Polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material and preparation method and application thereof
By coating the antimony selenide/carbon nanotube composite with polyethylene dioxythiophene, the problem of mechanical strain caused by the volume change of antimony selenide in lithium-ion batteries is solved, and high cycle stability and rate performance are improved, making it suitable for use in For lithium-ion battery anode materials.
Patent Information
- Application Number
- CN202410916271.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Mechanical strain caused by volume changes during the removal/insertion process of existing antimony selenide in lithium-ion batteries affects battery performance.
Antimony selenide/carbon nanotube composite material is coated with polyethylene dioxythiophene. Through the double-layer structure of carbon nanotubes and conductive polymer polyethylene dioxythiophene, volume expansion is suppressed and conductive channels are provided to improve cycle stability and rate. performance.
It significantly improves the cycle life and rate performance of the antimony selenide-based anode material, enhances the long-term cycle stability and rate performance of the battery, and is suitable for large-scale clean production.
Smart Images

Figure CN118738341A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of negative electrode materials for lithium ion batteries, and specifically relates to a polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material and a preparation method and application thereof. Background Art
[0002] At present, the global energy supply is still dominated by traditional fossil energy, and the many energy and environmental problems brought about by this are becoming more and more serious. New renewable energy sources such as solar energy, wind energy, and tidal energy are relatively clean, but they are highly dependent on factors such as time, region, and environment. They often need to be combined with energy storage stations to be connected to the power grid to become available resources. Electrochemical energy storage is an effective one. Among them, lithium-ion batteries have high energy density and strong stability, and have been widely used in electric vehicles, mobile device terminals, and electrical energy storage. However, after a long period of development, the graphite negative electrode material widely used in lithium-ion batteries has approached the limit of its theoretical specific capacity (372mAh g -1 ), so it is necessary to find other negative electrode materials to meet the social development demand for high energy density lithium-ion batteries.
[0003] Antimony selenide (Sb2Se3) has a high theoretical capacity (660 mAh g -1 ) and appropriate working potential. Compared with pure selenium and pure antimony materials, the synergistic effect between selenium and antimony can significantly improve the cycle stability of antimony selenide. However, antimony selenide will undergo drastic volume changes due to alloying reactions during the process of lithium extraction / insertion, causing mechanical strain, thus affecting the performance of the battery.
[0004] In view of the technical problem that the existing antimony selenide undergoes drastic volume changes during the process of lithium extraction / insertion, causing mechanical strain and thus affecting battery performance, it is urgently necessary to conduct modification research on antimony selenide and develop a low-cost, high-capacity, long-life and high-power density antimony selenide-based lithium-ion battery negative electrode material. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a polyethylene dioxythiophene (PEDOT)-coated antimony selenide / carbon nanotube composite negative electrode material and a preparation method thereof, so as to solve the technical problem that the existing antimony selenide undergoes drastic volume changes during the process of lithium extraction / insertion, causing mechanical strain and thus affecting battery performance.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention discloses a method for preparing a polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material, comprising the following steps:
[0008] Mixing antimony powder and selenium powder to obtain a mixture of antimony powder and selenium powder, adding multi-walled carbon nanotubes to the mixture of antimony powder and selenium powder and mixing evenly to obtain a mixed powder, placing the mixed powder in a vacuum atmosphere for high-temperature reaction, cooling to room temperature after the reaction, and then washing and drying to obtain an antimony selenide / carbon nanotube composite material;
[0009] The ammonium persulfate and antimony selenide / carbon nanotube composite material are added to a mixed solution of 3,4-ethylenedioxythiophene and dilute hydrochloric acid, and mixed evenly for coating. After the coating is completed, the precipitate is collected, washed and dried to obtain the polyethylenedioxythiophene coated antimony selenide / carbon nanotube composite material.
[0010] The molar ratio of the antimony powder: selenium powder is (1.9-2.1):3.0; the mass ratio of the mixture of antimony powder and selenium powder: multi-walled carbon nanotubes is (3.0-7.0):(3.0-7.0).
[0011] The step of placing the mixed powder in a vacuum atmosphere for high temperature reaction comprises:
[0012] The pressure of the vacuum atmosphere is 1×10 -5 ~1×10 -3 Pa; the high temperature reaction condition is to keep the reaction at 800-850°C for 48-60h.
[0013] The step of adding multi-walled carbon nanotubes to the mixture of antimony powder and selenium powder and mixing them uniformly comprises grinding and stirring the mixture of antimony powder and selenium powder and the multi-walled carbon nanotubes for 15 to 30 minutes; and the step of washing comprises washing with deionized water and ethanol alternately.
[0014] The mass concentration of the dilute hydrochloric acid is 0.1 M, and the volume ratio of the 3,4-ethylenedioxythiophene to the dilute hydrochloric acid is (0.9-1.1):800.
[0015] The molar ratio of ammonium persulfate to 3,4-ethylenedioxythiophene is (0.7-0.9):1.0; and the mixing and stirring time is 10-12 hours.
[0016] The mass ratio of the antimony selenide / carbon nanotube composite material to ammonium persulfate is (1.9-2.1):1.0.
[0017] The drying condition is drying at 60-80° C. for 10-12 hours.
[0018] The invention also discloses a polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material prepared according to the preparation method.
[0019] The present invention also discloses the application of the above-mentioned polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material in lithium ion batteries. The polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material is applied to a lithium ion secondary battery, wherein the lithium ion secondary battery is assembled from a counter electrode, a separator, an electrolyte and a lithium ion secondary battery working electrode sheet; the lithium ion secondary battery working electrode sheet comprises a current collector and an active material coating coated on the current collector; the current collector is a copper foil; the active material coating comprises a binder, a conductive agent and a polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite material; the mass ratio of the binder: conductive agent: polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite material is 1.0:1.0:(4.7-8.0); the binder is polyvinylidene fluoride; the conductive agent is Super-P, conductive carbon black or acetylene black.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The invention discloses a method for preparing a polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material. The method of coating antimony selenide with multi-walled carbon nanotubes and polyethylene dioxythiophene conductive polymer can suppress the large volume expansion during the cycle, thereby improving the cycle life of the antimony selenide-based negative electrode material. Antimony selenide nanoparticles are uniformly filled in the carbon nanotubes and further coated with polyethylene dioxythiophene. The double-layer structure of carbon nanotubes and conductive polymer polyethylene dioxythiophene can be used as a solid volume expansion buffer layer and conductive enhancement layer. The composite material has excellent long-cycle stability and excellent rate performance when used as a negative electrode of a lithium-ion battery. The preparation process is simple and safe, environmentally friendly, and suitable for large-scale clean production.
[0022] The present invention also discloses a polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material prepared by the above-mentioned preparation method. The polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material has distinct structural characteristics. Antimony selenide is confined in carbon nanotubes. Since the average pore size of carbon nanotubes is only 5-20nm, the nano-sizing of antimony selenide particles can be achieved. The structural stress generated by antimony selenide particles of this size during multiple lithium extraction / insertion processes is relatively small compared to large-sized antimony selenide particles, and structural collapse is not easy to occur. Carbon nanotubes, as a solid physical barrier, can buffer the volume expansion of antimony selenide and provide a three-dimensional conductive channel. Polyethylene dioxythiophene is a commonly used conjugated polymer with the advantages of high electrical conductivity, good thermal stability, etc. The polyethylene dioxythiophene coating can be used to improve the interfacial compatibility between the electrolyte and the active material, reduce side reactions during the cycle, and prevent the formation of an overly thick solid electrolyte interface. The polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material prepared by the invention has strong cycle stability, high specific capacity and excellent rate performance under the synergistic effect of the carbon nanotube and the polyethylene dioxythiophene layer.
[0023] The present invention also discloses the application of the above-mentioned polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material in lithium ion batteries. When used as a negative electrode material for lithium ion batteries, it undergoes an alloying reaction during the discharge process. During the reaction, the carbon nanotubes can accommodate the antimony selenide that undergoes volume expansion so that it does not fall off the current collector, and provide a three-dimensional conductive path; the polyethylene dioxythiophene coating layer can improve the interface compatibility between the electrolyte and the active material, reduce side reactions during the cycle process, and prevent the formation of an overly thick solid electrolyte interface. The carbon nanotubes and polyethylene dioxythiophene work together to improve the cycle stability. In view of the above characteristics, this material is very suitable for lithium ion battery negative electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following briefly introduces the drawings required for use in the embodiment:
[0025] Figure 1 This is the XRD pattern of the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material prepared in Example 1 of the present invention;
[0026] Figure 2 TEM image of the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material prepared in Example 1 of the present invention;
[0027] Figure 3 This is a Raman spectrum of the conductive polymer-coated antimony selenide / carbon nanotube composite negative electrode material prepared in Example 1 of the present invention;
[0028] Figure 4 This is a charge-discharge curve of the first cycle of the polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material prepared in Example 1 of the present invention in a lithium-ion battery at a current density of 0.1 A / g;
[0029] Figure 5 This is a cycle performance diagram of the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material prepared in Example 1 of the present invention in a lithium ion battery at a current density of 0.5 A / g;
[0030] Figure 6 This is a rate performance diagram of the polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material prepared in Example 1 of the present invention in a lithium-ion battery. DETAILED DESCRIPTION
[0031] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0032] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0033] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0034] The present invention discloses a method for preparing a polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material, comprising the following steps:
[0035] Step 1: Weigh selenium powder and antimony powder in a molar ratio, grind them evenly, add a certain amount of multi-walled carbon nanotubes (MWCNTs), stir evenly to obtain a mixture, and stir for 15 to 30 minutes;
[0036] Step 2: Transfer the mixture obtained in step 1 to a glass tube reaction container and evacuate the vacuum to a pressure of 1×10 -5 ~1×10 -3 Pa and seal, heat to 800-850℃ and keep warm for 48-60 hours, then cool naturally;
[0037] Step 3: taking out the product obtained in step 2 from the glass tube reaction container, washing the product alternately with deionized water and ethanol for multiple times, and then drying the product in an oven at 60° C. to obtain an antimony selenide / carbon nanotube composite material (Sb2Se3@MWCNTs composite material);
[0038] Step 4: Add the Sb2Se3@MWCNTs composite material described in step 3 and ammonium persulfate to a mixed solution of 3,4-ethylenedioxythiophene (EDOT) and 0.1M hydrochloric acid, and stir for 10 to 12 hours for coating. After the coating is completed, collect the precipitate, wash the precipitate with deionized water and ethanol, and place it in an oven at 80°C for 12 hours to obtain the target product, polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material (Sb2Se3@MWCNTs / PEDOT).
[0039] In step 1, the molar ratio of antimony powder:selenium powder is (1.9-2.1):3.0.
[0040] In step 1, the total mass ratio of the mixture of antimony powder and selenium powder: the mass ratio of multi-walled carbon nanotubes is (3.0-7.0): (3.0-7.0).
[0041] In step 4, the volume ratio of 3,4-ethylenedioxythiophene:dilute hydrochloric acid is 1:800.
[0042] In step 4, the molar ratio of ammonium persulfate to 3,4-ethylenedioxythiophene is (0.7-0.9):1.0.
[0043] In step 4, the mass ratio of Sb2Se3@MWCNTs to ammonium persulfate is (1.9-2.1):1.0.
[0044] The polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material prepared by the above method is used in a lithium ion battery. The specific application process is as follows:
[0045] A conductive polymer coated antimony selenide / carbon nanotube composite material is applied to a working electrode plate of a lithium-ion secondary battery. The lithium-ion secondary battery plate includes a current collector and an active material coating coated on the current collector; the active material coating includes a binder, a conductive agent and a conductive polymer coated antimony selenide / carbon nanotube composite material.
[0046] The mass ratio of the binder, the conductive agent and the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite material is 1.0:1.0:(4.7-8.0).
[0047] The current collector is copper foil, the binder is polyvinylidene fluoride, and the conductive additive is conductive carbon black, acetylene black, or Super-P.
[0048] The lithium-ion secondary battery is assembled from a counter electrode, a separator, an electrolyte and a lithium-ion secondary battery working electrode plate.
[0049] Example 1
[0050] A method for preparing a polyethylene dioxythiophene-coated antimony selenide / multi-walled carbon nanotube composite negative electrode material comprises the following steps:
[0051] 1) 32.0 mg of antimony metal powder, 29.6 mg of selenium powder and 61.6 mg of multi-walled carbon nanotubes were mixed uniformly and ground in a mortar for 30 minutes to obtain a mixture of antimony, selenium powder and multi-walled carbon nanotubes;
[0052] 2) Place the mixture obtained in step 1) in a glass tube, and evacuate the glass tube with a molecular pump to a pressure of 1.0×10 -5 When Pa, seal the glass tube;
[0053] 3) The sealed glass tube in step 2) is heated to 800°C at 1°C / min in a muffle furnace, kept at this temperature for 48 hours, and finally cooled naturally to room temperature. After the powder is taken out, it is washed alternately with deionized water and ethanol for multiple times to obtain a Sb2Se3@MWCNTs composite material. TEM image observation shows that antimony selenide is uniformly confined in the MWCNTs.
[0054] 4) Use a pipette to take 25 μl of 3,4-ethylenedioxythiophene (EDOT) and add 20 ml of 0.1 M hydrochloric acid, and stir vigorously at room temperature for 0.5 h to obtain a mixed solution of EDOT and hydrochloric acid;
[0055] 5) 78.5 mg of the Sb2Se3@MWCNTs composite material obtained in step 3) and 37.4 mg of ammonium persulfate were added to the mixed solution of EDOT and hydrochloric acid obtained in step 4), and stirred at room temperature for 10 h;
[0056] 6) The sample after stirring in step 5) was filtered and washed with deionized water and anhydrous ethanol, and finally dried in a vacuum drying oven at 80° C. for 12 h to obtain a polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material (Sb2Se3@MWCNTs / PEDOT).
[0057] Take 32 mg of the Sb2Se3@MWCNTs / PEDOT composite material prepared above, 4 mg each of acetylene black and polyvinylidene fluoride (PVDF) are added into a mortar and ground for 30 minutes, and then a few drops of N-methylpyrrolidone are added to make a uniform slurry and applied on the copper foil current collector. After vacuum drying at 110°C and standing for 12 hours, an electrode made of the Sb2Se3@MWCNTs / PEDOT composite material is obtained, and the prepared electrode is then cut into electrode sheets with a diameter of 12 mm.
[0058] A lithium sheet was used as the counter electrode of the electrode sheet, and a polypropylene film was used as the separator between the two. The electrolyte used was 1M LiPF6 with 5% FEC dissolved in an EC / DEC solution with a volume ratio of 1:1. A CR2032 half-cell was assembled in an argon-filled glove box, and constant current charge and discharge tests were carried out in a voltage window of 0.01 to 2.5 V.
[0059] The test results are as follows, see Figure 1 The XRD pattern of the polyethylene dioxythiophene coated antimony selenide / multi-walled carbon nanotube composite negative electrode material prepared in Example 1 of the present invention; Figure 1 It can be seen from the X-ray diffraction phase analysis results that the diffraction peaks of the prepared material are consistent with the standard card peaks, indicating that antimony selenide has been successfully synthesized.
[0060] See also Figure 2 TEM image of polyethylene dioxythiophene antimony selenide / multi-walled carbon nanotube composite negative electrode material prepared in Example 1 of the present invention; Figure 2 The microscopic morphology shows that antimony selenide is evenly filled into MWCNTs.
[0061] See also Figure 3 This is a Raman spectrum of the polyethylene dioxythiophene coated antimony selenide / multi-walled carbon nanotube composite negative electrode material prepared in Example 1 of the present invention; Figure 3 It can be seen that the bands observed in the Raman spectrum of Sb2Se3@MWCNTs / PEDOT (1429 and 1509 cm -1 ) is consistent with the Raman vibration of polyethylenedioxythiophene reported in the literature, indicating the successful polymerization and coating of polyethylenedioxythiophene.
[0062] See also Figure 4 is a charge-discharge curve of the first cycle of the polyethylene dioxythiophene-coated antimony selenide / multi-walled carbon nanotube composite negative electrode material prepared in Example 1 of the present invention in a lithium-ion battery at a current density of 0.1 A / g; Figure 4 It can be seen that in the lithium-ion half-cell, the electrode made of the Sb2Se3@MWCNTs / PEDOT composite material has a first discharge specific capacity of 1943 mAh / g and a charge and discharge efficiency of 52.45%.
[0063] See also Figure 5 is a cycle performance diagram of the polyethylene dioxythiophene coated antimony selenide / multi-walled carbon nanotube composite negative electrode material prepared in Example 1 of the present invention in a lithium ion battery with a current density of 0.5 A / g; Figure 5 It can be seen that in the lithium-ion half-cell, under the condition of a current density of 0.5 A / g, the electrode made of the Sb2Se3@MWCNTs / PEDOT composite material has a discharge capacity of up to 577.1 mAh / g after 150 cycles.
[0064] See also Figure 6 is a rate performance diagram of the polyethylene dioxythiophene coated antimony selenide / multi-walled carbon nanotube composite negative electrode material prepared in Example 1 of the present invention in a lithium ion battery; Figure 6It can be seen that in the lithium-ion half-cell, the reversible specific capacity of the battery negative electrode material prepared by Example 1 at current densities of 0.1, 0.2, 0.5, 1.0 and 2.0 A / g are 479.1, 414.6, 355.8, 316.7 and 281.3 mAh / g, respectively, indicating stable cycling and excellent rate performance.
[0065] Example 2
[0066] A method for preparing a polyethylene dioxythiophene-coated antimony selenide / multi-walled carbon nanotube composite negative electrode material comprises the following steps:
[0067] 1) 77.1 mg of antimony metal powder, 78.9 mg of selenium powder and 66.9 mg of multi-walled carbon nanotubes (MWCNTs) were mixed uniformly and ground in a mortar for 15 minutes to obtain a mixture of antimony metal powder, selenium powder and MWCNTs;
[0068] 2) Place the mixture obtained in step 1) in a glass tube, and evacuate the glass tube with a molecular pump to a pressure of 1.0×10 -3 When Pa, seal the glass tube;
[0069] 3) heating the sealed glass tube in step 2) to 850°C at 1°C / min in a muffle furnace, keeping the temperature for 60 hours, and finally cooling naturally to room temperature, taking out the powder and washing it alternately with deionized water and ethanol for multiple times, and finally drying the generated powder in an oven at 60°C to obtain the Sb2Se3@MWCNTs composite material;
[0070] 4) Use a pipette to take 50 μl of 3,4-ethylenedioxythiophene (EDOT) and add it to 40 ml of 0.1 M hydrochloric acid. Stir vigorously at room temperature for 0.5 h to obtain a mixed solution of EDOT and hydrochloric acid;
[0071] 5) Take 182.6 mg of the Sb2Se3@MWCNTs composite material prepared in step 3) and 96.1 mg of ammonium persulfate and add them to step 4)
[0072] The obtained mixed solution of EDOT and hydrochloric acid was stirred at room temperature for 12 h;
[0073] 6) The sample after stirring in step 5) was filtered and washed with deionized water and anhydrous ethanol, and finally dried in a vacuum drying oven at 80° C. for 12 h to obtain a polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material (Sb2Se3@MWCNTs / PEDOT).
[0074] Take 28 mg of the Sb2Se3@MWCNTs / PEDOT composite material prepared above, 6 mg each of conductive carbon black and PVDF, add them into a mortar and grind for 30 minutes, then add a few drops of N-methylpyrrolidone to make a uniform slurry and apply it on the copper foil current collector. After vacuum drying at 110°C and standing for 12 hours, an electrode made of the Sb2Se3@MWCNTs / PEDOT composite material is obtained, and then the prepared electrode is cut into electrode sheets with a diameter of 12 mm.
[0075] Example 3
[0076] A method for preparing a polyethylene dioxythiophene-coated antimony selenide / multi-walled carbon nanotube composite negative electrode material comprises the following steps:
[0077] 1) 16.0 mg of antimony metal powder, 14.8 mg of selenium powder and 71.8 mg of multi-walled carbon nanotubes (MWCNTs) were mixed uniformly and ground in a mortar for 25 minutes to obtain a mixture of antimony metal powder, selenium powder and MWCNTs;
[0078] 2) Place the mixture obtained in step 1) in a glass tube, and evacuate the glass tube with a molecular pump to a pressure of 1.0×10 -4 When Pa, seal the glass tube;
[0079] 3) The sealed glass tube in step 2) is heated to 820°C at 1°C / min in a muffle furnace, kept warm for 52 hours, and finally cooled naturally to room temperature. After the powder is taken out, it is washed alternately with carbon disulfide and ethanol for multiple times to obtain a Sb2Se3@MWCNTs composite material. TEM image observation shows that antimony selenide is uniformly confined in the pore channels of MWCNTs.
[0080] 4) Use a pipette to take 25 μl of 3,4-ethylenedioxythiophene and add 20 ml of 0.1 M hydrochloric acid, and stir vigorously at room temperature for 0.5 h to obtain a mixed solution of EDOT and hydrochloric acid;
[0081] 5) 85.4 mg of the Sb2Se3@MWCNTs composite material obtained in step 3) and 42.7 mg of ammonium persulfate were added to the mixed solution of EDOT and hydrochloric acid obtained in step 4), and stirred at room temperature for 11 h;
[0082] 6) The sample after stirring in step 5) was filtered and washed with deionized water and anhydrous ethanol, and finally dried in a vacuum drying oven at 80° C. for 12 h to obtain a polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material (Sb2Se3@MWCNTs / PEDOT).
[0083] Take 32 mg of the PEDOT-coated Sb2Se3@MWCNTs composite material prepared above, 4 mg each of Super-P and PVDF, add them into a mortar and grind for 30 minutes, then add a few drops of N-methylpyrrolidone to make a uniform slurry and apply it on the copper foil current collector. After vacuum drying at 110°C and standing for 12 hours, an electrode made of Sb2Se3@MWCNTs / PEDOT composite material is obtained, and then the prepared electrode is cut into electrode sheets with a diameter of 12 mm.
[0084] Example 4
[0085] A method for preparing a polyethylene dioxythiophene-coated antimony selenide / multi-walled carbon nanotube composite negative electrode material comprises the following steps:
[0086] 1) 16.0 mg of antimony metal powder, 14.8 mg of selenium powder and 71.8 mg of multi-walled carbon nanotubes (MWCNTs) were mixed uniformly and ground in a mortar for 25 minutes to obtain a mixture of antimony metal powder, selenium powder and MWCNTs;
[0087] 2) Place the mixture obtained in step 1) in a glass tube, and evacuate the glass tube with a molecular pump to a pressure of 1.0×10 -5 When Pa, seal the glass tube;
[0088] 3) The sealed glass tube in step 2) is heated to 830°C at 1°C / min in a muffle furnace, kept warm for 60 hours, and finally cooled naturally to room temperature. After the powder is taken out, it is washed alternately with carbon disulfide and ethanol for multiple times to obtain a Sb2Se3@MWCNTs composite material. TEM image observation shows that antimony selenide is uniformly confined in the pore channels of MWCNTs.
[0089] 4) Use a pipette to take 22.5 μl of 3,4-ethylenedioxythiophene and add 20 ml of 0.1 M hydrochloric acid, and stir vigorously at room temperature for 0.5 h to obtain a mixed solution of EDOT and hydrochloric acid;
[0090] 5) 76.8 mg of the Sb2Se3@MWCNTs composite material obtained in step 3) and 38.4 mg of ammonium persulfate were added to the mixed solution of EDOT and hydrochloric acid obtained in step 4), and stirred at room temperature for 11 h;
[0091] 6) The sample after stirring in step 5) was filtered and washed with deionized water and anhydrous ethanol, and finally dried in a vacuum drying oven at 80° C. for 12 h to obtain a polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material (Sb2Se3@MWCNTs / PEDOT).
[0092] Take 30 mg of the PEDOT-coated Sb2Se3@MWCNTs composite material prepared above, 5 mg each of Super-P and PVDF, add them into a mortar and grind for 30 minutes, then add a few drops of N-methylpyrrolidone to make a uniform slurry and apply it on the copper foil current collector. After vacuum drying at 110°C and standing for 12 hours, an electrode made of Sb2Se3@MWCNTs / PEDOT composite material is obtained, and then the prepared electrode is cut into electrode sheets with a diameter of 12 mm.
[0093] Example 5
[0094] A method for preparing a polyethylene dioxythiophene-coated antimony selenide / multi-walled carbon nanotube composite negative electrode material comprises the following steps:
[0095] 1) 81.2 mg of antimony metal powder, 79.0 mg of selenium powder and 80.1 mg of multi-walled carbon nanotubes (MWCNTs) were mixed uniformly and ground in a mortar for 25 minutes to obtain a mixture of antimony metal powder, selenium powder and MWCNTs;
[0096] 2) Place the mixture obtained in step 1) in a glass tube, and evacuate the glass tube with a molecular pump to a pressure of 1.0×10 -4 When Pa, seal the glass tube;
[0097] 3) The sealed glass tube in step 2) is heated to 850° C. at 1° C. / min in a muffle furnace, kept warm for 48 hours, and finally cooled naturally to room temperature. After taking out the powder, it is washed alternately with deionized water and ethanol for multiple times, and finally the generated powder is dried in an oven at 60° C. to obtain the Sb2Se3@MWCNTs composite material;
[0098] 4) Using a pipette, take 55 μl of 3,4-ethylenedioxythiophene (EDOT) and add it to 40 ml of 0.1 M hydrochloric acid. Stir vigorously at room temperature for 0.5 h to obtain a mixed solution of EDOT and hydrochloric acid.
[0099] 5) 200.9 mg of the Sb2Se3@MWCNTs composite material obtained in step 3) and 105.7 mg of ammonium persulfate were added to the mixed solution of EDOT and hydrochloric acid obtained in step 4), and stirred at room temperature for 12 h;
[0100] 6) The sample after stirring in step 5) was filtered and washed with deionized water and anhydrous ethanol, and finally dried in a vacuum drying oven at 80° C. for 12 h to obtain a polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material (Sb2Se3@MWCNTs / PEDOT).
[0101] Take 38 mg of the Sb2Se3@MWCNTs / PEDOT composite material prepared above, 6 mg each of conductive carbon black and PVDF, add them into a mortar and grind for 30 minutes, then add a few drops of N-methylpyrrolidone to make a uniform slurry and apply it on the copper foil current collector. After vacuum drying at 110°C and standing for 12 hours, an electrode made of the Sb2Se3@MWCNTs / PEDOT composite material is obtained, and then the prepared electrode is cut into electrode sheets with a diameter of 12 mm.
[0102] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, a person skilled in the art can still modify or make equivalent substitutions to the specific implementations of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention are within the scope of protection of the claims of the present invention to be approved.
Claims
1. A method for preparing a polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material, characterized in that: The following steps are involved: Mixing antimony powder and selenium powder to obtain a mixture of antimony powder and selenium powder, adding multi-walled carbon nanotubes to the mixture of antimony powder and selenium powder and mixing evenly to obtain a mixed powder, placing the mixed powder in a vacuum atmosphere for high-temperature reaction, cooling to room temperature after the reaction, and then washing and drying to obtain an antimony selenide / carbon nanotube composite material; The ammonium persulfate and antimony selenide / carbon nanotube composite material are added to a mixed solution of 3,4-ethylenedioxythiophene and dilute hydrochloric acid, and mixed evenly for coating. After the coating is completed, the precipitate is collected, washed and dried to obtain the polyethylenedioxythiophene coated antimony selenide / carbon nanotube composite material.
2. The method for preparing the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material according to claim 1, characterized in that: The molar ratio of the antimony powder: selenium powder is (1.9-2.1):3.0; the mass ratio of the mixture of antimony powder and selenium powder: multi-walled carbon nanotubes is (3.0-7.0):(3.0-7.0).
3. The method for preparing the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material according to claim 1, characterized in that: The step of placing the mixed powder in a vacuum atmosphere for high temperature reaction comprises: The pressure of the vacuum atmosphere is 1×10 -5 ~1×10 -3 Pa; the high temperature reaction condition is to keep the reaction at 800-850°C for 48-60h.
4. The method for preparing the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material according to claim 1, characterized in that: The step of adding multi-walled carbon nanotubes to the mixture of antimony powder and selenium powder and mixing them uniformly comprises grinding and stirring the mixture of antimony powder and selenium powder and the multi-walled carbon nanotubes for 15 to 30 minutes; and the step of washing comprises washing with deionized water and ethanol alternately.
5. The method for preparing the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material according to claim 1, characterized in that: The mass concentration of the dilute hydrochloric acid is 0.1 M, and the volume ratio of the 3,4-ethylenedioxythiophene to the dilute hydrochloric acid is (0.9-1.1):
800.
6. The method for preparing the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material according to claim 1, characterized in that: The molar ratio of ammonium persulfate to 3,4-ethylenedioxythiophene is (0.7-0.9):1.0; and the mixing and stirring time is 10-12 hours.
7. The method for preparing the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material according to claim 1, characterized in that: The mass ratio of the antimony selenide / carbon nanotube composite material to ammonium persulfate is (1.9-2.1):1.
0.
8. The method for preparing the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material according to claim 1, characterized in that: The drying condition is drying at 60-80° C. for 10-12 hours.
9. The polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the polyethylene dioxythiophene coated antimony selenide / carbon nanotube composite negative electrode material according to claim 9 in a lithium ion battery, characterized in that: The polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite negative electrode material is applied to a lithium-ion secondary battery, wherein the lithium-ion secondary battery is assembled from a counter electrode, a separator, an electrolyte, and a lithium-ion secondary battery working electrode sheet; the lithium-ion secondary battery working electrode sheet comprises a current collector and an active material coating coated on the current collector; The current collector is copper foil; the active material coating includes a binder, a conductive agent and a polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite material; the mass ratio of the binder: conductive agent: polyethylene dioxythiophene-coated antimony selenide / carbon nanotube composite material is 1.0:1.0:(4.7-8.0); The binder is polyvinylidene fluoride; the conductive agent is Super-P, conductive carbon black or acetylene black.
Citation Information
Patent Citations
Carbon / ferric oxide / multi-walled carbon nanotube composite material for negative electrode of lithium ion battery and preparation method
CN110492080A
Tin selenide-nitrogen doped carbon nanotube composite material and preparation method thereof, lithium ion battery negative electrode plate and lithium ion battery
CN115602834A
Preparation method and application of polyethylene dioxythiophene coated iron diselenide
CN116314706A
Conductive polymer coated tin phosphide / ordered mesoporous carbon composite negative electrode material as well as preparation method and application thereof
CN117790733A
Synthesis method for controlling antimony selenide nanostructure shapes
US9598283B1