Positive electrode material and preparation method and application thereof
By constructing a specific relationship to control the mass ratio of the cladding material and the core material, and adopting appropriate process methods, the contradiction between the energy density and interface stability of the cathode material is solved, and battery performance with high energy density and long life is achieved. .
Patent Information
- Application Number
- CN202411009686.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-25
AI Technical Summary
It is difficult for existing cathode materials to achieve high interface stability and low impedance while increasing energy density, and the coating effect is poor, resulting in insufficient battery cycle stability and lifespan.
By constructing a specific relationship to control the mass ratio of the coating material and the core material, combined with the preset activation and sintering temperatures, the spray drying method, solid phase grinding method or fluidized bed mixing method is used to form a coating layer to improve the performance of the cathode material. Interfacial stability and energy density.
It achieves high energy density and interface stability of the cathode material, extends the cycle life and structural stability of the battery, and improves the competitiveness and safety performance of the battery.
Smart Images

Figure CN118738348A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of batteries, and in particular to positive electrode materials and preparation methods and applications thereof. Background Art
[0002] With the development of the new energy industry, the requirements for battery life are getting higher and higher, so the battery needs to have a higher energy density. By increasing the upper charging limit voltage of the positive electrode material, thereby increasing the reversible capacity and voltage platform of the positive electrode material, the purpose of improving its energy density can be achieved. However, as the voltage increases, the stability of the positive electrode material decreases. By coating the positive electrode material, the interface stability of the positive electrode material can be improved, thereby improving the cycle stability of the battery. However, in the related art, the coating effect of the positive electrode material is poor, the agglomeration phenomenon is many, the reaction activity is low, and the specific surface area is small. It is difficult to obtain an ideal interface stability, and it is easy to cause the impedance of the positive electrode material to increase. Therefore, a method for preparing a positive electrode material that can improve the coating effect is needed to obtain a positive electrode material with both high interface stability and low impedance, which is conducive to improving the energy density of the positive electrode material. Summary of the invention
[0003] In view of this, the present application provides a positive electrode material and a preparation method and application thereof. In the preparation of the positive electrode material, the coating material and the core material are weighed according to a specific relationship constructed by the particle size of the core material, the particle size of the coating material, the preset activation temperature and the sintering temperature, so as to control the mass ratio of the coating material to the core material within a suitable range, which is beneficial to improving the coating effect of the positive electrode material, so as to obtain a positive electrode material with both high interface stability and low impedance, and is beneficial to improving the energy density of the positive electrode material.
[0004] In the first aspect, the present application provides a method for preparing a positive electrode material, weighing a first mass M1 of a coating material and a second mass M2 of a core material, mixing the weighed core material and the coating material, activating them at a first preset temperature, and then sintering them at a second preset temperature to obtain a positive electrode material; wherein the ratio M1 / M2 of the first mass M1 to the second mass M2 satisfies: M1 / M2={[A×(D50 particle size of the coating material / D10 particle size of the core material)]+[B×(coating The first preset temperature is within the range of 800°C-850°C, and the second preset temperature is within the range of 850°C-900°C.
[0005] Optionally, the D50 particle size of the coating material is 0.01 μm-20 μm, and the D50 particle size of the core material is 0.05 μm-100 μm.
[0006] Optionally, the D10 particle size of the core material is 0.01 μm-10 μm, and the D90 particle size of the core material is 0.05 μm-500 μm.
[0007] Optionally, the D50 particle size of the coating material is smaller than the D50 particle size of the core material.
[0008] Optionally, the difference between the D99 particle size of the coating material and the D50 particle size of the coating material is 100nm-5000nm.
[0009] Optionally, the difference between the D99 particle size of the coating material and the D10 particle size of the coating material is 300nm-3000nm.
[0010] Optionally, the coating material includes one or more of lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, lithium lanthanum zirconium oxide, lithium lanthanum zirconium titanium oxide, lithium aluminum zirconium phosphate, lithium zirconium phosphate, lithium molybdate, lithium niobate, lithium phosphate, lithium aluminum phosphate, lithium fluoroaluminum phosphate, lithium tantalate, lithium titanium phosphate, lithium aluminum silicate, lithium nickel manganese oxide, iridium phosphate, lithium cobalt phosphate, lithium aluminum cobalt phosphate, lithium aluminum vanadium phosphate and lithium vanadium manganese phosphate.
[0011] Optionally, the chemical formula of the core material is Li a Mn b Ni c Co d Al e O2, where a≥1; b+c+d=1 and e=0, or c+d+e=1 and b=0, or b+c+d+e=1 and c≥33.
[0012] Optionally, the mixing method includes one or more of spray drying, solid phase grinding, solid phase mixing and fluidized bed mixing.
[0013] Optionally, the sintering atmosphere includes one or more of oxygen, nitrogen and argon.
[0014] The preparation method of the positive electrode material provided in the present application weighs the coating material and the core material according to a specific relationship constructed by the particle size of the core material, the particle size of the coating material, the preset activation temperature and the sintering temperature, so as to control the mass ratio of the coating material to the core material within a suitable range, which is beneficial to improving the coating effect of the positive electrode material, so as to improve the interface stability of the positive electrode material, and further help to improve the energy density of the positive electrode material.
[0015] In a second aspect, the present application provides a positive electrode material, wherein the positive electrode material is a positive electrode material prepared by the preparation method described in the first aspect.
[0016] Optionally, the positive electrode material includes a core and a coating layer coated on the surface of the core; the core includes the core material, and the coating layer includes the coating material; in the positive electrode material, the mass percentage of the coating layer is 0.1%-10%.
[0017] Optionally, the particle size D50 of the positive electrode material is 0.05 μm-100 μm.
[0018] Optionally, the specific surface area of the positive electrode material is 0.1 m 2 / g-20m 2 / g.
[0019] The positive electrode material provided in the present application has excellent coating effect, high energy density and good interface stability.
[0020] In a third aspect, the present application provides a positive electrode plate, comprising a positive electrode collector and a positive electrode active material layer arranged on the surface of the positive electrode collector, wherein the positive electrode active material layer comprises the positive electrode material prepared by the preparation method described in the first aspect or the positive electrode material described in the second aspect.
[0021] The positive electrode plate provided in the present application has high specific capacity, good structural stability and long service life.
[0022] In a fourth aspect, the present application provides a battery, comprising a negative electrode plate and the positive electrode plate described in the third aspect.
[0023] The battery provided in this application has good cycle stability and high reliability, which is conducive to improving the product competitiveness of the battery.
[0024] In a fifth aspect, the present application provides an electrical device, wherein the electrical device comprises the battery described in the fourth aspect.
[0025] The electrical equipment provided in this application has excellent safety performance and good electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the embodiments or the prior art description. The specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0027] Figure 1 A schematic diagram of the cross-sectional structure of a positive electrode material provided in one embodiment of the present application;
[0028] Figure 2This is a scanning electron microscope image of the positive electrode material prepared in Example 1 of the present application;
[0029] Figure 3 This is a scanning electron microscope image of the positive electrode material prepared in Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0031] The present application provides a method for preparing a positive electrode material, comprising: weighing a first mass M1 of a coating material and a second mass M2 of a core material, mixing the weighed core material and the coating material, activating them at a first preset temperature, and then sintering them at a second preset temperature to obtain a positive electrode material; wherein the ratio M1 / M2 of the first mass M1 to the second mass M2 satisfies: M1 / M2={[A×(D50 particle size of the coating material / D10 particle size of the core material)]+[B×(D50 particle size of the coating material / D10 particle size of the core material)] The first preset temperature is within the range of 800°C-850°C, and the second preset temperature is within the range of 850°C-900°C. The preparation method of the positive electrode material provided in the present application weighs the coating material and the core material according to a specific relationship constructed by the particle size of the core material, the particle size of the coating material, the preset activation temperature and the sintering temperature, so as to control the mass ratio of the coating material to the core material within a suitable range, which is beneficial to improving the coating effect of the positive electrode material. The coating layer with suitable thickness and / or coating method can obtain a positive electrode material with high interface stability and low impedance, which is beneficial to improving the rate performance and energy density of the positive electrode material.
[0032] In one embodiment of the present application, the coating material forms a coating layer on the surface of the core. Specifically, the coating material may include, but is not limited to, lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, lithium lanthanum zirconium oxide, lithium lanthanum zirconium titanium oxide, lithium aluminum zirconium phosphate, lithium zirconium phosphate, lithium molybdate, lithium niobate, lithium phosphate, lithium aluminum phosphate, lithium fluoroaluminum phosphate, lithium tantalate, lithium titanium phosphate, lithium aluminum silicate, lithium nickel manganese oxide, iridium phosphate, lithium cobalt phosphate, lithium aluminum cobalt phosphate, lithium aluminum vanadium phosphate and lithium vanadium manganese oxide. In one embodiment of the present application, the coating material may be lithium phosphate. In another embodiment of the present application, the coating material may be lithium nickel manganese oxide.
[0033] In one embodiment of the present application, the D50 particle size of the coating material is 0.01μm-20μm. The D50 particle size of the appropriate coating material can improve the coating effect and enhance the energy density and interface stability of the positive electrode material. Specifically, the D50 particle size of the coating material may be, but is not limited to, 0.01μm, 1μm, 2μm, 5μm, 8μm, 0.01μm, 10μm, 15μm or 20μm, etc. In one embodiment of the present application, the D50 particle size of the coating material may be 0.01μm-10μm. In another embodiment of the present application, the D50 particle size of the coating material may be 8μm-20μm.
[0034] In one embodiment of the present application, the difference between the D99 particle size of the coating material and the D50 particle size of the coating material is 100nm-5000nm. Controlling the overall particle size distribution of the coating material can improve the matching degree of the particle size distribution of the coating material and the core material, improve the coating effect of the coating material on the core material, avoid the formation of voids, and help to form a uniform, dense and thin coating layer on the surface of the core, thereby better taking into account the low impedance and interface stability of the positive electrode material, and helping to improve the energy density of the positive electrode material. Specifically, the difference between the D99 particle size of the coating material and the D50 particle size of the coating material can be, but is not limited to, 100nm, 150nm, 200nm, 500nm, 1200nm, 2000nm, 3000nm, 4000nm or 5000nm, etc. In one embodiment of the present application, the difference between the D99 particle size of the coating material and the D50 particle size of the coating material is 100nm-2000nm, which can further promote the coating of the coating material to the core material and improve the coating effect.
[0035] In one embodiment of the present application, the difference between the D99 particle size of the coating material and the D10 particle size of the coating material is 300nm-3000nm. Controlling the overall particle size distribution of the coating material can improve the matching degree of the particle size distribution of the coating material and the core material, improve the coating effect of the coating material on the core material, avoid the formation of voids, and facilitate the formation of a uniform, dense and thin coating layer on the surface of the core. Specifically, the difference between the D99 particle size of the coating material and the D10 particle size of the coating material can be, but is not limited to, 300nm, 500nm, 800nm, 1000nm, 1500nm, 2000nm, 2500nm or 3000nm, etc. In one embodiment of the present application, the difference between the D99 particle size of the coating material and the D10 particle size of the coating material can be 300nm-1500nm, which can further improve the coating effect of the positive electrode material and improve the electrochemical performance of the positive electrode material.
[0036] In one embodiment of the present application, the chemical formula of the core material is Li a Mn b Nic Co d Al e O2, where a≥1; b+c+d=1 and e=0, or c+d+e=1 and b=0, or b+c+d+e=1, and c≥33. In one embodiment of the present application, when a≥1, b+c+d=1 and e=0, the chemical formula of the core material can be Li a Mn b Ni c Co d O2, in this case, a can be 1, b can be 0.2, c can be 0.3, d can be 0.5, and the core material can be LiMn 0.2 Ni 0.3 Co 0.5 In another embodiment of the present application, when a≥1, c+d+e=1 and b=0, the chemical formula of the core material can be Li a Ni c Co d Al e O2, in this case, a can be 1, c can be 0.2, d can be 0.4, e can be 0.4, and the core material can be LiNi 0.2 Co 0.4 Al 0.4 In another embodiment of the present application, when a≥1, b+c+d+e=1, and c≥33, the chemical formula of the core material can be Li a Mn b Ni c Co d Al e O2, at this time, a can be 1, b is 0.1, c is 0.7, d is 0.1, e is 0.1, at this time, the core material can be LiMn 0.1 Ni 0.7 Co 0.1 Al 0.1 O2.
[0037] In one embodiment of the present application, the D90 particle size of the core material is 0.05μm-500μm. The D90 particle size of the appropriate core material can improve the coating effect, and enhance the energy density and interface stability of the positive electrode material. Specifically, the D90 particle size of the core material may be, but is not limited to, 0.05μm, 50μm, 100μm, 200μm, 300μm, 350μm, 400μm or 500μm, etc. In one embodiment of the present application, the D90 particle size of the core material may be 0.05μm-150μm. In another embodiment of the present application, the D90 particle size of the core material may be 100μm-500μm.
[0038] In one embodiment of the present application, the D50 particle size of the core material is 0.05μm-100μm. The D50 particle size of the appropriate core material can improve the coating effect, and enhance the energy density and interface stability of the positive electrode material. Specifically, the D50 particle size of the core material may be, but is not limited to, 0.05μm, 10μm, 20μm, 40μm, 60μm, 80μm, 90μm or 100μm, etc. In one embodiment of the present application, the D50 particle size of the core material may be 0.05μm-20μm. In another embodiment of the present application, the D50 particle size of the core material may be 20μm-100μm.
[0039] In one embodiment of the present application, the D50 particle size of the coating material is larger than the D50 particle size of the core material, which is conducive to forming a uniform and thin coating layer on the surface of the core, avoiding the occurrence of uneven coating layer and shedding, improving the coating effect of the coating material, and enhancing the electrochemical performance of the positive electrode material.
[0040] In one embodiment of the present application, the D10 particle size of the core material is 0.01 μm-10 μm. Specifically, the D50 particle size of the coating material may be, but is not limited to, 0.01 μm, 1 μm, 2 μm, 5 μm, 8 μm, 0.01 μm, 10 μm, 15 μm or 20 μm, etc. In one embodiment of the present application, the D50 particle size of the coating material may be 0.01 μm-10 μm. In another embodiment of the present application, the D50 particle size of the coating material may be 8 μm-20 μm.
[0041] In one embodiment of the present application, A is a proportional coefficient of the ratio between the D50 particle size of the coating material and the D10 particle size of the core material, 0.01≤A≤0.1, specifically, the value of A can be, but is not limited to, 0.01, 0.02, 0.04, 0.06, 0.08 or 0.1, etc. In one embodiment of the present application, the value of A can be 0.01-0.06. In another embodiment of the present application, the value of A can be 0.04-0.1. The D50 particle size of the coating material and the D10 particle size of the core material are the same unit.
[0042] In one embodiment of the present application, B is a proportional coefficient of the ratio between the D50 particle size of the coating material and the D50 particle size of the core material, 0.001≤B≤0.09. Specifically, the value of B can be, but is not limited to, 0.001, 0.002, 0.008, 0.01, 0.02, 0.04, 0.06 or 0.09, etc. In one embodiment of the present application, the value of B can be 0.001-0.04. In another embodiment of the present application, the value of B can be 0.03-0.09. The D50 particle size of the coating material and the D50 particle size of the core material are the same unit.
[0043] In one embodiment of the present application, C is a proportional coefficient of the ratio between the D50 particle size of the coating material and the D90 particle size of the core material, 0.002≤C≤0.1. Specifically, the value of C can be, but is not limited to, 0.002, 0.005, 0.008, 0.01, 0.02, 0.04, 0.06, 0.08 or 0.1, etc. In one embodiment of the present application, the value of C can be 0.002-0.08. In another embodiment of the present application, the value of C can be 0.07-0.1. The D50 particle size of the coating material and the D90 particle size of the core material are the same unit.
[0044] In one embodiment of the present application, the first preset temperature is 800°C-850°C. At the first preset temperature, activating the coating material can promote the subsequent uniform bonding of the coating material on the surface of the core material, thereby improving the coating effect. Specifically, the first preset temperature may be, but is not limited to, 800°C, 810°C, 820°C, 830°C, 840°C or 850°C. In one embodiment of the present application, the first preset temperature may be 800°C-830°C. In another embodiment of the present application, the first preset temperature may be 825°C-850°C.
[0045] In one embodiment of the present application, the second preset temperature is 850°C-900°C. The second preset temperature can make the coating material firmly coated and bonded to the surface of the core material to form a coating layer, which is conducive to improving the stability of the positive electrode material. Specifically, the second preset temperature can be, but is not limited to, 850°C, 860°C, 870°C, 880°C, 890°C or 900°C. In one embodiment of the present application, the second preset temperature can be 850°C-870°C. In another embodiment of the present application, the second preset temperature can be 865°C-900°C.
[0046] In one embodiment of the present application, D is an optimization parameter of the first preset temperature and the second preset temperature, and 20≤D≤100. Specifically, the value of D can be, but is not limited to, 20, 40, 50, 60, 80 or 100, etc.
[0047] In one embodiment of the present application, K is a correction parameter for the amount of coating material used, and 0.5≤K≤1. Since the coating material will be lost and fail during the sintering process, the correction value K is required to correct the amount of coating material used to improve the coating efficiency of the coating material. Specifically, the value of K can be, but is not limited to, 0.5, 0.6, 0.7, 0.8, 0.9 or 1. In one embodiment of the present application, the value of K can be 0.5-0.8. In another embodiment of the present application, the value of K can be 0.7-1.
[0048] In one embodiment of the present application, the mixing method of the coating material and the core material may include but is not limited to one or more of spray drying, solid phase grinding, solid phase mixing and fluidized bed mixing, which can promote the uniform mixing of the coating material and the core material and improve the coating effect of the coating material. In one embodiment of the present application, the mixing method may be spray drying. In another embodiment of the present application, the mixing method may be solid phase grinding.
[0049] In one embodiment of the present application, the sintering atmosphere may include, but is not limited to, one or more of oxygen, nitrogen and argon. In one embodiment of the present application, the sintering atmosphere may be oxygen.
[0050] The present application also provides a positive electrode material, which is prepared by the preparation method of any one of the above embodiments. The positive electrode material provided by the present application has high interface stability and excellent energy density, and can improve the specific capacity and electrochemical performance of the positive electrode sheet.
[0051] See also Figure 1 , is a schematic diagram of the cross-sectional structure of a positive electrode material provided in one embodiment of the present application, wherein the positive electrode material 100 includes a core 10 and a coating layer 20 coated on the surface of the core 10, wherein the core 10 includes a core material, and the core 10 is obtained by sintering the core material, and the coating layer 20 includes a coating material, and the coating layer 20 is obtained by sintering the coating material.
[0052] In one embodiment of the present application, in the positive electrode material, the mass percentage of the coating layer is 0.1%-10%. The appropriate amount of coating layer mass can maintain the excellent energy density of the positive electrode material, improve the coating effect of the positive electrode material, and enhance the interface stability of the positive electrode material. Specifically, in the positive electrode material, the mass percentage of the coating layer can be, but is not limited to, 0.1%, 1%, 2%, 4%, 6%, 8% or 10%, etc. In one embodiment of the present application, in the positive electrode material, the mass percentage of the coating layer can be 0.1%-5%. In another embodiment of the present application, in the positive electrode material, the mass percentage of the coating layer can be 3%-10%.
[0053] In one embodiment of the present application, the coating layer may be coated in a point-like manner or / and an island-like manner. Point-like coating means that after the coating material is sintered, the coating material is distributed in a granular state on the surface of the inner core to form a coating layer. Island-like coating means that after the coating material is sintered, the coating material is coated in an agglomerated state on the surface of the inner core to form a coating layer.
[0054] In one embodiment of the present application, the particle size D50 of the positive electrode material is 0.05μm-100μm. The D50 particle size of a suitable positive electrode material can improve the energy density and cycle stability of the battery. Specifically, the D50 particle size of the positive electrode material may be, but is not limited to, 0.05μm, 10μm, 20μm, 40μm, 60μm, 80μm, 90μm or 100μm, etc. In one embodiment of the present application, the D50 particle size of the positive electrode material may be 0.05μm-20μm. In another embodiment of the present application, the D50 particle size of the positive electrode material may be 20μm-100μm.
[0055] In one embodiment of the present application, the specific surface area of the positive electrode material is 0.1 m 2 / g-20m 2 / g. A suitable specific surface area can increase the compaction density of the positive electrode sheet and improve the capacity density of the battery. Specifically, the specific surface area of the positive electrode material can be, but is not limited to, 0.1 m 2 / g, 1m 2 / g, 5m 2 / g, 8m 2 / g, 10m 2 / g, 12m 2 / g, 15m 2 / g or 20m 2 In one embodiment of the present application, the specific surface area of the positive electrode material can be 0.1 m 2 / g-10m 2 In another embodiment of the present application, the specific surface area of the positive electrode material is 10m 2 / g-20m 2 / g.
[0056] The present application provides a positive electrode plate, the positive electrode plate comprising a positive electrode current collector and a positive electrode active material layer arranged on the surface of the positive electrode current collector, the positive electrode active material layer comprising the positive electrode material described in any one of the above embodiments. The positive electrode material provided by the present application has good coating effect, high specific capacity, large specific surface area, high reaction activity, and is conducive to improving the energy density and electrochemical performance of the positive electrode plate.
[0057] In one embodiment of the present application, the positive electrode current collector has good conductivity and high electrochemical stability, which can improve the electrochemical stability of the positive electrode sheet. Specifically, the positive electrode current collector can be, but is not limited to, one of nickel, titanium, aluminum, stainless steel, aluminum coated with carbon or nickel, and stainless steel coated with carbon or nickel. In one embodiment of the present application, the positive electrode current collector can be aluminum foil. In some embodiments, the surface of the positive electrode current collector is rough or mesh-like, which can improve the bonding strength between the positive electrode active material layer and the positive electrode current collector. In some embodiments, the shape of the positive electrode current collector can be one or more of a film, a sheet, a foil, a mesh, and a porous body.
[0058] In one embodiment of the present application, the thickness of the positive electrode current collector is 1 μm-500 μm. Specifically, the thickness of the positive electrode current collector may be, but is not limited to, 1 μm, 10 μm, 100 μm, 200 μm, 300 μm, 400 μm or 500 μm. In one embodiment of the present application, the thickness of the positive electrode current collector may be 1 μm-300 μm. In another embodiment of the present application, the thickness of the positive electrode current collector may be 250 μm-500 μm.
[0059] In one embodiment of the present application, the positive electrode active material layer further includes a positive electrode binder and a positive electrode conductor, which can improve the structural stability and electrochemical performance of the positive electrode sheet.
[0060] In one embodiment of the present application, the positive electrode binder can improve the structural stability of the positive electrode sheet, which is beneficial to improve the cycle life of the positive electrode sheet. Specifically, the positive electrode binder can be, but is not limited to, one or more of polyvinylidene fluoride, fluoroethylene-hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, polyacrylic acid, polyethylene oxide polytetrafluoroethylene and hydrogenated nitrile rubber. In one embodiment of the present application, the positive electrode binder can be polyvinylidene fluoride.
[0061] In one embodiment of the present application, the weight average molecular weight of the positive electrode binder is 50000-500000, which can improve the stability and uniformity of the positive electrode sheet. Specifically, the weight average molecular weight of the positive electrode binder can be, but is not limited to, 50000, 100000, 200000, 300000, 400000 or 500000. In one embodiment of the present application, the weight average molecular weight of the positive electrode binder can be 50000-300000. In another embodiment of the present application, the weight average molecular weight of the positive electrode binder can be 250000-500000.
[0062] In one embodiment of the present application, the positive electrode conductive agent can improve the conductivity of the positive electrode plate. Specifically, the positive electrode conductive agent can be, but is not limited to, one or more of acetylene black, conductive carbon black, graphene, and carbon nanotubes. In one embodiment of the present application, the positive electrode conductive agent can be acetylene black.
[0063] The present application also provides a battery, which includes the positive electrode plate described in any one of the above embodiments, and can improve the service life and electrochemical performance of the battery.
[0064] In one embodiment of the present application, the battery further comprises a negative electrode plate, the negative electrode plate comprising a negative electrode current collector and a negative electrode active layer disposed on the surface of the negative electrode current collector. Specifically, the negative electrode current collector may include, but is not limited to, one or more of copper, aluminum, nickel and stainless steel. In one embodiment of the present application, the negative electrode current collector may be copper foil.
[0065] In one embodiment of the present application, the negative electrode active layer includes a negative electrode active material, and the negative electrode active material may include, but is not limited to, one or more of silicon, tin, germanium, lithium, and alloys thereof, and carbon materials. Among them, the carbon material may include, but is not limited to, one or more of non-graphitized carbon, graphite, pyrolytic carbon, coke, and activated carbon. In one embodiment of the present application, the negative electrode active material may be a carbon material. In another embodiment of the present application, the negative electrode active material may be a silicon alloy (an alloy material formed by Si and one or more of Ti, Fe, Co, Ni, and Cu).
[0066] In one embodiment of the present application, the negative electrode active layer also includes a negative electrode conductive agent. The negative electrode conductive agent can increase the conductivity between active materials and improve electronic conductivity. Specifically, the negative electrode conductive agent may include but is not limited to one or more of acetylene black, conductive carbon black, graphene and carbon nanotubes. In one embodiment of the present application, the negative electrode conductive agent may be graphite. In another embodiment of the present application, the negative electrode conductive agent may be carbon black.
[0067] In one embodiment of the present application, the negative electrode active layer further includes a negative electrode binder, which can improve the binding ability of the components in the negative electrode active layer and improve the binding ability between the negative electrode active layer and the negative electrode current collector. Specifically, the negative electrode binder can be, but is not limited to, one or more of polyvinylidene fluoride, polyacrylate, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose and styrene-butadiene rubber. In one embodiment of the present application, the negative electrode binder can be polyvinylidene fluoride.
[0068] In one embodiment of the present application, the battery further comprises an electrolyte. At least part of the positive electrode sheet and at least part of the negative electrode sheet are immersed in the electrolyte, and the electrolyte comprises an electrolyte and an organic solvent. Specifically, the electrolyte may be, but is not limited to, one or more of LiPF6, LiBF4, LiCl, LiAlCl4, LiSbF6, LiSCN, LiCF3SO3, LiCF3CO2, LiN(CF3SO2) and LiAsF6, and the organic solvent may be, but is not limited to, one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate and vinylene carbonate.
[0069] In the present application, the battery also includes a diaphragm, which can perform ion exchange and form a complete ion conduction path. Specifically, the diaphragm can be but not limited to a woven membrane, a non-woven fabric, a microporous membrane, a composite membrane, a rolled membrane or a diaphragm paper, and the material of the diaphragm can be but not limited to polyethylene, polypropylene, polyvinylidene fluoride and a composite membrane.
[0070] The present application also provides an electrical device, which includes the battery described in any of the above embodiments. The electrical device provided in the present application has high energy density, good cycle performance, and high safety performance. Electrical equipment includes vehicles, electronic equipment, energy storage systems, etc., wherein the electronic equipment may include, for example, mobile phones, tablets, watches, VR glasses, etc. In one embodiment of the present application, the battery can be used in vehicles, which can improve the service life and cycle performance of the vehicle, improve the widespread application of new energy vehicles, and facilitate the construction of a green and environmentally friendly environment. In another embodiment of the present application, the battery can also be used in mobile phones, which can reduce the preparation cost of the battery and improve the safety of battery use. The above-mentioned battery of the present application can be arranged in the electrical equipment in the form of a single cell, a battery module, a battery pack, etc.
[0071] The effect of the technical solution of the present application is further illustrated below through specific examples.
[0072] Example 1
[0073] A method for preparing a positive electrode material, comprising:
[0074] (1) Select a core material (lithium cobalt oxide) and a coating material (nano-lithium aluminum titanium phosphate), wherein the D50 particle size of the coating material is 412 nm, the D90 particle size of the core material is 27168 nm, the D50 particle size of the core material is 16360 nm, and the D10 particle size of the core material is 5190 nm. Set the first preset temperature to 850 ° C, the second preset temperature to 850 ° C, take A to 0.01, B to 0.001, C to 0.002, D to 100, and K to 1. According to the relationship M1 / M2={[A×(D50 particle size of coating material / D10 particle size of core material)]+[B×(D50 particle size of coating material / D50 particle size of core material)]+[C×(D50 particle size of coating material / D90 particle size of core material)]}×[1+second preset temperature / (D×first preset temperature)] / K, the ratio of the mass M1 of the coating material to the mass M2 of the core material is calculated to be M1 / M2=0.000858;
[0075] (2) According to M1 / M2=0.000858, 0.429 g of coating material and 500 g of core material were weighed, and the core material and coating material were placed in a 1.0 L ball mill, and 500 g of large, medium and small zirconium beads were added. The mixture was covered with a lid and placed on a jar mill for ball milling for 6 h. The coating material and core material that were evenly mixed were then placed in a sagger, placed in a muffle furnace, activated at a first preset temperature for 2 h, and then sintered at a second preset temperature for 8 h to obtain a positive electrode material.
[0076] Example 2
[0077] The difference from Example 1 is that the first preset temperature is set to 800°C, the second preset temperature is set to 900°C, A is taken as 0.1, B is 0.09, C is 0.1, D is 20, K is 0.5, and M1 / M2 is calculated to be 0.0248; based on M1 / M2=0.0248, 12.381g of coating material and 500g of core material are weighed.
[0078] Example 3
[0079] The difference from Example 1 is that the first preset temperature is set to 820°C, the second preset temperature is set to 870°C, A is taken as 0.013, B is 0.009, C is 0.0041, D is 20, K is 0.67, and M1 / M2 is calculated to be 0.00208. According to M1 / M2=0.00208, 1.038g of coating material and 500g of core material are weighed.
[0080] Example 4
[0081] The difference from Example 1 is that the first preset temperature is set to 850°C, the second preset temperature is set to 900°C, A is taken as 0.013, B is 0.009, C is 0.0041, D is 79, K is 0.67, and M1 / M2 is calculated to be 0.00200. According to M1 / M2=0.00200, 0.999g of coating material and 500g of core material are weighed.
[0082] Example 5
[0083] The difference from Example 1 is that the D50 particle size of the coating material is 48nm, the D90 particle size of the core material is 26186nm, the D50 particle size of the core material is 16986nm, and the D10 particle size of the core material is 4972nm. It is calculated that M1 / M2=0.000104. According to M1 / M2=0.000104, 0.052g of coating material and 500g of core material are weighed.
[0084] Example 6
[0085] The difference from Example 1 is that the D50 particle size of the coating material is 48nm, the D90 particle size of the core material is 26186nm, the D50 particle size of the core material is 16986nm, the D10 particle size of the core material is 4972nm, the first preset temperature is set to 800°C, and the second preset temperature is set to 900°C; A is taken as 0.1, B is 0.09, C is 0.1, D is 20, and K is 0.5, and M1 / M2=0.00296 is calculated. According to M1 / M2=0.00296, 1.482g of coating material and 500g of core material are weighed.
[0086] Example 7
[0087] The difference from Example 1 is that the D50 particle size of the coating material is 2549 nm, A is 0.01, B is 0.001, C is 0.002, D is 100, and K is 1, and M1 / M2=0.00531 is calculated. Based on M1 / M2=0.00531, 2.654 g of coating material and 500 g of core material are weighed.
[0088] Example 8
[0089] The difference from Example 1 is that the D50 particle size of the coating material is 2549 nm, A is 0.1, B is 0.09, C is 0.1, D is 100, and K is 1, and M1 / M2 is calculated to be 0.0732. Based on M1 / M2=0.0732, 36.622 g of coating material and 500 g of core material are weighed.
[0090] Example 9
[0091] The difference from Example 1 is that the D50 particle size of the coating material is 2549nm, the D90 particle size of the core material is 25481nm, the D50 particle size of the core material is 14681nm, and the D10 particle size of the core material is 4268nm. Taking A as 0.01, B as 0.001, C as 0.002, D as 100, and K as 1, it is calculated that M1 / M2=0.00641. According to M1 / M2=0.00641, 3.205g of coating material and 500g of core material are weighed.
[0092] Example 10
[0093] The difference from Example 1 is that the D50 particle size of the coating material is 2549nm, the D90 particle size of the core material is 25481nm, the D50 particle size of the core material is 14681nm, the D10 particle size of the core material is 4268nm, the first preset temperature is set to 800°C, the second preset temperature is set to 900°C, A is taken as 0.1, B is taken as 0.09, C is taken as 0.1, D is taken as 20, and K is taken as 0.5, and M1 / M2=0.180 is calculated. According to M1 / M2=0.180, 90.155g of coating material and 500g of core material are weighed.
[0094] Comparative Example 1
[0095] The difference from Example 1 is that 0.248 g of the coating material and 500 g of the core material are weighed, and the mass ratio of the coating material to the core material is less than M1 / M2.
[0096] Comparative Example 2
[0097] The difference from Example 2 is that 20 g of the coating material and 500 g of the core material are weighed, and the mass ratio of the coating material to the core material is greater than M1 / M2.
[0098] Performance Testing
[0099] The positive electrode materials prepared in the above Examples 1 to 10 and Comparative Examples 1 to 2 were mixed with a binder and a conductive agent and dissolved in N-methylpyrrolidone to obtain a positive electrode slurry, wherein the mass ratio of the positive electrode material, the conductive agent and the binder was 100:3:2; the positive electrode slurry was coated on a single side of a 16 μm thick positive electrode current collector aluminum foil, and then dried with air at 85° C. for 24 h, cold pressed and vacuum dried to obtain a positive electrode sheet.
[0100] The positive electrode sheets, separators and negative electrode sheets prepared in the above-mentioned embodiments 1 to 10 and comparative examples 1 to 2 are stacked and wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging foil, the electrolyte is injected into the dried battery cell, and then the battery is obtained through vacuum packaging, standing, forming, shaping and other processes; wherein, the preparation of the negative electrode sheet: the negative electrode active material (artificial graphite), conductive agent, binder and thickener are dissolved in a solvent (deionized water) in a mass ratio of 97:1:1.5:0.5 to prepare a negative electrode slurry, which is coated on the front and back sides of the negative electrode collector copper foil, and then dried at 80°C for 20 hours, cold pressed and vacuum dried to obtain a negative electrode sheet.
[0101] The batteries prepared in the above-mentioned Examples 1 to 10 and Comparative Examples 1 to 2 were subjected to rate performance tests. The test process was as follows: the batteries were allowed to stand for 5 minutes at 25°C, charged at a constant current of 0.1C to a voltage of 4.60V, then charged at a constant voltage of 4.60V to a current of 0.05C, allowed to stand for 5 minutes, and then discharged at constant currents of 0.1C and 1C to a voltage of 3.0V, respectively. Four lithium-ion batteries were taken from each group for testing, and the average value was taken; the rate performance (%) of the battery = the discharge capacity of the second cycle of the battery at 1C / the discharge capacity of the first cycle of the battery at 0.1C × 100%. The test results are shown in Table 1.
[0102] The batteries prepared in the above-mentioned Examples 1 to 10 and Comparative Examples 1 to 2 were subjected to a low temperature performance test. The test process was as follows: the battery was allowed to stand for 5 minutes at 25°C, charged at a constant current of 0.1C to a voltage of 4.60V, then charged at a constant voltage of 4.60V to a current of 0.05C, and allowed to stand for 5 minutes. The battery was allowed to stand for 60 minutes at -20°C, and then discharged at a constant current of 1C to a voltage of 3.0V. Four batteries were taken from each group for testing, and the average value was taken; the low temperature performance of the battery (%) = the discharge capacity of the battery at -20°C, 1C / the discharge capacity of the battery in the first cycle at 0.1C × 100%. The test results are shown in Table 1.
[0103] The batteries prepared in the above-mentioned Examples 1 to 10 and Comparative Examples 1 to 2 were subjected to a high temperature performance test. The test process was as follows: the battery was left at rest for 60 minutes at 45°C, charged at a constant current of 0.5C to a voltage of 4.60V, then charged at a constant voltage of 4.60V to a current of 0.05C, and left at rest for 5 minutes. Then, it was discharged at a constant current of 0.5C to a voltage of 3.0V, and this cycle was repeated for 50 cycles. Four batteries were taken from each group for testing, and the average value was taken. The high temperature cycle performance of the battery (%) = the discharge capacity of the battery at 0.5C after 50 cycles / the discharge capacity of the battery at 0.5C in the first cycle × 100%. The test results are shown in Table 1.
[0104] Figure 2 This is a scanning electron microscope image of the positive electrode material prepared in Example 1 of the present application. Figure 3 This is a scanning electron microscope image of the positive electrode material prepared in comparative example 1 of the present application. It can be seen that the surface of the positive electrode material of Example 1 is smoother than that of the positive electrode material of comparative example 1, indicating that the coating material can be closely combined with the core material, significantly improving the protective effect of the coating material on the positive electrode material.
[0105] Table 1 Battery performance test results
[0106] Rate performance (%) Low temperature performance(%) High temperature cycle performance (%) Example 1 91 78 80 Example 2 93 81 82 Example 3 89 81 82 Example 4 92 83 81 Example 5 93 76 83 Example 6 94 78 85 Example 7 94 78 79 Example 8 90 75 76 Example 9 93 81 84 Example 10 91 80 82 Comparative Example 1 85 68 71 Comparative Example 2 75 51 70
[0107] According to Examples 1 to 10 and Comparative Examples 1 to 2, it can be seen that the ratio M1 / M2 of the coating material of the first mass M1 and the core material of the second mass M2 of the positive electrode material provided in the present application satisfies a specific relationship constructed by the particle size of the core material, the particle size of the coating material, the preset activation temperature and the sintering temperature, which improves the coating uniformity of the coating material, and the battery has excellent rate performance, low temperature performance and high temperature cycle performance, which is beneficial to improve the energy density and cycle life of the battery. According to Example 1 and Comparative Example 1, it can be seen that in the present application, the positive electrode material obtained by satisfying the specific relationship can achieve a close combination of the coating layer and the core, enhance the protective effect of the coating material on the positive electrode material, and enhance the cycle stability of the coating material.
[0108] The above is a preferred embodiment of the present application, but it should not be understood as limiting the scope of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A method for preparing a positive electrode material, characterized in that: include: Weighing a first mass M1 of coating material and a second mass M2 of core material, mixing the weighed core material and the coating material, activating them at a first preset temperature, and then sintering them at a second preset temperature to obtain a positive electrode material; Among them, the ratio M1 / M2 of the first mass M1 to the second mass M2 satisfies: M1 / M2={[A×(D50 particle size of coating material / D10 particle size of core material)]+[B×(D50 particle size of coating material / D50 particle size of core material)]+[C×(D50 particle size of coating material / D90 particle size of core material)]}×[1+second preset temperature / (D×first preset temperature)] / K, 0.01≤A≤0.1, 0.001≤B≤0.09, 0.002≤C≤0.1, 20≤D≤100, 0.5≤K≤1; the first preset temperature is in the range of 800℃-850℃, and the second preset temperature is in the range of 850℃-900℃.
2. The preparation method according to claim 1, characterized in that The D50 particle size of the coating material is 0.01 μm-20 μm, the D50 particle size of the core material is 0.05 μm-100 μm, the D10 particle size of the core material is 0.01 μm-10 μm, and the D90 particle size of the core material is 0.05 μm-500 μm.
3. The preparation method according to claim 1, characterized in that: The D50 particle size of the coating material is smaller than the D50 particle size of the core material.
4. The preparation method according to claim 1, characterized in that: The difference between the D99 particle size of the coating material and the D50 particle size of the coating material is 100nm-5000nm, and the difference between the D99 particle size of the coating material and the D10 particle size of the coating material is 300nm-3000nm.
5. The preparation method according to claim 1, characterized in that: The coating material includes one or more of lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, lithium lanthanum zirconium oxide, lithium lanthanum zirconium titanium oxide, lithium zirconium aluminum phosphate, lithium zirconium phosphate, lithium molybdate, lithium niobate, lithium phosphate, lithium aluminum phosphate, lithium fluoroaluminum phosphate, lithium tantalate, lithium titanium phosphate, lithium aluminum silicate, lithium nickel manganese oxide, iridium phosphate, lithium cobalt phosphate, lithium cobalt aluminum phosphate, lithium aluminum vanadium phosphate and lithium vanadium manganese phosphate.
6. The preparation method according to claim 1, characterized in that: The chemical formula of the core material is Li a Mn b Ni c Co d Al e O2, Among them, a≥1; b+c+d=1 and e=0, or c+d+e=1 and b=0, or b+c+d+e=1, and c≥0.
33.
7. The preparation method according to claim 1, characterized in that: The mixing method includes one or more of spray drying, solid phase grinding, solid phase mixing and fluidized bed mixing; The sintering atmosphere includes one or more of oxygen, nitrogen and argon.
8. A positive electrode material, characterized in that The positive electrode material is prepared by the preparation method according to any one of claims 1 to 7.
9. The positive electrode material according to claim 8, characterized in that The positive electrode material comprises a core and a coating layer coated on the surface of the core; the core comprises the core material, and the coating layer comprises the coating material; In the positive electrode material, the mass percentage of the coating layer is 0.1%-10%.
10. The positive electrode material according to claim 8, characterized in that The particle size D50 of the positive electrode material is 0.05 μm-100 μm, and the specific surface area of the positive electrode material is 0.1 m 2 / g-20m 2 / g.
11. A positive electrode sheet, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer arranged on the surface of the positive electrode current collector, and the positive electrode active material layer comprises the positive electrode material prepared by the preparation method according to any one of claims 1 to 7 or the positive electrode material according to any one of claims 8 to 10.
12. A battery, characterized in that: The battery comprises a negative electrode sheet and the positive electrode sheet according to claim 11.
13. An electrical equipment, characterized in that: The electrical device comprises the battery according to claim 12.
Citation Information
Patent Citations
Positive electrode active material and preparation method thereof, positive electrode plate and lithium battery
CN115663165A
Multi-doped composite coated lithium cobalt oxide positive electrode material as well as preparation method and application thereof
CN116314669A
Positive electrode material and preparation method thereof, positive electrode plate and battery
CN117352709A
Quaternary positive electrode material for lithium ion battery and preparation method therefor, and lithium ion battery
WO2021068448A1
High-nickel ternary positive electrode material using lithium fast-ion conductor as coating layer, preparation method therefor, and application thereof
WO2024113626A1
Cited By
Composite lithium cobalt oxide positive electrode material, preparation method thereof, positive electrode plate and lithium ion battery
CN119725480A