Silicon-carbon coated lithium iron phosphate positive electrode material and preparation method thereof, positive electrode plate, lithium ion battery and electric equipment

By coating the lithium iron phosphate cathode material with silicon carbon, and using the coating layer of lithium-embedded silicon carbon material and amorphous carbon material, the problems of low energy density and short cycle life of lithium iron phosphate batteries are solved, and high energy density is achieved. and long cycle life battery performance.

CN118738337AActive Publication Date: 2024-10-01HONEYCOMB ENERGY TECH (SHANGRAO) CO LTD

Patent Information

Application Number
CN202410884851.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-01
Estimated Expiration
2044-07-03

Smart Images

  • Figure CN118738337A_ABST
    Figure CN118738337A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion battery positive electrode materials, in particular to a silicon-carbon coated lithium iron phosphate positive electrode material and a preparation method thereof, a positive electrode plate, a lithium ion battery and electric equipment. The silicon-carbon coated lithium iron phosphate positive electrode material comprises lithium iron phosphate and a coating layer coated on the surface of the lithium iron phosphate, wherein the coating layer comprises a lithium-intercalated silicon-carbon material and an amorphous carbon material; the mass of the silicon carbon material in the lithium-embedded silicon carbon material accounts for 0.5%-3.5% of the mass of lithium iron phosphate; the percentage W2 of the mass of the silicon element in the lithium-intercalated silicon carbon material to the mass of the silicon carbon material in the lithium-intercalated silicon carbon material is 10-80%; w1 and W2 satisfy 5 < = 350W1 + 3150W1 * W2 < = 65. The silicon-carbon coated lithium iron phosphate positive electrode material provided by the invention has high capacity, high energy density, high first efficiency and excellent cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to a silicon-carbon coated lithium iron phosphate positive electrode material and a preparation method thereof, a positive electrode sheet, a lithium ion battery and electrical equipment. Background Art

[0002] Lithium-ion batteries are currently the most widely used high-performance energy storage devices that can be cyclically charged and discharged. Lithium-ion batteries refer to the general term for batteries with lithium-ion embedded compounds as positive electrode materials. The internal structure of lithium-ion batteries consists of four parts: positive electrode, negative electrode, electrolyte and diaphragm. The essence of lithium-ion batteries is concentration difference batteries. The positive and negative electrodes are lithium storage materials that allow lithium ions to be reversibly embedded and de-inserted. The operating voltage of the battery is determined by the lithium-intercalated compounds after the electrodes are embedded with lithium. The charging and discharging of lithium-ion batteries is the embedding and de-embedding of lithium ions between the positive and negative electrode materials. During the embedding and de-embedding process of lithium ions, the embedding and de-embedding of equivalent electrons to lithium ions are also accompanied (it is customary to use embedding or de-embedding for the positive electrode, and insertion or de-insertion for the negative electrode). During the charging and discharging process, lithium ions are embedded / de-embedded and inserted / de-inserted back and forth between the positive and negative electrodes, which is vividly called a "rocking chair battery".

[0003] The performance of lithium-ion batteries is largely determined by the performance of electrode materials (battery active substances). Excellent positive and negative electrode materials usually have the advantages of long cycle life, high reversible specific capacity, low synthesis cost, safe and pollution-free, and reliable safety performance. Since the first appearance of lithium-ion batteries, after decades of development and research, many lithium-insertion compounds that can be used as positive electrode materials for secondary lithium batteries have been discovered and have high redox potentials, such as Li(Ni 0.8 Co 0.15 Al 0.05 )O2 and Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O2 and other positive electrode materials containing lithium and less cobalt. This type of material reduces the proportion of LiCoO2 and greatly reduces the manufacturing cost of the battery; LiFePO4 positive electrode material has an operating voltage of 3.25V; vanadium phosphate compounds include LiVPO4F and Li3V2P3O 12 , with a higher charging and discharging platform, high energy density, etc.

[0004] At present, lithium iron phosphate (LiFePO4, abbreviated as LFP) is the most widely used lithium battery positive electrode material and is widely used in energy storage and commercial vehicle fields. However, due to the characteristics of the material itself, the voltage platform of lithium iron phosphate material is only about 3.3V, the platform is low, and the energy density is not high, which limits its use environment.

[0005] The next generation material, lithium iron manganese phosphate / lithium manganese phosphate, is relatively Li + The electrode potential of lithium manganese phosphate increases with the increase of manganese content, the theoretical capacity density is high, and the cost of raw materials for synthesizing lithium manganese phosphate is low, which makes it have great market prospects in the field of power supply. However, during the discharge process, too much Li + It will be embedded in LiMn2O4 and even form Li2Mn2O4, which will appear when the discharge reaches 3V. At this time, the material changes from cubic phase to tetragonal phase, which leads to an increase in the unit cell volume. The electrode material collapses during the discharge cycle, causing the discharge capacity to decay sharply and Mn to dissolve seriously. In addition, lithium manganese iron phosphate / lithium manganese phosphate both have low conductivity, large DCR, and it is difficult to fully utilize the capacity.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The first purpose of the present invention is to provide a silicon-carbon coated lithium iron phosphate positive electrode material, which utilizes silicon carbon to store active lithium, so that the material itself has a lithium replenishing effect in the battery, compensates for the lithium loss caused by the formation of the negative electrode SEI film, increases the total amount of reversible active lithium in the system, enhances the partial capacity of the iron lithium material, and improves the energy density of the positive electrode material.

[0008] The second purpose of the present invention is to provide a method for preparing a silicon-carbon coated lithium iron phosphate positive electrode material, which adopts silicon-carbon coating and pre-lithiation to enable the prepared silicon-carbon coated lithium iron phosphate positive electrode material to have a higher lithium content that can be inserted and removed than conventional lithium iron phosphate.

[0009] The third object of the present invention is to provide a positive electrode sheet having the advantages of high capacity, high energy density, high initial efficiency, and excellent cycle performance.

[0010] A fourth object of the present invention is to provide a lithium-ion battery having high capacity, high energy density, high initial efficiency and long cycle life.

[0011] A fifth object of the present invention is to provide an electrical device.

[0012] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0013] The present invention first provides a silicon-carbon coated lithium iron phosphate positive electrode material, comprising lithium iron phosphate and a coating layer coated on the surface of the lithium iron phosphate, wherein the coating layer comprises a lithium-embedded silicon-carbon material and an amorphous carbon material;

[0014] Wherein, the mass percentage W1 of the silicon-carbon material in the lithium-embedded silicon-carbon material to the mass percentage of the lithium iron phosphate is 0.5% to 3.5%;

[0015] The mass of the silicon element in the lithium-intercalated silicon-carbon material accounts for a percentage W2 of the mass of the silicon-carbon material in the lithium-intercalated silicon-carbon material of 10% to 80%;

[0016] The W1 and the W2 satisfy the following relationship: 5≤350W1+3150W1×W2≤65.

[0017] Preferably, the particle size D of the silicon-carbon coated lithium iron phosphate positive electrode material is 50 0.2~2μm.

[0018] The present invention further provides a method for preparing the silicon-carbon coated lithium iron phosphate positive electrode material, comprising the following steps:

[0019] The lithium iron phosphate, the lithium source, the carbon source and the silicon-carbon material are mixed and sintered.

[0020] Preferably, the carbon source comprises at least one of citric acid, glucose, sucrose and polyethylene glycol.

[0021] Preferably, the molar ratio of the lithium iron phosphate to the lithium source is 1:0.02-0.3.

[0022] Preferably, the mass of the carbon source is 1% to 10% of the mass of the lithium iron phosphate.

[0023] Preferably, the mass of the silicon-carbon material is 0.5% to 3.5% of the mass of the lithium iron phosphate.

[0024] Preferably, the sintering is performed in an oxygen-free atmosphere.

[0025] Preferably, the sintering temperature is 700-800° C., and the holding time is 2-12 hours.

[0026] Preferably, a dispersant is added during the mixing process, and the mixture is dried after the mixing, and then the sintering is performed.

[0027] The present invention further provides a positive electrode sheet, comprising the silicon-carbon coated lithium iron phosphate positive electrode material.

[0028] The present invention further provides a lithium ion battery, comprising the positive electrode sheet.

[0029] The present invention also provides an electrical device, comprising the lithium-ion battery.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The silicon-carbon coated lithium iron phosphate positive electrode material provided by the present invention utilizes silicon-carbon to store active lithium, which can enable the material to have a lithium replenishing effect in the battery itself, compensate for the lithium loss caused by the formation of the negative electrode SEI film, increase the total amount of reversible active lithium in the system, enhance the partial capacity of the iron-lithium material, and improve the energy density of the positive electrode material.

[0032] (2) The silicon-carbon coated lithium iron phosphate positive electrode material provided by the present invention can store the reserve lithium in the negative electrode after the first charge and continuously release it during the cycle process to make up for the reversible lithium loss of the battery system and significantly improve the cycle life of the battery.

[0033] (3) The silicon-carbon coated lithium iron phosphate positive electrode material provided by the present invention has a small and uniformly distributed particle size, a stable structure, and a surface uniformly coated with a completely pre-lithiated silicon-carbon material. It can release sufficient active lithium ions to compensate for the film formation loss of the negative electrode during the initial process of the first charging of the full battery of the material, thereby increasing the total amount of reversible lithium in the battery system, solving the problem of low initial efficiency of the lithium iron phosphate full battery, and increasing the energy density of the full battery by more than 8%. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 This is a schematic flow chart of the method for preparing the silicon-carbon coated lithium iron phosphate positive electrode material of Example 1 provided by the present invention. DETAILED DESCRIPTION

[0036] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0037] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0038] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0039] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.

[0040] In a first aspect, the present invention provides a silicon-carbon coated lithium iron phosphate positive electrode material, which includes lithium iron phosphate and a coating layer coated on the surface of the lithium iron phosphate.

[0041] Wherein, the coating layer includes lithium-embedded silicon-carbon material (referring to a composite material in which lithium is embedded in silicon-carbon material) and an amorphous carbon material.

[0042] In some specific embodiments, amorphous carbon can be produced by decomposing an added organic carbon source, and its function is to create a reducing atmosphere environment for the reaction, and is combined with a lithium-embedded silicon-carbon material to uniformly coat the surface of the lithium iron phosphate material.

[0043] Among them, the percentage W1 of the mass of the silicon-carbon material in the lithium-embedded silicon-carbon material to the mass of the lithium iron phosphate is 0.5% to 3.5%, including but not limited to any point value of 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or any range value between two of them.

[0044] The percentage W2 of the mass of the silicon element in the lithium-embedded silicon-carbon material (or the mass of the silicon element in the silicon-carbon material) to the mass of the silicon-carbon material in the lithium-embedded silicon-carbon material is 10% to 80%; including but not limited to any point value of 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80% or a range value between any two of them.

[0045] The W1 and W2 satisfy the following relationship: 5≤350W1+3150W1×W2≤65. The value of 350W1+3150W1×W2 includes but is not limited to any one of 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65 or a range between any two of them.

[0046] The silicon-carbon coated lithium iron phosphate positive electrode material provided by the present invention utilizes silicon carbon to store active lithium, so that the material itself has a lithium replenishing effect in the battery, compensates for the lithium loss caused by SEI film formation at the negative electrode, increases the total amount of reversible active lithium in the system, enhances the partial capacity of the lithium iron phosphate material, and improves the energy density of the positive electrode material, thus greatly compensating for the defect of low energy density of LFP.

[0047] At the same time, the reserve lithium can also be stored in the negative electrode after the first charge and continuously released during the cycle process to make up for the reversible lithium loss of the battery system and significantly improve the cycle life of the battery.

[0048] In addition, the surface is evenly coated with fully pre-lithiated silicon-carbon material (i.e., lithium-embedded silicon-carbon material), which can release sufficient active lithium ions to compensate for the negative electrode film formation loss during the initial process of the first charging of the full battery, thereby increasing the total amount of reversible lithium in the battery system and solving the problem of low first efficiency (i.e., first coulombic efficiency) of the lithium iron phosphate full battery.

[0049] The present invention can control the pre-lithium amount of the material to achieve the required lithium replenishment effect by regulating the pre-lithium silicon-carbon coating amount and the silicon content. When 350W1+3150W1×W2<5, the lithium replenishment effect is weak and has no practical application value. In the range of 5-65, the lithium replenishment effect gradually increases with the increase of the value. When it is in the range of 5-25, the value increases, and the energy density of the battery made of the material gradually increases. When it is in the range of 25-65, the value increases, and the lithium replenishment amount exceeds the reversible value of the LFP material. The excess lithium will be stored in the negative electrode and continuously released during the cycle process to make up for the lithium consumed by the side reaction, thereby greatly improving the cycle performance of the material (the higher the value, the greater the increase in the cycle performance). When the formula value is greater than 65, the lithium replenishment amount is too large and there is no practical application demand.

[0050] In some specific embodiments, the pre-lithium silicon-carbon coated lithium iron phosphate positive electrode material provided by the present invention can improve the energy density of the whole battery by more than 8% compared with conventional LFP materials.

[0051] In some specific embodiments, the particle size D of the silicon-carbon coated lithium iron phosphate positive electrode material is 50 It is 0.2-2 μm, including but not limited to any point value of 0.2 μm, 0.5 μm, 0.8 μm, 1 μm, 1.3 μm, 1.5 μm, 1.8 μm, 2 μm or a range value between any two of them.

[0052] The silicon-carbon coated lithium iron phosphate positive electrode material provided by the present invention has a small particle size, excellent rate performance, and is evenly distributed.

[0053] In a second aspect, the present invention provides a method for preparing the above-mentioned silicon-carbon coated lithium iron phosphate positive electrode material, comprising the following steps: mixing lithium iron phosphate, a lithium source, a carbon source and a silicon-carbon material and sintering them.

[0054] The present invention adopts silicon-carbon coating and pre-lithiation, so that the prepared silicon-carbon coated lithium iron phosphate positive electrode material can have a higher lithium content that can be intercalated and deintercalated compared with conventional lithium iron phosphate.

[0055] Specifically, the use of silicon carbon to store active lithium during the material preparation process can enable the material to have a lithium replenishment effect in the battery itself, make up for the lithium loss of the negative electrode SEI film, increase the total amount of reversible active lithium in the system, and enhance the partial capacity of the iron-lithium material, so that the energy density of the whole battery of this material is increased by more than 8% relative to conventional LFP materials. In addition, the reserve lithium can also be stored in the negative electrode after the first charge, and is continuously released during the cycle process, making up for the reversible lithium loss of the battery system and significantly improving the cycle life of the battery.

[0056] It is understandable that the lithium source anions decompose during the sintering process, leaving only lithium embedded in the silicon carbon to form a lithium-embedded silicon-carbon material. The organic carbon source will also decompose during the sintering process, and only a small part will form amorphous carbon. Therefore, in the final silicon-carbon coated lithium iron phosphate positive electrode material, the mass of the lithium-embedded silicon-carbon material accounts for 0.5% to 3.5% of the mass of the silicon-carbon coated lithium iron phosphate positive electrode material, and the mass of silicon in the lithium-embedded silicon-carbon material accounts for 10% to 80% of the mass of the lithium-embedded silicon-carbon material.

[0057] In some specific embodiments, the carbon source includes at least one of citric acid, glucose, sucrose and polyethylene glycol.

[0058] In some specific embodiments, the molar ratio of the lithium iron phosphate to the lithium source is 1:0.02-0.3, including but not limited to any one of 1:0.02, 1:0.05, 1:0.08, 1:0.1, 1:0.15, 1:0.2, 1:0.25, 1:0.3 or a range between any two of them.

[0059] The above molar ratio is used to achieve good pre-lithiation effect.

[0060] In some specific embodiments, the mass of the carbon source is 1% to 10% of the mass of the lithium iron phosphate; including but not limited to any point value of 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range value between any two of them.

[0061] In some specific embodiments, the mass of the silicon-carbon material is 0.5% to 3.5% of the mass of the lithium iron phosphate, including but not limited to any point value of 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or a range value between any two of them.

[0062] In some specific embodiments, the sintering is performed in an oxygen-free atmosphere, ie, an atmosphere that does not contain oxygen.

[0063] In some specific embodiments, the sintering temperature is 700-800°C, including but not limited to any one of 700°C, 720°C, 750°C, 780°C, 800°C or a range between any two of them.

[0064] In some specific embodiments, the sintering holding time is 2 to 12 hours, including but not limited to any one of 2 hours, 3 hours, 5 hours, 8 hours, 10 hours, and 12 hours, or a range between any two of them.

[0065] In some specific implementations, a dispersant is added during the mixing process, and the mixture is dried after the mixing, and then sintered.

[0066] In some specific embodiments, the dispersant includes one of deionized water, methanol solution, ethanol solution, acetone solution and polyol solution.

[0067] In some specific implementations, the mass of the dispersant is 5 to 10 times the mass of lithium iron phosphate.

[0068] In some specific embodiments, the lithium source includes a soluble lithium source, such as at least one of lithium hydroxide, lithium carbonate, lithium chloride, lithium nitrate, lithium dihydrogen phosphate, and lithium acetate, but is not limited thereto.

[0069] In some specific embodiments, the raw materials are mixed uniformly by grinding.

[0070] In some specific embodiments, the gas used in the oxygen-free atmosphere includes one or more of nitrogen, argon, and carbon dioxide.

[0071] In some specific embodiments, the sintering further includes a pulverizing step, preferably using air flow pulverizing.

[0072] In some specific embodiments, the method for preparing the silicon-carbon coated lithium iron phosphate positive electrode material specifically comprises: mixing and grinding lithium iron phosphate, a lithium source, a carbon source and a dispersant, wherein the grinding is performed until the particle size D of the mixed material is 50The silicon-carbon material is added thereto, mixed evenly and then spray-dried, then sintered in an oxygen-free atmosphere, and then pulverized to a particle size D after cooling. 50 The thickness of the silicon-carbon coated lithium iron phosphate positive electrode material is 0.2-2 μm, and the silicon-carbon coated lithium iron phosphate positive electrode material is obtained.

[0073] In some specific embodiments, lithium iron phosphate is prepared by a hydrothermal method, and the preparation method of lithium iron phosphate includes: weighing a soluble lithium source, an iron source and a phosphorus source according to a molar ratio of lithium element: iron element: phosphorus element = 1.01 to 1.05 (including but not limited to any one of 1.01, 1.02, 1.03, 1.04, 1.05 or a range between any two): 0.99 to 1:1, pouring them into a solvent, stirring on an automatic stirrer for 0.5 to 1h to mix evenly, to obtain a precursor solution; transferring the precursor solution into a hydrothermal reactor in an oxygen-free gas atmosphere, and heating at 100 to 200°C (including but not limited to 100°C, 130°C, 150°C, 180 ℃, 200℃, or any range between them) for 2-12h (including but not limited to 2h, 3h, 5h, 8h, 10h, or any range between them), cooled to room temperature, filtered to obtain a solid material, washed with anhydrous ethanol, and then vacuum dried at 100-200℃ (including but not limited to 100℃, 130℃, 150℃, 180℃, 200℃, or any range between them) for 2-10h (including but not limited to 2h, 3h, 5h, 8h, or any range between them) to obtain the lithium iron phosphate.

[0074] The lithium source includes a soluble lithium source, such as one or more of lithium hydroxide, lithium carbonate, lithium chloride, lithium nitrate, lithium dihydrogen phosphate, and lithium acetate, but is not limited thereto.

[0075] The iron source includes a soluble iron source, such as one or more of ferrous sulfate, ferrous nitrate, and ferrous chloride, but is not limited thereto.

[0076] The phosphorus source includes a soluble phosphorus source, such as one or more of phosphoric acid, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, and lithium dihydrogen phosphate, but is not limited thereto.

[0077] In a third aspect, the present invention provides a positive electrode sheet comprising the above-mentioned silicon-carbon-coated lithium iron phosphate positive electrode material.

[0078] The positive electrode sheet provided by the present invention has the advantages of high capacity, high energy density, high initial efficiency, excellent cycle performance, etc.

[0079] Optionally, the positive electrode sheet further includes a binder and / or a conductive agent, which is not limited in the present invention.

[0080] In a fourth aspect, the present invention provides a lithium-ion battery comprising the above-mentioned positive electrode sheet.

[0081] The lithium ion battery provided by the present invention has high capacity, high energy density, high initial efficiency and long cycle life.

[0082] Optionally, the lithium-ion battery further includes a negative electrode sheet, a separator and an electrolyte, which is not limited in the present invention.

[0083] In a fifth aspect, the present invention provides an electrical device comprising the above-mentioned lithium-ion battery.

[0084] The electrical equipment includes any equipment or device using the above-mentioned lithium-ion battery, such as electric vehicles, electric motorcycles, electric bicycles, electric tools, starting power supplies, energy storage devices, electronic products and office equipment, etc., and the present invention does not limit this.

[0085] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0086] Example 1

[0087] The method for preparing the silicon-carbon coated lithium iron phosphate positive electrode material provided in this embodiment comprises the following steps:

[0088] (1) Synthesis of lithium iron phosphate by hydrothermal method: Weigh 2.45 g of lithium hydroxide (lithium source), 15.00 g of ferrous sulfate (iron source), and 9.80 g of solid phosphoric acid (phosphorus source), pour them into 150 ml of deionized water in sequence, stir them on an automatic stirrer for 1 h to mix evenly and completely dissolve them into a solution to obtain a precursor solution; transfer the precursor solution into a hydrothermal reactor in an oxygen-free gas atmosphere (nitrogen), keep it warm at 200°C for 6 h, cool it to room temperature, filter to obtain a solid material, wash it with anhydrous ethanol, and then vacuum dry it at 150°C for 4 h to obtain lithium iron phosphate.

[0089] (2) Pre-lithiation silicon-carbon coated lithium iron phosphate: Weigh 10.00 g of lithium iron phosphate obtained in step (1) and 0.08 g of lithium hydroxide (i.e., the molar ratio of lithium iron phosphate to the lithium source is 1:0.052), pour them into deionized water in turn, and then add 0.8 g of glucose (i.e., the mass of the carbon source is 8% of the mass of the lithium iron phosphate), grind them with a sand mill, and control the particle size D 50 The particle size of the coated material is 0.5 μm, and then 0.05 g of silicon-carbon material is added (i.e., the mass of the silicon-carbon material is 0.5% of the mass of the lithium iron phosphate, the mass fraction of silicon in the silicon-carbon material is 50%, and the silicon-carbon material is Lanxi Zhide S0310 silicon-carbon ratio customized model). After mixing evenly, spray drying is performed, and then sintering is performed at 750 ° C for 6 h in an oxygen-free atmosphere (nitrogen). After cooling, the coated material is subjected to air flow pulverization to a particle size of D 50 The thickness of the silicon-carbon coated lithium iron phosphate positive electrode material is 0.7 μm, and the silicon-carbon coated lithium iron phosphate positive electrode material is obtained. The silicon-carbon coated lithium iron phosphate positive electrode material includes lithium iron phosphate and a coating layer coated on the surface of the lithium iron phosphate, and the coating layer includes a lithium-embedded silicon-carbon material and an amorphous carbon material.

[0090] Figure 1 Schematic diagram of the process of preparing the silicon-carbon coated lithium iron phosphate positive electrode material of this embodiment.

[0091] Example 2

[0092] The method for preparing the silicon-carbon coated lithium iron phosphate positive electrode material provided in this embodiment comprises the following steps:

[0093] (1) Synthesis of lithium ferrous phosphate by hydrothermal method: 3.87 g of lithium carbonate, 18.00 g of ferrous nitrate, and 14.9 g of ammonium phosphate solid were weighed and poured into 200 ml of 50% ethanol solution in sequence, and stirred on an automatic stirrer for 1 h to mix evenly and completely dissolve into a solution to obtain a precursor solution; the precursor solution was transferred into a hydrothermal reactor in an oxygen-free gas atmosphere (nitrogen), kept warm at 170° C. for 6 h, cooled to room temperature, filtered to obtain a solid material, washed with anhydrous ethanol, and vacuum dried at 110° C. for 7 h to obtain lithium ferrous phosphate.

[0094] (2) Pre-lithiation silicon-carbon coated lithium iron phosphate: Weigh 10.00 g of lithium iron phosphate obtained in step (1) and 0.18 g of lithium hydroxide (i.e., the molar ratio of lithium iron phosphate to the lithium source is 1:0.12), pour them into deionized water in sequence, and then add 0.6 g of glucose (i.e., the mass of the carbon source is 6% of the mass of the lithium iron phosphate), grind them with a sand mill, and control the particle size D 50The particle size of the coated material is 0.3 μm, and then 0.20 g of silicon-carbon material is added (i.e., the mass of the silicon-carbon material is 2% of the mass of the lithium iron phosphate, the mass fraction of silicon in the silicon-carbon material is 30%, and the silicon-carbon material is Lanxi Zhide S0310 silicon-carbon ratio customized model). After mixing evenly, spray drying is performed, and then sintering is performed at 730 ° C for 7 h in an oxygen-free atmosphere (nitrogen). After cooling, the coated material is air flow crushed to a particle size D 50 The thickness of the silicon-carbon coated lithium iron phosphate positive electrode material was 0.5 μm.

[0095] Example 3

[0096] The preparation method of the silicon-carbon coated lithium iron phosphate positive electrode material provided in this embodiment comprises the following steps:

[0097] (1) Synthesis of lithium iron phosphate by hydrothermal method: Weigh 10.39 g of lithium dihydrogen phosphate, 25.20 g of ferrous chloride, and 11.5 g of ammonium dihydrogen phosphate solid, pour them into 170 ml of 40% methanol solution in sequence, stir them on an automatic stirrer for 1.2 h to mix evenly, and completely dissolve them into a solution to obtain a precursor solution; transfer the precursor solution into a hydrothermal reactor in an oxygen-free gas atmosphere (argon), keep it warm at 150° C. for 9 h, cool it to room temperature, filter to obtain a solid material, wash it with anhydrous ethanol, and then vacuum dry it at 140° C. for 5.5 h to obtain lithium iron phosphate.

[0098] (2) Pre-lithiation silicon-carbon coated lithium iron phosphate: Weigh 10.00 g of lithium iron phosphate obtained in step (1) and 0.47 g of lithium carbonate (i.e., the molar ratio of lithium iron phosphate to the lithium source is 1:0.1), pour them into a 60% ethanol solution in sequence, add 0.5 g of glucose (i.e., the mass of the carbon source is 5% of the mass of the lithium iron phosphate), and grind them with a sand mill to control the particle size D 50 The particle size of the coated material is 0.4 μm, and then 0.15 g of silicon-carbon material is added (i.e., the mass of the silicon-carbon material is 1.5% of the mass of the lithium iron phosphate, the mass fraction of silicon in the silicon-carbon material is 60%, and the silicon-carbon material is Lanxi Zhide S0310 silicon-carbon ratio customized model). After mixing evenly, spray drying is performed, and then sintering is performed at 760 ° C for 10 h in an oxygen-free atmosphere (argon). After cooling, the coated material is air flow crushed to a particle size D 50 The particle size of the silicon-carbon coated lithium iron phosphate positive electrode material was 0.8 μm.

[0099] Example 4

[0100] The preparation method of the silicon-carbon coated lithium iron phosphate positive electrode material provided in this embodiment is basically the same as that in Example 1, except that, in step (2), the mass of lithium hydroxide is replaced by 0.40 g, that is, the molar ratio of lithium iron phosphate to the lithium source is 1:0.26; and the added amount of silicon-carbon material is replaced by 0.25 g (that is, the mass of silicon-carbon material is 2.5% of the mass of lithium iron phosphate).

[0101] Example 5

[0102] The preparation method of the silicon-carbon coated lithium iron phosphate positive electrode material provided in this embodiment is basically the same as that in Example 1, except that in step (2), glucose is replaced by an equal mass of citric acid.

[0103] Comparative Example 1

[0104] The positive electrode material provided in this comparative example is lithium iron phosphate prepared in step (1) of Example 1.

[0105] Comparative Example 2

[0106] The preparation method of the positive electrode material provided in this comparative example is basically the same as that of Example 1, except that in step (2), lithium hydroxide is not added.

[0107] Comparative Example 3

[0108] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 1, except that in step (2), no silicon-carbon material is added.

[0109] Comparative Example 4

[0110] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 1, except that in step (2), the mass of lithium hydroxide is replaced by 0.80 g, that is, the molar ratio of lithium iron phosphate to the lithium source is 1:0.52; and the amount of silicon-carbon material added is replaced by 0.50 g (that is, the mass of silicon-carbon material is 5.0% of the mass of lithium iron phosphate). The values ​​of W1, W2 and 350W1+3150W1×W2 in the positive electrode materials prepared in each embodiment and each comparative example are shown in Table 1.

[0111] Table 1 Values ​​of W1, W2 and 350W1+3150W1×W2

[0112] Group <![CDATA[W1]]> <![CDATA[W2]]> <![CDATA[350W1+3150W1×W2]]> Example 1 0.5% 50% 9.625 Example 2 2.0% 30% 25.9 Example 3 1.5% 60% 33.6 Example 4 2.5% 50% 48.12 Example 5 0.5% 50% 9.625 Comparative Example 1 0% 0% 0 Comparative Example 2 0% 50% 0 Comparative Example 3 0% 0% 0 Comparative Example 4 5% 50% 96.25

[0113] Experimental example

[0114] The positive electrode materials obtained in each embodiment and each comparative example were assembled into a full battery in a glove box. The negative electrode adopted a conventional graphite negative electrode. The positive electrode formula and surface density were kept the same as the negative electrode formula. The negative electrode coating surface density was adjusted by charging NP ratio 1.04. Then, the electrochemical performance was tested with the Xinwei test system. The electrical performance test results are shown in Table 2.

[0115] Among them, the working voltage range of the electrochemical test is 2.0-3.8V.

[0116] Table 2 Full battery electrical performance test results

[0117]

[0118]

[0119] It can be seen from Table 2 that the silicon-carbon coated lithium iron phosphate positive electrode material prepared in each embodiment has excellent 0.33C gram capacity performance, far exceeding LFP (related to the pre-lithium silicon-carbon coating amount and silicon content), and the performance is consistent at high rates, indicating that the process has a superior capacity enhancement effect.

[0120] It can be seen from Example 3 that when the amount of lithium supplemented by the pre-lithium silicon-carbon coating is higher than the amount of lithium consumed by the negative electrode film formation, the total amount of reversible lithium in the battery system is higher than the reversible amount of lithium iron phosphate, and the remaining reversible lithium will be stored at the negative electrode and continuously released during the cycle process to make up for the reversible lithium loss of the battery system, so that the capacity of the battery cell does not decay during the long cycle process, significantly improving the cycle life of the battery.

[0121] By comparing Example 1 and Comparative Example 2, it can be seen that the addition of a pre-lithiation lithium source can embed lithium into the silicon-carbon material through sintering, thereby achieving a lithium supplementation effect. If no lithium source is added, the silicon-carbon material alone has no effect.

[0122] By comparing Example 1 and Comparative Example 3, it can be seen that the coated silicon-carbon material can become a carrier of lithium, so that the pre-lithiated silicon-carbon can play a lithium supplementing effect. If no silicon-carbon material is added, the lithium source alone cannot be sintered into the material and has no effect.

[0123] By comparing Examples 2, 3, 4 and Comparative Example 4, it can be seen that when the relationship 350W1+3150W1×W2 is greater than 25, the gram capacity does not increase but decreases, the energy density does not increase, and the excess lithium is reserved in the negative electrode to improve the cycle. When 350W1+3150W1×W2 is greater than 65, the gram capacity decreases significantly, and the negative electrode reserves too much lithium content, which has no practical application significance.

[0124] In summary, the silicon-carbon coated lithium iron phosphate positive electrode material provided by the present invention can effectively improve the capacity and cycle stability by coating the lithium iron phosphate with a specific coating layer and regulating the silicon-carbon material and silicon dosage.

[0125] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A silicon-carbon coated lithium iron phosphate positive electrode material, characterized in that: It comprises lithium iron phosphate and a coating layer coated on the surface of the lithium iron phosphate, wherein the coating layer comprises a lithium-embedded silicon-carbon material and an amorphous carbon material; Wherein, the mass percentage W1 of the silicon-carbon material in the lithium-embedded silicon-carbon material to the mass percentage of the lithium iron phosphate is 0.5% to 3.5%; The mass of the silicon element in the lithium-intercalated silicon-carbon material accounts for a percentage W2 of the mass of the silicon-carbon material in the lithium-intercalated silicon-carbon material of 10% to 80%; The W1 and the W2 satisfy the following relationship: 5≤350W1+3150W1×W2≤65.

2. The silicon-carbon coated lithium iron phosphate positive electrode material according to claim 1, characterized in that: The particle size D of the silicon-carbon coated lithium iron phosphate positive electrode material 50 0.2~2μm.

3. The method for preparing the silicon-carbon coated lithium iron phosphate positive electrode material according to claim 1 or 2, characterized in that: The steps include: The lithium iron phosphate, the lithium source, the carbon source and the silicon-carbon material are mixed and sintered.

4. The method for preparing the silicon-carbon coated lithium iron phosphate positive electrode material according to claim 3, characterized in that: The carbon source includes at least one of citric acid, glucose, sucrose and polyethylene glycol.

5. The method for preparing the silicon-carbon coated lithium iron phosphate positive electrode material according to claim 3, characterized in that: At least one of the following conditions is met: (1) The molar ratio of the lithium iron phosphate to the lithium source is 1:0.02-0.3; (2) The mass of the carbon source is 1% to 10% of the mass of the lithium iron phosphate; (3) The mass of the silicon-carbon material is 0.5% to 3.5% of the mass of the lithium iron phosphate.

6. The method for preparing the silicon-carbon coated lithium iron phosphate positive electrode material according to claim 3, characterized in that: At least one of the following conditions is met: (1) The sintering is carried out in an oxygen-free atmosphere; (2) The sintering temperature is 700-800°C and the holding time is 2-12h.

7. The method for preparing the silicon-carbon coated lithium iron phosphate positive electrode material according to claim 3, characterized in that: A dispersant is added during the mixing process, and the mixture is dried after the mixing, and then the sintering is performed.

8. A positive electrode sheet, characterized in that: It comprises the silicon-carbon coated lithium iron phosphate positive electrode material as described in claim 1 or 2.

9. A lithium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 8.

10. An electrical device, characterized in that: Comprising the lithium ion battery as claimed in claim 9.

Citation Information

Patent Citations

  • Method for preparing lithium iron phosphate positive material

    CN103390750A

  • Preparation method for carbon-silicon coated lithium iron phosphate composite material for lithium ion battery

    CN105609716A

  • Positive electrode material as well as preparation method and application thereof

    CN115020687A

  • Preparation method of titanium lithium stannate and carbon co-coated modified lithium iron phosphate positive electrode material

    CN117117108A

  • Modified lithium iron phosphate composite positive electrode material and preparation method thereof

    CN117691057A

Cited By

  • Silicon-carbon-coated lithium iron phosphate positive electrode material and preparation method therefor, positive electrode sheet, lithium-ion battery, and electric device

    WO2026007934A1