection of the present invention. All equivalent changes or modifications made according to the spirit of the present invention should be included in the scope of protection of the present invention.

[0036] The present invention provides a negative electrode material, which includes: a carbon layer; and a silicon layer located on at least a portion of the surface of the carbon layer, and the negative electrode material satisfies the following relationship:

[0037] Y≤40%;

[0038] Y is the crushing coefficient of the negative electrode material, where Y satisfies the following relationship:

[0039] Y = (D2 - D1) / D2 × 100%;

[0040] Wherein, D2 is the particle size corresponding to 10% of the cumulative particle size distribution of the negative electrode material before powder pressing treatment, in μm; D1 is the particle size corresponding to 10% of the cumulative particle size distribution of the negative electrode material after powder pressing treatment, in μm;

[0041] In the present invention, the electrochemical device made of the negative electrode sheet formed by the negative electrode material having the above-mentioned specific selected technical characteristics (the crushing coefficient Y satisfies the following formula: Y≤40%) has excellent cycle stability and excellent power performance. If the crushing coefficient Y>40%, the electrochemical device made of the negative electrode sheet formed by the negative electrode material has poor cycle stability and poor power performance.

[0042] In some embodiments, the negative electrode material satisfies the following relationship:

[0043] Y≤25%.

[0044] In the present invention, if the crushing coefficient Y is ≤25%, the cycle stability and power performance of the lithium-ion battery made of the negative electrode sheet formed by the negative electrode material can be further improved.

[0045] In some embodiments, the negative electrode material satisfies the following relationship:

[0046] Y≤10%.

[0047] In the present invention, if the crushing coefficient Y is ≤10%, the cycle stability and power performance of the lithium-ion battery made of the negative electrode sheet formed by the negative electrode material can be further improved.

[0048] In some embodiments, the powder pressing treatment includes: increasing the pressure to 150 MPa at a pressure increasing rate of 3 MPa / min, and then maintaining the pressure at 150 MPa for 20 minutes.

[0049] In some embodiments, the negative electrode material satisfies the following relationship:

[0050] 30%≤R≤70%;

[0051] Wherein, R is the porosity utilization rate of the negative electrode material, and R satisfies the following relationship:

[0052] R=[m×P / 2.21] / [1-m×n / 2.25]×100%;

[0053] Where m is the true density of the negative electrode material, in g / cm 3 , n and P are the mass percentages of carbon and silicon in the negative electrode material, respectively, in wt%.

[0054] In the present invention, if the pore utilization rate R satisfies the following relationship: 30%≤R≤60, the cycle stability and power performance of the lithium-ion battery made of the negative electrode sheet formed by the negative electrode material can be further improved.

[0055] In some embodiments, the negative electrode material satisfies the following relationship:

[0056] 30%≤R≤60%.

[0057] In the present invention, if the pore utilization rate R satisfies the following relationship: 30%≤R≤60, the cycle stability and power performance of the lithium-ion battery made of the negative electrode sheet formed by the negative electrode material can be further improved.

[0058] In some embodiments, the carbon layer further includes carbon-containing nanomaterials, and the carbon-containing nanomaterials include carbon nanofibers (CNF for short in English), carbon nanotubes (CNT for short in English), or a mixture of the two.

[0059] In some embodiments, the carbon nanofibers have a diameter of 5-30 nm, preferably 5-25 nm.

[0060] In some embodiments, the carbon nanotubes have a diameter of 5-30 nm, preferably 5-25 nm.

[0061] In the present invention, the carbon nanofibers, carbon nanotubes or a mixture of the above-mentioned specific diameter (5-30nm) can form a skeleton structure, thereby improving the strength of the negative electrode material and improving the cycle stability of the electrochemical device made of the negative electrode sheet formed by the negative electrode material. If the diameter is greater than 30nm, the strength of the negative electrode material is poor, resulting in poor cycle performance of the electrochemical device made of the negative electrode sheet formed therefrom. If the diameter is less than 5nm, the carbon-containing nanomaterial is not easy to disperse, and the structural strength of the negative electrode material is insufficient, resulting in poor cycle performance of the electrochemical device made of the negative electrode sheet formed therefrom.

[0062] In some embodiments, the aspect ratio of the carbon nanofibers is 10:1-100:1, preferably 10:1-50:1.

[0063] In some embodiments, the aspect ratio of the carbon nanotubes is 10:1-100:1, preferably 10:1-50:1.

[0064] In the present invention, if the aspect ratio is greater than 100:1, the dispersion of the carbon-containing nanomaterial is poor, which is not conducive to the formation of the skeleton structure, resulting in poor strength of the negative electrode material, resulting in poor cycle performance of the electrochemical device made of the negative electrode sheet formed therefrom. If the aspect ratio is less than 10:1, the purpose of structural strengthening cannot be achieved, resulting in poor cycle performance of the electrochemical device made of the negative electrode sheet formed therefrom.

[0065] In some embodiments, based on the mass of the carbon layer, the mass of the carbon-containing nanomaterial is 0.05 wt %-2 wt %, preferably 1 wt %-2 wt %.

[0066] In the present invention, based on the mass of the carbon layer, if the mass of the carbon-containing nanomaterial is greater than 2wt%, the dispersion of the carbon-containing nanomaterial is poor, which is not conducive to the formation of the skeleton structure, resulting in poor strength of the negative electrode material, resulting in poor cycle performance of the electrochemical device made of the negative electrode sheet formed therefrom. Based on the mass of the carbon layer, if the mass of the carbon-containing nanomaterial is less than 0.05wt%, the purpose of structural reinforcement cannot be achieved, resulting in poor cycle performance of the electrochemical device made of the negative electrode sheet formed therefrom.

[0067] In some embodiments, the silicon layer includes a silicon substrate, which is silicon, silicon oxide, or a mixture of the two.

[0068] In a second aspect, the present invention further provides an electrochemical device, which includes a negative electrode plate, wherein the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector, wherein the negative electrode active material layer includes the negative electrode material as described above.

[0069] The electrochemical device of the present application includes any device in which an electrochemical reaction occurs, and its specific examples include all kinds of primary batteries, secondary batteries, fuel cells, solar cells or capacitors. The electrochemical device is a sodium metal battery, and the battery includes at least one of a soft pack, a square aluminum shell, a square steel shell, a cylindrical aluminum shell and a cylindrical steel shell battery.

[0070] The following description will only take lithium-ion secondary batteries as an example.

[0071] The negative electrode sheet can be obtained by mixing a negative electrode material and a binder (if necessary) in a solvent to obtain a negative electrode material composition, and coating the negative electrode material composition on a negative electrode current collector.

[0072] As the negative electrode current collector, it can be copper foil, nickel foil, stainless steel foil, titanium foil, foamed nickel, foamed copper, a polymer substrate coated with a conductive metal, or a combination thereof.

[0073] As for the above-mentioned lithium-ion battery, it can be obtained by stacking the positive electrode sheet and the negative electrode sheet on each other, and separating the positive electrode sheet and the negative electrode sheet by a diaphragm with a porous structure (if necessary) (the pores of the diaphragm are evenly distributed in the entire diaphragm). Specifically, the stacked body formed by the positive electrode sheet, the diaphragm (if necessary) and the negative electrode sheet is immersed in the electrolyte, that is, the electrolyte is filled in the entire battery body. In other words, the electrolyte is filled between the positive electrode sheet, the negative electrode sheet and the diaphragm, and also filled in the pores of the diaphragm. It should be understood that the diaphragm is not a necessary component, and in certain specific types of lithium-ion batteries, a diaphragm may not be required.

[0074] As for the above-mentioned lithium-ion battery, there is no limitation on its structure. For example, the positive electrode plate, the separator (if necessary) and the negative electrode plate can be stacked on each other and then wound into a flat spiral to form a wound electrode plate group, or the positive electrode plate, the separator (if necessary) and the negative electrode plate can be stacked on each other to form a flat electrode plate group, and then the electrode plate group can be assembled into a casing (if necessary).

[0075] The shape of the lithium ion battery is not limited in any way, and examples thereof include paper-shaped, button-shaped, coin-shaped, laminated, cylindrical, and square-shaped batteries.

[0076] As for the above-mentioned positive electrode sheet, it includes a positive electrode current collector and a positive electrode slurry layer located on the positive electrode current collector, wherein the positive electrode current collector can be made of copper foil, stainless steel foil, titanium foil or a combination thereof.

[0077] As for the positive electrode slurry layer, it includes positive electrode materials, and the positive electrode materials can be porous carbon, lithium manganese oxide (LiMnO2), lithium cobalt oxide (LiCoO2), lithium dichromate (Li2Cr2O7), lithium chromate (Li2CrO4), lithium nickel oxide (LiNiO2), lithium ferrite (LiFeO2), lithium nickel cobalt composite oxide (such as LiNi x Co 1-x O2, 0<x<1; such as LiNi x Co y Mn z O2, x+y+z=1), phosphate complex salt (LiMPO4, M is iron, manganese, cobalt, nickel, etc.), lithium nickel manganese oxide (LiMn 0.5 Ni 0.5 O2), spinel (such as LiMn2O4; such as LiMc 0.5 Mn 1.5 O4, Mc is a divalent metal), polyacetylene, polyphenylene, polypyrrole, polythiophene, polyacene and the like.

[0078] There is no limitation on the material of the above-mentioned diaphragm, and examples thereof include polyethylene (PE), polypropylene (PP), polytetrafluoroethylene film, polyamide film, polyvinyl chloride film, polyvinyl difluoride film, polyaniline film, polyimide film, nonwoven fabric, polyethylene terephthalate, polystyrene (PS), cellulose or a combination thereof.

[0079] As for the above-mentioned electrolyte, its main components are organic solvents and lithium salts. Among them, the organic solvent can be listed as ethylene carbonate, propylene carbonate, butylene carbonate, ethylene carbonate (EC), vinylene carbonate, propylene carbonate (PC), diethyl carbonate (DEC), propyl acetate (PA), dimethyl carbonate (DMC), diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, butyl ethyl carbonate, methyl acetate, ethyl acetate, butyl lactone (γ-butyrolactone, GBL), cyclopentanone, sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane and other substances. Examples of lithium salts include lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium hexafluoroantimonate (LiSbF6), lithium perchlorate (LiClO4), lithium tetrafluoroaluminate (LiAlCl4), tetrachlorogallate (LiGaCl4), lithium nitrate (LiNO3), tris-(trifluoromethylsulfonyl)methyllithium (LiC(SO2CF3)3), bis-(trifluoromethylsulfonyl)imide lithium (LiN(SO2CF3)2), lithium thiocyanate (LiSCN), lithium trifluoromethylsulfonate (LiO3SCF2CF3), lithium fluorosulfonate (LiSO3F), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(oxalatoborate) (LiB(C2O4)2), LiC6F5SO3, LiO2CCF3, LiB(C6H5)4 and the like.

[0080] The present application provides an electronic device, which includes the electrochemical device as described above.

[0081] The use of the electrochemical device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the electrochemical device of the present application can be used for, but not limited to, laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries, energy storage and sodium ion capacitors, etc.

[0082] The present invention is described in detail below by specific examples. It should also be understood that the following examples are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0083] Example 1

[0084] This embodiment provides a negative electrode material, which is prepared according to the following steps:

[0085] A. Dissolve phenolic resin and polyethylene glycol in anhydrous ethanol in turn and mix them evenly, and add carbon-containing nanomaterials (specifically carbon nanotube CNT powder with a diameter of 20 nm and an aspect ratio of 30:1), the mass ratio of phenolic resin, polyethylene glycol and carbon-containing nanomaterials is 90:9:1, the mass ratio of the total mass of phenolic resin, polyethylene glycol and carbon-containing nanomaterials to anhydrous ethanol is 1:10, and add 0.1wt% of the mass of anhydrous ethanol as dispersant K30 and ultrasonically disperse for 3h; transfer to a 60°C oven and heat for 4h, dry the solvent, transfer to a box-type resistance furnace, and cure at a constant temperature of 130°C for 3h. After curing, cool to room temperature and crush;

[0086] B. The solid prepared in step A is transferred to a box-type resistance furnace, heated to 800° C. in a nitrogen atmosphere, and kept at this temperature for 2 h for carbonization, and the carbonized product is further crushed to obtain a carbon material;

[0087] C. Add 5 kg of the carbon material prepared in step B into the deposition chamber, and introduce inert gas argon to expel the original air so that the reaction chamber is filled with argon, and heat to the reaction temperature of 500°C, and introduce monosilane, ethylene and protective atmosphere gas (composed of argon and hydrogen) into the vacuum reaction chamber formed in step a); perform chemical vapor deposition for 4 hours, so that carbon and silicon are co-deposited on the carbon substrate to obtain a silicon-carbon composite material; wherein the flow rate of monosilane is 1 L / min, the flow rate of ethylene is 1 L / min, the flow rate of argon is 0.8 L / min, and the flow rate of hydrogen is 0.82 L / min.

[0088] Example 2

[0089] The difference between this embodiment and embodiment 1 is that the mass ratio of phenolic resin, polyethylene glycol and carbon-containing nanomaterial is 90:7:3.

[0090] Example 3

[0091] The difference between this embodiment and embodiment 1 is that the mass ratio of phenolic resin, polyethylene glycol and carbon-containing nanomaterial is 90:6:4.

[0092] Example 4

[0093] The difference between this embodiment and embodiment 2 is that the carbon-containing nanomaterial is carbon nanofiber CNF with a diameter of 20 nm and an aspect ratio of 30:1, and the mass ratio of phenolic resin, polyethylene glycol, and carbon-containing nanomaterial is 90:7:3.

[0094] Comparative Example 1

[0095] The difference between this comparative example and Example 1 is that no carbon-containing nanomaterial is added, and the mass ratio of phenolic resin to polyethylene glycol is 90:10.

[0096] Comparative Example 2

[0097] The difference between this comparative example and Example 1 is that the carbon-containing nanomaterial is carbon nanotube CNT powder, and the mass ratio of phenolic resin, polyethylene glycol and carbon-containing nanomaterial is 90:5:5.

[0098] Comparative Example 3

[0099] The difference between this comparative example and Example 1 is that in step C, the deposition time is 8 hours.

[0100] Comparative Example 4

[0101] The difference between this comparative example and Example 1 is that in step C, the deposition time is 2 hours.

[0102] Comparative Example 5

[0103] The difference between this comparative example and Example 1 is that in step A, the diameter of the carbon nanotube CNT powder is 40 nm, and the aspect ratio is 150:1.

[0104] Comparative Example 6

[0105] The difference between this comparative example and Example 1 is that in step A, the diameter of the carbon nanotube CNT powder is 3 nm, and the aspect ratio is 8:1.

[0106] test

[0107] The crushing coefficient Y, powder conductivity and pore utilization rate R of the negative electrode materials of Examples 1-4 and Comparative Examples 1-6 were tested, and the results are shown in Table 1;

[0108] The crushing coefficient Y test steps are as follows: first, use a particle size tester to measure the particle size D2 corresponding to the cumulative particle size distribution number of the negative electrode material before powder pressing treatment reaches 10%; then take 10g of the negative electrode material, use a powder automatic compaction density meter, and perform powder pressing treatment on it, specifically: increase the pressure to 150Mpa at a pressure increase rate of 3MPa / min, then maintain the pressure at 150MPa for 20min, take out the powder after the powder pressing treatment, use a particle size tester to measure the particle size D1 corresponding to the cumulative particle size distribution number of the negative electrode material after the powder pressing treatment reaches 10%, and then calculate the crushing coefficient Y according to formula (1):

[0109] Y = (D2 - D1) / D2 × 100% (1);

[0110] Wherein, D2 is the particle size corresponding to 10% of the cumulative particle size distribution number of the negative electrode material before powder pressing treatment, in μm, and D1 is the particle size corresponding to 10% of the cumulative particle size distribution number of the negative electrode material before powder pressing treatment, in μm;

[0111] The conductivity of the powder is tested using a four-probe conductivity meter;

[0112] The test method of the porosity utilization rate R is as follows: firstly test the true density, silicon element mass percentage n and carbon element mass percentage P of the negative electrode material, wherein the true density is tested by a powder true density meter, and the silicon element mass percentage n and carbon element mass percentage P are obtained by elemental analysis test using an inductively coupled plasma-emission spectrometer, and then calculate the porosity utilization rate R according to formula (2):

[0113] R=[m×P / 2.21] / [1-m×n / 2.25]×100% (2);

[0114] Where m is the true density of the negative electrode material, in g / cm 3 , n and P are the mass percentages of carbon and silicon in the negative electrode material, respectively, in wt%.

[0115] The negative electrode materials of Examples 1-4 and Comparative Examples 1-6 were respectively made into lithium-ion batteries, and the specific steps were as follows:

[0116] Preparation of positive electrode sheet: The positive electrode material NCM (i.e. LiNi 0.8 Co 0.1 Mn 0.1O2), conductive agent high conductive carbon black Super P and binder polyvinylidene fluoride (English abbreviation PVDF) are mixed in a mass ratio of 97:1.5:1.5, solvent N-methylpyrrolidone (NMP) is added to the mixture, the mass ratio of N-methylpyrrolidone (NMP) to positive electrode material NCM811 is 1:1, and the mixture is fully stirred to obtain positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector aluminum foil, and the positive electrode sheet is obtained through drying, cold pressing, slitting and other processes.

[0117] Preparation of negative electrode sheets: negative electrode material, conductive agent acetylene black, thickener sodium carboxymethyl cellulose (CMC) and binder styrene butadiene latex (SBR) are mixed in a mass ratio of 96.4:1:1.2:1.4, and deionized water is added as solvent, with the mass ratio of deionized water to sample being 2:1. The mixture is stirred and mixed thoroughly to obtain negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil, and the negative electrode sheet is prepared through processes such as drying, cold pressing and slitting.

[0118] Preparation of electrolyte

[0119] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain a solvent, and then fully dried lithium salt LiPF6 is dissolved in the solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0120] Diaphragm: A polyethylene porous membrane with a thickness of 11 um, an air permeability of 280 s / 100 mL and a porosity of 40% is used as the diaphragm;

[0121] Preparation of lithium-ion secondary batteries: The prepared positive electrode sheet, separator and negative electrode sheet are stacked in sequence, with the separator placed between the positive electrode sheet and the negative electrode sheet to play a separating role, and then wrapped with aluminum-plastic film, and after drying, the above-mentioned electrolyte is injected. After packaging, standing, formation and other processes, a soft-pack battery (i.e., lithium-ion battery) with a capacity of 1Ah is obtained.

[0122] The cycle performance and initial DC resistance of the lithium ion battery prepared above were tested respectively, and the results are shown in Table 1;

[0123] The test steps for the cycle formation are: cycle at 25°C with a charge and discharge rate of 0.21A / g (calculated based on the mass of the positive electrode material) and 2.8-4.25V; the number of cycles with 80% SOH cutoff is used as the data recording point;

[0124] The initial DC resistance (DCR) test steps are as follows: at a temperature of 25°C, when the battery is discharged to 50% SOC (state of charge, reflecting the remaining capacity of the battery) at a current of 1C, the current is increased to 4C and maintained for 30s, and the difference between the updated stable voltage and the original platform voltage is detected. The ratio of its value to the 3C current value is the DC resistance of the battery. The DCR test result after the battery is fully charged for the first time is the initial DCR of the battery.

[0125] Table 1 Test results

[0126]

[0127] It can be seen from Table 1 that the number of cycles of the lithium-ion battery made of the negative electrode sheet formed by the negative electrode material of Examples 1-5 is ≥703 cycles, and the initial direct current resistance (DCR) is ≤110mΩ. This result shows that the lithium-ion battery made of the negative electrode sheet formed by the negative electrode material of the present invention has excellent cycle performance and power performance.

[0128] It can be seen from Table 1 that the crushing coefficient of the negative electrode material of Comparative Example 1 is greater than 40% (specifically 50.2%), and the number of cycles of the lithium-ion battery made of the negative electrode sheet formed therefrom is only 523 cycles, and the initial DC resistance (DCR) is 120.3 mΩ; while the crushing coefficients of the negative electrode materials of Examples 1-5 are all ≤40%, and the number of cycles of the lithium-ion batteries made of the negative electrode sheets formed therefrom is 703-1201 cycles, and the initial DC resistance (DCR) is 90.2-110 mΩ. The results show that by limiting the crushing coefficient of the negative electrode material to a specific range (crushing coefficient ≤40%), the cycle performance and power performance of the lithium-ion battery made of the negative electrode sheet formed by the negative electrode material can be improved.

[0129] It can be seen from Table 1 that the number of cycles of the lithium ion battery made of the negative electrode sheets formed by the negative electrode materials of Examples 1-4 (based on the mass of the carbon layer, the mass of the carbon nanomaterial is 0.05wt%-2wt%) is ≥703 cycles, while the number of cycles of the lithium ion battery made of the negative electrode sheets formed by the negative electrode materials of Comparative Example 1 (based on the mass of the carbon layer, the mass of the carbon nanomaterial is 0wt%) and Comparative Example 2 (based on the mass of the carbon layer, the mass of the carbon nanomaterial is 5wt%) are 523 cycles and 830 cycles, respectively. Controlling the content of nano-carbonaceous material within a specific range (based on the mass of the carbon layer, the mass of the carbon nanomaterial is 0.05wt%-2wt%) is beneficial to improving the cycle performance of the lithium ion battery made of the negative electrode sheet formed by the negative electrode material.

[0130] It can be seen from Table 1 that the number of cycles of the lithium ion battery made of the negative electrode sheet formed by the negative electrode material of Examples 1-4 (the diameter of the carbon-containing nanomaterial is 5-30nm, and the aspect ratio is 10:1-100:1) is ≥703, while the number of cycles of the lithium ion battery made of the negative electrode sheet formed by the negative electrode material of Comparative Example 5 (the diameter of the carbon-containing nanomaterial is 40nm, and the aspect ratio is 150:1) and Comparative Example 6 (the diameter of the carbon-containing nanomaterial is 3nm, and the aspect ratio is 8:1) are 599 and 567, respectively. Controlling the diameter and aspect ratio of the carbon-containing nanomaterial within a specific range (diameter of 5-30nm, aspect ratio of 10:1-100:1) is beneficial to improving the strength of the negative electrode material, thereby improving the cycle performance of the lithium ion battery made of the formed negative electrode sheet.

[0131] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A negative electrode material, characterized in that: The negative electrode material comprises: a carbon layer; and a silicon layer located on at least a portion of the surface of the carbon layer, and the negative electrode material satisfies the following relationship: Y≤40%; Y is the crushing coefficient of the negative electrode material, wherein Y satisfies the following relationship: Y = (D2 - D1) / D2 × 100%; Wherein, D2 is the particle size corresponding to 10% of the cumulative particle size distribution number of the negative electrode material before powder pressing treatment, in μm, and D1 is the particle size corresponding to 10% of the cumulative particle size distribution number of the negative electrode material after powder pressing treatment, in μm.

2. The negative electrode material according to claim 1, characterized in that The negative electrode material satisfies the following relationship: Y≤25%。 3. The negative electrode material according to claim 1, characterized in that The powder pressing treatment includes: increasing the pressure to 150 MPa at a pressure increasing rate of 3 MPa / min, and then maintaining the pressure at 150 MPa for 20 minutes.

4. The negative electrode material according to claim 1, characterized in that The negative electrode material satisfies the following relationship: 30%≤R≤70%; Wherein, R is the porosity utilization rate of the negative electrode material, and R satisfies the following relationship: R=[m×P / 2.21] / [1-m×n / 2.25]×100%; Wherein, m is the true density of the negative electrode material, in g / cm 3 , n and P are the mass percentages of carbon and silicon in the negative electrode material, respectively, in wt%.

5. The negative electrode material according to claim 4, characterized in that The negative electrode material satisfies the following relationship: 30%≤R≤50%。 6. The negative electrode material according to claim 1, characterized in that The carbon layer further comprises carbon-containing nanomaterials, and the carbon-containing nanomaterials comprise carbon nanofibers, carbon nanotubes or a mixture of the two.

7. The negative electrode material according to claim 6, characterized in that The diameter of the carbon nanofiber is 5-30 nm.

8. The negative electrode material according to claim 6, characterized in that Based on the mass of the carbon layer, the mass of the carbon-containing nanomaterial is 0.05wt%-2wt%.

9. An electrochemical device, characterized in that: The invention comprises a negative electrode plate, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector, wherein the negative electrode active material layer comprises the negative electrode material according to any one of claims 1 to 8.

10. An electronic device, characterized in that: Comprising the electrochemical device as claimed in claim 9.

Citation Information

Cited By

  • Active material, negative electrode sheet, battery and electric equipment

    WO2026194922A1