Conversion-type cobalt polysulfide composite positive electrode material with high sulfur content and preparation method of conversion-type cobalt polysulfide composite positive electrode material

By combining amorphous cobalt polysulfide nanoparticles with high sulfur content and conductive agents, the problem of volume change and low sulfur content of conversion materials during discharge is solved, high conductivity and cycle stability are achieved, and lithium-ion batteries are improved. The specific discharge capacity and Coulombic efficiency of the battery.

CN118738340APending Publication Date: 2024-10-01NANJING NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410897381.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The volume change of existing conversion-type lithium-ion battery cathode materials during the discharge process slows down the kinetics, and the low sulfur content limits the output of high discharge specific capacity, hindering its further development.

Method used

Amorphous cobalt polysulfide nanoparticles with high sulfur content are combined with a conductive agent to generate amorphous cobalt polysulfide through a displacement reaction, and the conductive agent is used as a carrier to form a composite material to improve conductivity and cycle stability.

Benefits of technology

It significantly improves the conductivity and cycle stability of the material, increases the reaction interface and diffusion channel, shortens the migration path of ions, achieves a high specific surface area, and improves the discharge specific capacity and first-cycle Coulombic efficiency of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738340A_ABST
    Figure CN118738340A_ABST
Patent Text Reader

Abstract

The invention discloses a conversion type cobalt polysulfide composite positive electrode material with high sulfur content. The composite material is composed of a conductive agent and cobalt polysulfide nanoparticles loaded on the conductive agent, the cobalt polysulfide nanoparticles are of an amorphous structure. The invention also discloses a preparation method of the conversion type cobalt polysulfide composite material. According to the composite material, the sulfur content of the material is increased, amorphous cobalt polysulfide is generated, and the conductive agent is used as a carrier to be compounded with the cobalt polysulfide, so that on one hand, the conductivity of the material can be greatly improved, and on the other hand, the volume change of a cobalt polysulfide positive electrode in the charge-discharge process can be effectively improved; when the material is used as a lithium ion battery positive electrode material, the material has good cycling stability, high specific discharge capacity and high first-circle coulombic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a conversion type cobalt polysulfide composite positive electrode material with a high sulfur content, and also relates to a preparation method of the conversion type cobalt polysulfide composite material. Background Art

[0002] Lithium-ion batteries are the most promising new generation of secondary chemical power sources, which realize the mutual conversion of chemical energy and electrical energy. At present, the positive electrode materials of lithium-ion batteries include lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMnO2), lithium iron phosphate (LiFePO4), ternary materials (NCM), etc. Among them, lithium cobalt oxide (LiCoO2) is the earliest commercialized and most successfully applied lithium-ion battery positive electrode material. However, the above positive electrode materials have low energy density, and will produce irreversible structural transformation at high voltages. At the same time, they will react adversely with the electrolyte, resulting in rapid battery capacity decay and decreased cycle stability.

[0003] Based on conversion cathode materials, such as FeS2, MoS2, VS2, etc., multi-electron reactions will occur, making the energy density about 3 times higher than that of embedded cathode materials. The metal bond-S they form can improve the electronic conductivity of the positive electrode material. At the same time, it has the advantages of low price, non-toxicity, and abundant reserves. It is considered to be a class of highly promising battery positive electrode materials. However, these conversion materials will undergo phase transitions during the battery discharge process, resulting in huge volume changes, which will slow down the battery's dynamics and cause the capacity to decay rapidly; at the same time, the low sulfur content limits the output of high discharge specific capacity. These problems have seriously hindered its further development. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a conversion-type cobalt polysulfide composite positive electrode material with a high sulfur content, which can solve the problems of low sulfur content in the conversion-type material in the prior art and volume change during discharge leading to kinetic slowdown; another purpose of the present invention is to provide a method for preparing the above-mentioned conversion-type cobalt polysulfide composite material.

[0005] Technical solution: The high-sulfur-content conversion-type cobalt polysulfide composite positive electrode material described in the present invention comprises a conductive agent and cobalt polysulfide nanoparticles loaded on the conductive agent; the cobalt polysulfide nanoparticles are of an amorphous structure.

[0006] The particle size of the cobalt polysulfide nanoparticles is 10-20 nm.

[0007] The preparation method of the above-mentioned conversion type cobalt polysulfide composite positive electrode material comprises the following steps:

[0008] (1) adding sulfide to deionized water and heating it in an inert gas atmosphere by condensation reflux;

[0009] (2) adding sulfur powder to the sulfide solution obtained in step (1), heating by condensation reflux in an inert gas atmosphere, and cooling the obtained polysulfide solution to room temperature after all the sulfur powder has reacted; the formed polysulfide refers to a sulfide in which the sulfur content and valence are increased compared with the sulfide before the reaction;

[0010] (3) placing the conductive agent in deionized water and ultrasonically dispersing the conductive agent, then adding the cobalt source to the conductive agent solution, mixing and stirring to obtain a mixed solution;

[0011] (4) adding the mixed solution obtained in step (3) dropwise to the polysulfide solution in step (2), mixing and stirring to allow for a full reaction; homogeneously reacting at low temperature to form an amorphous material;

[0012] (5) The solid product obtained after the reaction in step (4) is washed several times with deionized water and anhydrous ethanol, and then dried in a vacuum oven to obtain a cobalt polysulfide composite material.

[0013] Wherein, in step (1), the sulfide is at least one of sodium sulfide, potassium sulfide or ammonium sulfide.

[0014] Wherein, in step (1), the sulfide is heated in deionized water at a temperature of 30 to 150° C., and is heated while being stirred for a heating time of 20 to 60 minutes.

[0015] Wherein, in step (2), the molar ratio of the sulfur powder to the sulfide is 1 to 10:1.

[0016] Wherein, in step (2), the reaction temperature of the sulfur powder and the sulfide solution is 20 to 150° C., and the heating is carried out while stirring for a stirring time of 0.05 to 12 hours.

[0017] Wherein, in step (3), the conductive agent is one of oxidized carbon nanotubes, graphene oxide, biochar or Ketjen black; and the cobalt source is one of cobalt nitrate, cobalt sulfate, cobalt chloride, cobalt acetate, cobalt carbonate or cobalt fluoride.

[0018] Wherein, in step (3), the molar ratio of the cobalt source to the conductive agent is 0.1 to 100:1.

[0019] Wherein, in step (3), the ultrasonic time for forming the conductive agent solution is 10 to 1200 min; the stirring temperature of the conductive agent solution and the cobalt source is 30 to 100° C., and the stirring time is 1 to 24 h.

[0020] Wherein, in step (4), the molar ratio of the cobalt source to the polysulfide is 1:1; the stirring temperature of the mixed solution and the polysulfide solution is 20 to 160° C., and the stirring time is 2 to 12 hours.

[0021] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: on the one hand, the present invention uses a replacement reaction to homogeneously react a cobalt source with polysulfide at low temperature to generate amorphous cobalt polysulfide, and on the other hand, uses a conductive agent as a carrier to compound with cobalt polysulfide to obtain a cobalt polysulfide composite material; the composite material of the present invention increases the sulfur content of the material, generates amorphous cobalt polysulfide, and uses a conductive agent as a carrier to compound with cobalt polysulfide, which, on the one hand, greatly improves the conductivity of the material, and on the other hand, effectively improves the volume change of cobalt polysulfide during the charge and discharge process. At the same time, the composite positive electrode material also has an ultrafine nanoparticle morphology, so it has a high specific surface area, can increase the reaction interface and provide more active sites and diffusion channels, shorten the migration path of ions, thereby increasing the diffusion rate of ions, so that it has good cycle stability, high discharge specific capacity and high first-cycle coulomb efficiency when used as a positive electrode material for lithium-ion batteries; at 0.1A g -1 It can generate 840mAh g -1 The discharge specific capacity is about 4 to 5 times higher than that of traditional embedded positive electrode materials (lithium iron phosphate). BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the XRD pattern of the cobalt polysulfide composite positive electrode material prepared in Example 1;

[0023] Figure 2 TEM image of the cobalt polysulfide composite positive electrode material prepared in Example 1;

[0024] Figure 3 For a lithium ion battery based on the cobalt polysulfide composite positive electrode material of Example 1 at 0.1A g -1 The charge and discharge curve of

[0025] Figure 4 For a lithium ion battery based on the cobalt polysulfide composite positive electrode material of Example 1 at 0.1A g -1 Cycle performance diagram of

[0026] Figure 5 For a lithium-ion battery based on the cobalt polysulfide composite positive electrode material of Example 2 at 0.1A g -1 The charge and discharge curve of

[0027] Figure 6 For a lithium-ion battery based on the cobalt polysulfide composite positive electrode material of Example 2 at 0.1A g -1 Cycle performance diagram of

[0028] Figure 7 For a lithium ion battery based on the cobalt polysulfide composite positive electrode material of Example 3 at 0.1A g -1 The charge and discharge curve of

[0029] Figure 8 For a lithium ion battery based on the cobalt polysulfide composite positive electrode material of Example 3 at 0.1A g -1 Cycle performance diagram of

[0030] Fig. 9 For a lithium ion battery based on the cobalt polysulfide composite positive electrode material of Example 4 at 0.1A g -1 The charge and discharge curve of

[0031] Fig.10 For a lithium ion battery based on the cobalt polysulfide composite positive electrode material of Example 4 at 0.1A g -1 Cycle performance diagram of

[0032] Fig.11 For a lithium ion battery based on the cobalt polysulfide positive electrode material of Comparative Example 1 at 0.1A g -1 The charge and discharge curve of

[0033] Fig.12 For a lithium ion battery based on the cobalt polysulfide positive electrode material of Comparative Example 1 at 0.1A g -1 Cycle performance diagram of

[0034] Fig.13 This is the XRD diagram of the iron polysulfide composite material based on Comparative Example 2. DETAILED DESCRIPTION

[0035] Example 1

[0036] The method for preparing the conversion type cobalt polysulfide composite positive electrode material of the present invention comprises the following steps:

[0037] (1) Add 1 g of Na2S 9H2O to 20 mL of deionized water, heat to 50° C. in an inert gas atmosphere by condensation reflux, and stir for 30 min to obtain a Na2S solution;

[0038] (2) Add 0.6 g of sulfur powder to the Na2S solution in step (1), heat to 140° C. in an inert gas atmosphere by condensation reflux, and stir for 12 h. When all the sulfur powder reacts, Na2S is obtained. x The obtained Na2S x The solution was cooled to room temperature and Na2S x The solution is stored in a sealed container;

[0039] (3) 0.25 g of oxidized carbon nanotubes was placed in 30 mL of deionized water for ultrasonic dispersion. After ultrasonic dispersion for 12 h, a conductive agent solution was obtained. 1.1 g of CoSO4 7H2O was added to the conductive agent solution and stirred at 60 °C for 15 h to obtain a mixed solution of cobalt sulfate and the conductive agent.

[0040] (4) Add the mixed solution obtained in step (3) dropwise to the Na2S x The solution was stirred at 80 °C for 12 h;

[0041] (5) The precipitate (solid product) obtained after the reaction in step (4) is washed several times with deionized water and anhydrous ethanol, and then dried in a vacuum oven at 80° C. for 10 h to obtain a cobalt polysulfide composite material.

[0042] The cobalt polysulfide composite material prepared in Example 1 was made into a positive electrode sheet, a metal lithium sheet was used as a negative electrode, Celgard 2500 was selected as a separator, and a commercial 1M LiPF6, 1:1 (v / v) carbonate electrolyte of ethylene carbonate (EC) and diethyl carbonate (DEC) was selected. The battery was assembled in an Ar-filled glove box. After the assembly was completed, a battery sealer was used to seal the battery. After standing for 12 hours, the assembled lithium-ion battery was subjected to a charge and discharge cycle performance test.

[0043] like Figure 1 , which is an XRD diagram of the cobalt polysulfide composite material prepared in Example 1. It can be seen from the diagram that the cobalt polysulfide composite material is in an amorphous state.

[0044] like Figure 2 , which is a TEM image of the cobalt polysulfide composite material prepared in Example 1, it can be seen that the prepared cobalt polysulfide has a smaller size and is uniformly attached to the tube wall of the oxidized carbon nanotube.

[0045] like Figure 3 The figure shows the first cycle charge and discharge curve of the cobalt polysulfide composite material prepared in Example 1 tested in the blue electric test system. -1 At the current density, the first cycle discharge capacity is 818 mAh g -1 , the first Coulombic efficiency reached 90%.

[0046] like Figure 4 As shown, the cobalt polysulfide composite material prepared in Example 1 is -1 At the same current density, it can still maintain 750.5mAh g after 50 cycles. -1 capacity.

[0047] Example 2

[0048] The preparation method of the conversion type cobalt polysulfide composite material of the present invention comprises the following steps:

[0049] (1) Add 1 g of Na2S 9H2O to 20 mL of deionized water, heat to 50° C. in an inert gas atmosphere by condensation reflux, and stir for 30 min to obtain a Na2S solution;

[0050] (2) Add 0.6 g of sulfur powder to the Na2S solution in step (1), heat to 140° C. in an inert gas atmosphere by condensation reflux, and stir for 12 h. When all the sulfur powder reacts, Na2S is obtained. x The obtained Na2S x The solution was cooled to room temperature and Na2S x The solution is stored in a sealed container;

[0051] (3) 0.3 g of graphene oxide was placed in 30 mL of deionized water for ultrasonic dispersion. After ultrasonic dispersion for 12 h, a conductive agent solution was obtained. 1.1 g of CoSO4 7H2O was added to the conductive agent solution and stirred at 80 ° C for 15 h to obtain a mixed solution of cobalt sulfate and the conductive agent.

[0052] (4) Add the mixed solution obtained in step (3) dropwise to the Na2S x The solution was stirred at 80 °C for 12 h;

[0053] (5) The precipitate (solid product) obtained after the reaction in step (4) is washed several times with deionized water and anhydrous ethanol, and then dried in a vacuum oven at 80° C. for 10 h to obtain a cobalt polysulfide composite material.

[0054] The cobalt polysulfide composite material prepared in Example 2 was made into a positive electrode sheet, a metal lithium sheet was used as a negative electrode, Celgard 2500 was selected as a separator, and a commercial 1M LiPF6, 1:1 (v / v) carbonate electrolyte of ethylene carbonate (EC) and diethyl carbonate (DEC) was selected. The battery was assembled in an Ar-filled glove box. After the assembly was completed, a battery sealer was used to seal the battery. After standing for 12 hours, the assembled lithium-ion battery was subjected to a charge and discharge cycle performance test.

[0055] like Figure 5 The figure shows the first cycle charge and discharge curve of the cobalt polysulfide composite material prepared in Example 2 tested in the blue electric test system. -1 At the current density, the first cycle discharge capacity is 844.7 mAh g -1 , the first Coulombic efficiency reached 90.3%.

[0056] like Figure 6 As shown, the polysulfide composite material prepared in Example 2 is -1 At the same current density, it can still maintain 759.4 mAh g after 50 cycles.-1 capacity.

[0057] Example 3

[0058] The preparation method of the conversion type cobalt polysulfide composite material of the present invention comprises the following steps:

[0059] (1) Add 1 g of Na2S 9H2O to 20 mL of deionized water, heat to 50° C. in an inert gas atmosphere by condensation reflux, and stir for 30 min to obtain a Na2S solution;

[0060] (2) Add 0.6 g of sulfur powder to the Na2S solution in step (1), heat to 140° C. in an inert gas atmosphere by condensation reflux, and stir for 12 h. When all the sulfur powder reacts, Na2S is obtained. x The obtained Na2S x The solution was cooled to room temperature and Na2S x The solution is stored in a sealed container;

[0061] (3) 0.5 g of biochar was placed in 30 mL of deionized water for ultrasonic dispersion. After 12 h of ultrasonic dispersion, a conductive agent solution was obtained. 1.1 g of CoSO4 7H2O was added to the conductive agent solution and stirred at 100 °C for 15 h to obtain a mixed solution of cobalt sulfate and conductive agent.

[0062] (4) Add the mixed solution obtained in step (3) dropwise to the Na2S x The solution was stirred at 80 °C for 12 h;

[0063] (5) The precipitate (solid product) obtained after the reaction in step (4) is washed several times with deionized water and anhydrous ethanol, and then dried in a vacuum oven at 80° C. for 10 h to obtain a cobalt polysulfide composite material.

[0064] The cobalt polysulfide composite material prepared in Example 3 was made into a positive electrode sheet, a metal lithium sheet was used as a negative electrode, Celgard 2500 was selected as a separator, and a commercial 1M LiPF6, 1:1 (v / v) carbonate electrolyte of ethylene carbonate (EC) and diethyl carbonate (DEC) was selected. The battery was assembled in an Ar-filled glove box. After the assembly was completed, a battery sealer was used to seal the battery. After standing for 12 hours, the assembled lithium-ion battery was subjected to a charge and discharge cycle performance test.

[0065] like Figure 7 The figure shows the first cycle charge and discharge curve of the cobalt polysulfide composite material prepared in Example 3 tested in the blue electric test system. -1 At the current density, the first cycle discharge capacity is 738.6 mAh g -1, the first Coulombic efficiency reached 92.6%.

[0066] like Figure 8 As shown, the polysulfide composite material prepared in Example 3 is 0.1Ag -1 At the same current density, it can still maintain 689.6 mAh g after 50 cycles. -1 capacity.

[0067] Example 4

[0068] The preparation method of the conversion type cobalt polysulfide composite material of the present invention comprises the following steps:

[0069] (1) Add 1 g of Na2S 9H2O to 20 mL of deionized water, heat to 50° C. in an inert gas atmosphere by condensation reflux, and stir for 30 min to obtain a Na2S solution;

[0070] (2) Add 0.6 g of sulfur powder to the Na2S solution in step (1), heat to 140° C. in an inert gas atmosphere by condensation reflux, and stir for 12 h. When all the sulfur powder reacts, Na2S is obtained. x The obtained Na2S x The solution was cooled to room temperature and Na2S x The solution is stored in a sealed container;

[0071] (3) 0.55 g of Ketjen black was placed in 30 mL of deionized water for ultrasonic dispersion. After ultrasonic dispersion for 12 h, a conductive agent solution was obtained. 1.2 g of CoSO4 7H2O was added to the conductive agent solution and stirred at 80 °C for 12 h to obtain a mixed solution of cobalt sulfate and the conductive agent.

[0072] (4) Add the mixed solution obtained in step (3) dropwise to the Na2S x The solution was stirred at 80 °C for 12 h;

[0073] (5) The precipitate (solid product) obtained after the reaction in step (4) is washed several times with deionized water and anhydrous ethanol, and then dried in a vacuum oven at 80° C. for 10 h to obtain a cobalt polysulfide composite material.

[0074] The cobalt polysulfide composite material prepared in Example 4 was made into a positive electrode sheet, a metal lithium sheet was used as a negative electrode, Celgard 2500 was selected as a separator, and a commercial 1M LiPF6, 1:1 (v / v) carbonate electrolyte of ethylene carbonate (EC) and diethyl carbonate (DEC) was selected. The battery was assembled in an Ar-filled glove box. After the assembly was completed, a battery sealer was used to seal the battery. After standing for 12 hours, the assembled lithium-ion battery was subjected to a charge and discharge cycle performance test.

[0075] like Fig. 9 The figure shows the first cycle charge and discharge curve of the cobalt polysulfide composite material prepared in Example 4 tested in the blue electric test system. -1 At the current density, the first cycle discharge capacity is 836.1 mAh g -1 , the first Coulombic efficiency reached 89.6%.

[0076] like Fig.10 As shown, the polysulfide composite positive electrode material prepared in Example 4 is -1 At the same current density, it can still maintain 738.6 mAh g after 50 cycles. -1 capacity.

[0077] The high sulfur content of the composite material of the present invention enables the material to have a high initial discharge specific capacity; the capacity retention of not less than 90% after 50 cycles indicates that the composite material still has a high capacity after 50 cycles, has a good retention rate and good stability.

[0078] Comparative Example 1

[0079] A method for preparing a cobalt polysulfide material comprises the following steps:

[0080] (1) Add 1 g of Na2S 9H2O to 20 mL of deionized water, heat to 50° C. in an inert gas atmosphere by condensation reflux, and stir for 30 min to obtain a Na2S solution;

[0081] (2) Add 0.6 g of sulfur powder to the Na2S solution in step (1), heat to 140° C. in an inert gas atmosphere by condensation reflux, and stir for 12 h. When all the sulfur powder reacts, Na2S is obtained. x The obtained Na2S x The solution was cooled to room temperature and Na2S x The solution is stored in a sealed container;

[0082] (3) Add 1.1 g of CoSO4 7H2O to 20 mL of deionized water and dissolve by ultrasonication to obtain a cobalt sulfate solution;

[0083] (4) Add the cobalt sulfate solution of step (3) dropwise to the Na2S x The solution was stirred at 80 °C for 12 h;

[0084] (5) The precipitate (solid product) obtained after the reaction in step (4) is washed several times with deionized water and anhydrous ethanol, and then dried in a vacuum oven at 80° C. for 10 h to obtain a cobalt polysulfide material.

[0085] The cobalt polysulfide material prepared in Comparative Example 1 was made into the positive electrode sheet, the metal lithium sheet was used as the negative electrode, Celgard2500 was selected as the separator, and a commercial 1M LiPF6, 1:1 (v / v) carbonate electrolyte of ethylene carbonate (EC) and diethyl carbonate (DEC) was selected. The battery was assembled in an Ar-filled glove box. After the assembly was completed, a battery sealer was used to seal the battery. After standing for 12 hours, the assembled lithium-ion battery was subjected to a charge and discharge cycle performance test.

[0086] like Fig.11 The figure shows the first cycle charge and discharge curve of the cobalt polysulfide material prepared in Comparative Example 1 tested in the blue electric test system. -1 At the current density, the first cycle discharge capacity is 977.7 mAh g -1 , the first Coulombic efficiency is 84.9%.

[0087] like Fig.12 As shown, the polysulfide positive electrode material prepared in Comparative Example 1 is 0.1Ag -1 At this current density, after 20 cycles, the current density was only 151 mAh g -1 The capacity of the cobalt polysulfide material can be improved by adding a conductive agent, which can improve the battery dynamics of the cobalt polysulfide material, enhance the electronic conductivity of the cobalt polysulfide, and improve the cycle stability of the battery. The material synthesized in Comparative Example 1 is pure phase cobalt polysulfide. In terms of stability, the stability of the cobalt polysulfide composite material is far superior to that of the pure phase cobalt polysulfide.

[0088] Comparative Example 2

[0089] A method for preparing an iron polysulfide composite material comprises the following steps:

[0090] (1) Add 1 g of Na2S 9H2O to 20 mL of deionized water, heat to 50° C. in an inert gas atmosphere by condensation reflux, and stir for 30 min to obtain a Na2S solution;

[0091] (2) Add 0.6 g of sulfur powder to the Na2S solution in step (1), heat to 140° C. in an inert gas atmosphere by condensation reflux, and stir for 12 h. When all the sulfur powder reacts, Na2S is obtained. x The obtained Na2S x The solution was cooled to room temperature and Na2S x The solution is stored in a sealed container;

[0092] (3) 0.5 g of biochar was placed in 30 mL of deionized water for ultrasonic dispersion. After 12 h of ultrasonic dispersion, a conductive agent solution was obtained. 1.1 g of FeSO4 7H2O was added to the conductive agent solution and stirred at 100 °C for 15 h to obtain a mixed solution of cobalt sulfate and conductive agent.

[0093] (4) Add the mixed solution obtained in step (3) dropwise to the Na2S x The solution was stirred at 80 °C for 12 h;

[0094] (5) The precipitate (solid product) obtained after the reaction in step (4) is washed several times with deionized water and anhydrous ethanol, and then dried in a vacuum oven at 80° C. for 10 h to obtain an iron polysulfide composite material.

[0095] like Fig.13 As shown in FIG. 1 , it is an XRD diagram of the iron polysulfide composite material prepared in Comparative Example 2. It can be seen from the figure that the prepared material contains crystal peaks of elemental sulfur and FeOOH. Figure 1 XRD shows that the cobalt polysulfide composite material has no other crystal peaks, indicating that the synthesized cobalt polysulfide composite material has high purity.

[0096] The test results of the cobalt polysulfide composite materials prepared in Examples 1 to 4 and the cobalt polysulfide material prepared in Comparative Example 1 are shown in Table 1.

[0097] Table 1

[0098] Test items Coulomb efficiency / % <![CDATA[Specific capacity / mAh g -1 > Capacity retention rate / % Comparative Example 1 84.9 977.7 15 Example 1 90 818 91.7 Example 2 90.3 844.7 90 Example 3 92.6 738.6 93.4% Example 4 89.6% 836.1 88.3

[0099] As shown in Table 1, the cobalt polysulfide material has a high initial discharge capacity (977.7 mAh g -1 ), showing a high sulfur content. Since the cobalt polysulfide composite material contains some conductive agent, the initial discharge capacity of pure phase cobalt polysulfide is 130-240 mAh g higher than that of the cobalt polysulfide composite material. -1 (Cobalt polysulfide composite materials contain a portion of inactive substances, which reduces the energy density of active materials. Therefore, the discharge capacity of pure phase cobalt polysulfide is higher than that of cobalt polysulfide composite materials). Since pure phase cobalt polysulfide undergoes a large volume change during the charge and discharge process, the discharge specific capacity decays rapidly.

[0100] Due to the addition of conductive agent, the conductivity of cobalt polysulfide composite material is enhanced, the volume change of cobalt polysulfide during charging and discharging is improved, and the battery electrode reaction kinetics are improved; this positive electrode material is also compatible with commercial carbonate electrolytes, avoiding the use of highly volatile and dangerous ether electrolytes, and is a highly promising next-generation high-energy-density lithium-ion battery positive electrode material.

Claims

1. A high-sulfur-content conversion-type cobalt polysulfide composite cathode material, characterized by: The composite material consists of a conductive agent and cobalt polysulfide nanoparticles loaded on the conductive agent; the cobalt polysulfide nanoparticles are in an amorphous structure.

2. The method for preparing the conversion-type cobalt polysulfide composite positive electrode material according to claim 1, characterized in that: The steps include: (1) adding sulfide to deionized water and heating it in an inert gas atmosphere by condensation reflux; (2) adding sulfur powder to the sulfide solution obtained in step (1), heating the mixture under condensation reflux in an inert gas atmosphere, and cooling the obtained polysulfide solution to room temperature after all the sulfur powder has reacted; (3) placing the conductive agent in deionized water and ultrasonically dispersing it, then adding the cobalt source to the conductive agent solution, mixing and stirring to obtain a mixed solution; (4) adding the mixed solution obtained in step (3) dropwise to the polysulfide solution in step (2), mixing and stirring to allow for sufficient reaction; (5) washing the solid product obtained after the reaction in step (4) with deionized water and anhydrous ethanol several times, and drying it in a vacuum oven after washing to obtain a cobalt polysulfide composite material.

3. The method for preparing a conversion-type cobalt polysulfide composite cathode material according to claim 2, characterized in that: In step (1), the sulfide is at least one of sodium sulfide, potassium sulfide or ammonium sulfide.

4. The method for preparing a conversion-type cobalt polysulfide composite cathode material according to claim 2, wherein: In step (1), the sulfide is heated in deionized water at a temperature of 30 to 150° C. while being stirred, and the heating time is 20 to 60 minutes.

5. The method for preparing a conversion-type cobalt polysulfide composite cathode material according to claim 2, wherein: In step (2), the molar ratio of the sulfur powder to the sulfide is 1 to 10:

1.

6. The method for preparing a conversion-type cobalt polysulfide composite cathode material according to claim 2, wherein: In step (2), the reaction temperature of the sulfur powder and the sulfide solution is 20-150° C., and the mixture is heated while being stirred for 0.05-12 h.

7. The method for preparing a conversion-type cobalt polysulfide composite cathode material according to claim 2, wherein: In step (3), the conductive agent is one of oxidized carbon nanotubes, graphene oxide, biochar or Ketjen black; and the cobalt source is one of cobalt nitrate, cobalt sulfate, cobalt chloride, cobalt acetate, cobalt carbonate or cobalt fluoride.

8. The method for preparing a conversion-type cobalt polysulfide composite cathode material according to claim 2, wherein: In step (3), the molar ratio of the cobalt source to the conductive agent is 0.1 to 100:

1.

9. The method for preparing a conversion-type cobalt polysulfide composite cathode material according to claim 2, wherein: In step (3), the ultrasonic time for forming the conductive agent solution is 10 to 1200 minutes; the stirring temperature of the conductive agent solution and the cobalt source is 30 to 100° C., and the stirring time is 1 to 24 hours.

10. The method for preparing a conversion-type cobalt polysulfide composite cathode material according to claim 2, wherein: In step (4), the molar ratio of the cobalt source to the polysulfide is 1:1; the stirring temperature of the mixed solution and the polysulfide solution is 20 to 160° C., and the stirring time is 2 to 12 hours.