Negative electrode material and preparation method thereof, negative electrode plate and battery

Through the composite material of hard carbon graphite particles and silicon-based particles, and the coating structure of porous hard carbon layer and soft carbon layer, the problem of insufficient capacity and fast charging performance of lithium-ion batteries during fast charging is solved, and high capacity is achieved. and excellent cycle performance.

CN118738385APending Publication Date: 2024-10-01BEIJING ELECTRIC VEHICLE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410710285.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing graphite materials are difficult to meet the high capacity and fast charging performance requirements of lithium-ion batteries, especially when performing poor performance during fast charging.

Method used

It uses a composite material of hard carbon graphite particles and silicon-based particles. Through the coating structure of porous hard carbon layer and soft carbon layer, the insertion and extraction of ions is faster, increasing the interface transmission channel of lithium ions, and improving the fast charging and cycle of the battery. performance.

Benefits of technology

It achieves the high capacity of the battery and excellent fast charging performance, while improving the cycle performance to ensure the stability and efficiency of the battery during fast charging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738385A_ABST
    Figure CN118738385A_ABST
Patent Text Reader

Abstract

The invention discloses a negative electrode material and a preparation method thereof, a negative electrode plate and a battery. The negative electrode material comprises an inner core and a shell layer, the inner core comprises hard carbon graphite particles and silicon-based particles, the hard carbon graphite particles comprise a graphite material and a porous hard carbon layer, and the porous hard carbon layer coats the graphite material; the silicon-based particles are adjacent to the hard carbon graphite particles; the shell layer covers the inner core, the shell layer comprises a soft carbon layer and isotropic particles, and the isotropic particles are embedded into the soft carbon layer. The battery prepared from the negative electrode material not only has high capacity, but also has excellent quick charge performance and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries, and in particular relates to a negative electrode material and a preparation method thereof, a negative electrode plate and a battery. Background Art

[0002] Graphite materials have the advantages of low charge and discharge platform, good cycle performance, low price, and environmental friendliness. They are currently the most ideal and most commonly used negative electrode materials for lithium-ion batteries. However, as consumer electronics, especially the field of power batteries, put forward higher and higher requirements for fast charging, the negative electrode materials prepared from existing graphite materials are difficult to meet the requirements of battery fast charging performance. Therefore, special design and processing are required to make the graphite negative electrode material meet the performance requirements of high battery capacity and fast charging at the same time. Summary of the invention

[0003] The present invention aims to solve one of the technical problems in the related art to at least some extent. To this end, one object of the present invention is to provide a negative electrode material and a preparation method thereof, a negative electrode sheet and a battery. The battery prepared using the negative electrode material not only has a high capacity, but also has excellent fast charging performance and cycle performance.

[0004] In one aspect of the present invention, the present invention provides a negative electrode material. According to an embodiment of the present invention, it includes:

[0005] A kernel, the kernel comprising:

[0006] Hard carbon graphite particles, the hard carbon graphite particles comprising a graphite material and a porous hard carbon layer, the porous hard carbon layer coating the graphite material;

[0007] silicon-based particles, the silicon-based particles being adjacent to the hard carbon graphite particles;

[0008] The outer shell layer covers the inner core, and the outer shell layer includes a soft carbon layer and isotropic particles, wherein the isotropic particles are embedded in the soft carbon layer.

[0009] According to the negative electrode material of the above embodiment of the present invention, it includes an inner core and an outer shell layer, the inner core includes hard carbon graphite particles and silicon-based material particles, the hard carbon graphite particles include graphite material and a porous hard carbon layer, the porous hard carbon layer covers the graphite material, so that ions can be quickly embedded or removed, so the above hard carbon graphite particles enable the battery to have a high rate charging capability. The silicon-based particles are adjacent to the hard carbon graphite particles, which can significantly improve the battery capacity and the cycle performance of the battery. The outer shell layer covers the inner core, and the outer shell layer includes a soft carbon layer and isotropic particles. The isotropic particles are embedded in the soft carbon layer, and the isotropic particles and the soft carbon layer together form a coating layer on the surface. The isotropic particles are also a graphite material with high isotropy, and lithium ions can be more efficiently embedded in the coating layer. Therefore, the outer shell composite coating layer can significantly increase the lithium insertion and extraction channels on the surface of the negative electrode material particles, which helps Li + Rapid interface transmission effectively improves the fast charging characteristics of the negative electrode material. Therefore, the battery prepared using the negative electrode material not only has high capacity, but also has excellent fast charging performance and cycle performance.

[0010] In addition, the negative electrode material according to the above embodiment of the present invention may also have the following technical features:

[0011] In some embodiments of the present invention, the mass ratio of the hard carbon graphite particles to the silicon-based particles is (100-75): (10-1). Thus, the battery prepared from the negative electrode material has a high rate charging capability.

[0012] In some embodiments of the present invention, the mass ratio of the silicon-based particles to the soft carbon layer is (10-1):(15-1). Thus, the specific capacity and cycle performance of the battery can be improved.

[0013] In some embodiments of the present invention, the mass ratio of the core to the isotropic particles is (100-80):(20-1). Thus, the fast charging performance of the battery can be improved.

[0014] In some embodiments of the present invention, the mass ratio of the graphite material to the porous hard carbon layer is (80-90):(20-10).

[0015] In some embodiments of the present invention, the particle size of the silicon-based particles is 1 μm-10 μm, thereby improving the specific capacity and cycle performance of the battery.

[0016] In some embodiments of the present invention, the particle size of the isotropic particles is 100 nm to 500 nm, thereby improving the fast charging performance of the battery.

[0017] In some embodiments of the present invention, the isotropic particles include at least one of mesocarbon microbeads and solid pitch.

[0018] In some embodiments of the present invention, the thickness of the outer shell layer is 100 nm to 600 nm, thereby improving the fast charging performance of the battery.

[0019] In another aspect of the present invention, the present invention provides a method for preparing the above-mentioned negative electrode material. According to an embodiment of the present invention, the method comprises:

[0020] (1) mixing a graphite material precursor and a hard carbon material precursor, performing a first carbonization treatment and then a graphitization treatment to obtain hard carbon graphite particles;

[0021] (2) mixing the hard carbon graphite particles, the silicon-based material and the binder and performing negative pressure low-temperature melt granulation to obtain secondary composite particles;

[0022] (3) The secondary composite particles and the isotropic fine particles are mixed and subjected to a second carbonization treatment to obtain a negative electrode material.

[0023] According to the method for preparing negative electrode materials of the above embodiment of the present invention, a graphite material precursor and a hard carbon material precursor are first mixed and then subjected to a first carbonization treatment and then a graphitization treatment. The first carbonization treatment causes the hard carbon material precursor to change from a solid phase to a liquid phase at a high temperature, and then coats the surface of the graphite material precursor to form a dense hard carbon coating layer. At the same time, the graphite material precursor can remove ash and volatile components in the material at a high temperature. In the process of discharging the volatile components, a coating layer with a porous structure, i.e., a porous hard carbon layer, is formed. During the graphitization treatment, the graphite material precursor will form a layered graphite material at a high temperature, and since the porous hard carbon layer is difficult to graphitize, a hard carbon layer with a porous structure will still be retained on the surface of the graphite material, thereby obtaining hard carbon graphite particles. The structure of the porous hard carbon layer coating the graphite material allows ions to be quickly embedded or removed, so the above-mentioned hard carbon graphite particles enable the battery to have a high-rate charging capability. The hard carbon graphite particles, silicon-based materials and binder are then mixed and subjected to negative pressure low-temperature melt granulation to prepare secondary composite particles. The binder will melt at low temperatures and fully infiltrate into the solid particles under negative pressure, which can effectively fill the pores between the particles, thereby making the hard carbon graphite particles and silicon-based materials more densely bonded, thereby making the tap density of the secondary composite particles higher, which can effectively improve the processing performance. At the same time, the composite particles can also effectively reduce the expansion problem of silicon particles during the cycle process. The silicon-based particles are closely adjacent to the hard carbon graphite particles, which can significantly improve the battery capacity and battery cycle performance. The secondary composite particles and isotropic particles are mixed for a second carbonization treatment. Because the secondary composite particles contain a certain proportion of binder, the binder will melt at the second carbonization temperature, so a soft carbon layer will be formed on the surface of the secondary composite particles (hard carbon graphite particles and silicon-based material composite particles), and the isotropic particles are embedded in the soft carbon layer. The isotropic particles and the soft carbon layer together form a coating layer on the surface. The isotropic particles are also a kind of graphite material. The isotropic properties of this material are relatively high, and lithium ions can be more efficiently embedded in the coating layer. Therefore, the outer shell layer significantly increases the lithium deintercalation channel on the surface of the negative electrode material particles, which helps Li + Rapid interface transmission effectively improves the fast charging characteristics of the negative electrode material. Therefore, the method can be used to prepare a negative electrode material with high capacity, fast charging performance and excellent cycle performance. Specifically, the particle size D 50 7μm~15μm, tap density not less than 1g / cm 3 , the specific surface area is not more than 2m 2 / g.

[0024] In addition, the method for preparing the negative electrode material according to the above embodiment of the present invention may also have the following technical features:

[0025] In some embodiments of the present invention, the D of the graphite material precursor V50The thickness is 5 μm to 20 μm. This can increase the capacity of the negative battery.

[0026] In some embodiments of the present invention, the graphite material precursor includes at least one of petroleum coke, oil-based needle coke, coal-based needle coke, natural graphite and flake graphite.

[0027] In some embodiments of the present invention, the hard carbon material precursor includes at least one of phenolic resin, furfuryl alcohol resin, epoxy resin, polyurethane, starch and sugar organic matter.

[0028] In some embodiments of the present invention, the temperature of the first carbonization treatment is 1000° C. to 1300° C., and the time of the first carbonization treatment is 10 h to 20 h. Thus, the hard carbon material precursor can be carbonized to form a carbonized layer.

[0029] In some embodiments of the present invention, the temperature of the graphitization treatment is 2800° C. to 3000° C., and the time of the graphitization treatment is 24 hours to 48 hours. Thus, the graphite material precursor can be graphitized.

[0030] In some embodiments of the present invention, the negative pressure low temperature melt granulation has a pressure of 0 to -0.8 MPa, a temperature of 300°C to 700°C, and a granulation time of 6 hours to 12 hours, thereby improving the capacity and fast charging performance of the negative electrode material.

[0031] In some embodiments of the present invention, the binder includes at least one of petroleum asphalt and coal asphalt.

[0032] In some embodiments of the present invention, the temperature of the second carbonization treatment is 1200° C. to 1400° C., and the time of the second carbonization treatment is 10 hours to 20 hours. Thus, the fast charging performance of the battery can be improved.

[0033] In a third aspect of the present invention, the present invention provides a negative electrode sheet. According to an embodiment of the present invention, the negative electrode sheet includes the above-mentioned negative electrode material or the negative electrode material prepared by the above-mentioned method. Thus, a battery prepared by using the negative electrode sheet has a high capacity and excellent fast charging performance and cycle performance.

[0034] In a fourth aspect of the present invention, the present invention provides a battery. According to an embodiment of the present invention, the battery includes the above-mentioned negative electrode plate. As a result, the battery has high capacity, excellent fast charging performance and cycle performance. Specifically, the initial capacity of the battery is between 350mAh / g and 500mAh / g, and the initial efficiency is greater than 90%.

[0035] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0037] Figure 1 Schematic diagram of the structure of the negative electrode material of an embodiment of the present invention. DETAILED DESCRIPTION

[0038] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but should not be construed as limiting the present invention.

[0039] In one aspect of the present invention, the present invention provides a negative electrode material. According to an embodiment of the present invention, reference Figure 1 The negative electrode material includes: a core 100 and an outer shell layer 200 .

[0040] According to an embodiment of the present invention, the core 100 includes hard carbon graphite particles 110 and silicon-based particles 120, the hard carbon graphite particles 110 include graphite material 111 and porous hard carbon layer 112, the porous hard carbon layer 112 covers the graphite material 111, and the silicon-based particles 120 are adjacent to the hard carbon graphite particles 110. The porous hard carbon layer 112 covers the graphite material 111, so that ions can be quickly embedded or extracted, and thus the hard carbon graphite particles 110 enable the battery to have a high rate charging capability. The silicon-based particles 120 are adjacent to the hard carbon graphite particles 110, so that the battery capacity and the cycle performance of the battery can be significantly improved.

[0041] According to an embodiment of the present invention, the mass ratio of hard carbon graphite particles 110 to silicon-based particles 120 is (100-75): (10-1). The inventors found that since the theoretical capacity of graphite is about 372 mAh / g, the capacity of silicon negative electrode material can reach 1400-4200 mAh / g. Mixing graphite and silicon negative electrode in a certain proportion can greatly improve the capacity of the composite negative electrode material, especially controlling the mass ratio of hard carbon graphite particles 110 to silicon-based particles 120 within the above range, which can significantly improve the capacity of the battery and the cycle performance of the battery. Furthermore, the mass ratio of graphite material and porous hard carbon layer is (80-90): (20-10).

[0042] According to an embodiment of the present invention, the outer shell 200 covers the inner core 100, and the outer shell 200 includes a soft carbon layer 210 and isotropic particles 220, and the isotropic particles 220 are embedded in the soft carbon layer 210. The outer shell includes a soft carbon layer 210 and isotropic particles 220, and the isotropic particles 220 are embedded in the soft carbon layer 210. The isotropic particles 220 and the soft carbon layer 210 together form a coating layer (outer shell 200) on the surface. The isotropic particles are also a graphite material with high isotropy. Lithium ions can be more efficiently embedded in the outer shell 200. Therefore, the outer shell 200 significantly increases the lithium deintercalation channel on the surface of the negative electrode material particles, which helps Li + Fast interface transmission effectively improves the fast charging characteristics of negative electrode materials.

[0043] According to an embodiment of the present invention, the mass ratio of the silicon-based particles 120 to the soft carbon layer 210 is (10-1): (15-1). The inventors have found that when the mass ratio of the silicon-based particles 120 to the soft carbon layer 210 is within the above range, the rebound characteristics of the silicon material can be more effectively suppressed while ensuring the cycle performance of the composite material. If the silicon content is too high, the overall particle structure may break with the increase of cycles, which may lead to cell failure.

[0044] According to an embodiment of the present invention, the mass ratio of the core 100 to the isotropic particles 220 is (100-80): (20-1). The inventors found that the isotropic particles 220 belong to a graphite-like material with less volatile matter, but the soft carbon raw material contains volatile matter. By mixing the two substances, the soft carbon raw material can be used as a binder to bond the isotropic particles to the surface of the graphite silicon-based composite particles during the manufacturing process. Controlling the mass ratio of the core 100 to the isotropic particles 220 within the above range can reduce the expansion problem of the silicon-carbon material, increase the rate of lithium ion embedding, and thereby improve the fast charging performance of the negative electrode material.

[0045] According to an embodiment of the present invention, the particle size of the silicon-based particles 120 is 1 μm-10 μm. The inventors found that the particle size of the silicon-based particles 120 cannot be too large, otherwise the overall performance of the negative electrode material will be reduced. The particle size of the silicon-based particles 120 is controlled within the above range, which can improve the specific capacity and cycle performance of the battery.

[0046] According to an embodiment of the present invention, the particle size of the isotropic particles 220 is 100nm to 600nm. The inventors have found that the particle size of the isotropic particles 220 is controlled within the above range, the particle size of the graphite and silicon-based composite particles is at the micron level, and the particle size of the coating agent is at the nanometer level, so that they can be evenly coated on the surface of the composite particles. Furthermore, the isotropic particles 220 include at least one of mesophase carbon microspheres and solid asphalt. These materials need to be selected with high isotropy, which can effectively increase the transmission channel of lithium ions, thereby improving the transmission rate of lithium ions. It should be noted that the raw material D of the isotropic particles 220 is 50 The particle size of the isotropic particles 220 is controlled to be between 10 μm and 20 μm by wet grinding at the nanometer level (100 nm to 600 nm). The specific process is as follows: the raw material is mixed with anhydrous ethanol or other solvents to prepare a slurry, the solid content of the slurry is controlled to be 10 to 30%, the slurry is ground in a ball mill for 1 to 5 hours, and the slurry is sprayed into a spray drying device at a temperature of about 90° C. and a flow rate of about 5 mL / min for spray drying (the grinding balls in the ball mill become metal oxides of non-magnetic substances, such as zirconium oxide).

[0047] According to an embodiment of the present invention, the thickness of the outer shell layer 200 is 100nm to 500nm. The inventors found that the outer shell layer 200 is mainly used as a coating layer for coating the inner core 100, so the thickness of the outer shell layer 200 is controlled within the above range. The coating thickness or coating amount will affect the performance of the battery cell. By effectively controlling the coating amount, the fast charging and cycle performance of the battery cell can be met while ensuring the performance of the battery cell capacity and other performances.

[0048] In another aspect of the present invention, the present invention provides a method for preparing the above-mentioned negative electrode material. According to an embodiment of the present invention, the method comprises:

[0049] S100: Mixing the graphite material precursor and the hard carbon material precursor for a first carbonization treatment and then a graphitization treatment

[0050] In this step, the graphite material precursor and the hard carbon material precursor are mixed and then subjected to a first carbonization treatment and then a graphitization treatment. The first carbonization treatment causes the hard carbon material precursor to change from a solid phase to a liquid phase at a high temperature, and then is coated on the surface of the graphite material precursor to form a dense hard carbon coating layer. At the same time, the graphite material precursor can remove the ash and volatile components in the material at a high temperature. In the process of discharging the volatile components, a coating layer with a porous structure, i.e., a porous hard carbon layer, is formed. During the graphitization treatment, the graphite material precursor will form a layered graphite material at a high temperature, and since the porous hard carbon layer is difficult to graphitize, a hard carbon layer with a porous structure will still be retained on the surface of the graphite material, thereby obtaining hard carbon graphite particles. The structure of the porous hard carbon layer coating the graphite material allows ions to be quickly embedded or removed, so the above-mentioned hard carbon graphite particles enable the battery to have a high rate charging capability. It should be noted that the graphite material precursor and the hard carbon material precursor are conventional materials in the field, and those skilled in the art can select them according to actual conditions. For example, the graphite material precursor includes at least one of petroleum coke, oil-based needle coke, coal-based needle coke, natural graphite and flake graphite; the hard carbon material precursor includes at least one of phenolic resin, furfuryl alcohol resin, epoxy resin, polyurethane, starch and sugar organic matter.

[0051] According to an embodiment of the present invention, D of the graphite material precursor V50 The inventors found that the D of the graphite material precursor V50 Controlled within the above range, if the particle size is too small, the compaction and specific surface area of ​​the material will be large, which is not conducive to the energy density and cycle performance of the battery cell. If the particle size is large, the power performance of the battery cell will be reduced. Therefore, the material within this particle size range can ensure the comprehensive performance of the battery cell.

[0052] According to an embodiment of the present invention, the temperature of the first carbonization treatment is 1000°C to 1300°C, and the time of the first carbonization treatment is 10h to 20h. The inventors have found that by controlling the temperature and time of the first carbonization within the above range, the hard carbon material precursor can be carbonized to form a carbonized layer. Furthermore, the temperature of the graphitization treatment is 2800°C to 3000°C, and the time of the graphitization treatment is 24h to 48h, so that the graphite material precursor can be graphitized.

[0053] S200: Mix hard carbon graphite particles, silicon-based materials and binders for negative pressure low-temperature melting granulation

[0054] In this step, hard carbon graphite particles, silicon-based materials and binders are mixed and subjected to negative pressure low-temperature melt granulation to prepare secondary composite particles. The binder will melt at low temperatures and fully infiltrate the solid particles under negative pressure, which can effectively fill the pores between the particles, thereby making the hard carbon graphite particles and silicon-based materials more densely bonded, thereby making the tap density of the secondary composite particles higher, which can effectively improve the processing performance. At the same time, the composite particles can also effectively reduce the expansion problem of silicon particles during the cycle process. The silicon-based particles are closely adjacent to the hard carbon graphite particles, which can significantly improve the battery capacity and the cycle performance of the battery. It should be noted that silicon-based materials and binders are conventional materials in the field, and those skilled in the art can choose according to actual conditions. For example, silicon-based materials include but are not limited to at least one of silicon oxide and silicon carbon; binders include but are not limited to at least one of petroleum asphalt and coal asphalt.

[0055] According to an embodiment of the present invention, the pressure of negative pressure low temperature melt granulation is 0 to -0.8Mpa, the temperature is 300°C to 700°C, and the granulation time is 6h to 12h. The inventors found that when the pressure, temperature and time of negative pressure low temperature melt granulation are controlled within the above range, the binder can be fully melted and infiltrated into the solid particles, effectively filling the pores between the particles, and increasing the tap density of the particles, thereby improving the capacity and fast charging performance of the negative electrode material.

[0056] S300: Mixing secondary composite particles and isotropic particles for second carbonization treatment

[0057] In this step, the secondary composite particles and the isotropic particles are mixed for a second carbonization treatment. Because the secondary composite particles contain a certain proportion of a binder, the binder will melt at the second carbonization temperature, thereby forming a soft carbon layer on the surface of the secondary composite particles (hard carbon graphite particles and silicon-based material composite particles), and the isotropic particles are embedded in the soft carbon layer. The isotropic particles and the soft carbon layer together form a coating layer on the surface. The isotropic particles are also a graphite material with high isotropy. Lithium ions can be more efficiently embedded in the coating layer. Therefore, the outer shell layer significantly increases the lithium deintercalation channel on the surface of the negative electrode material particles, which helps Li + Rapid interface transmission effectively improves the fast charging characteristics of the negative electrode material. Furthermore, the temperature of the second carbonization treatment is 1200°C to 1400°C, and the time of the second carbonization treatment is 10h to 20h, thereby improving the fast charging performance of the battery.

[0058] In the third aspect of the present invention, the present invention proposes a negative electrode plate. According to an embodiment of the present invention, the negative electrode plate comprises the above-mentioned negative electrode material or the negative electrode material prepared by the above-mentioned method. As a result, the battery prepared by the negative electrode plate has a high capacity and excellent fast charging performance and cycle performance. It should be noted that the above-mentioned features and advantages described for the negative electrode material and the preparation of the negative electrode material are also applicable to the negative electrode plate, which will not be repeated here.

[0059] In a fourth aspect of the present invention, the present invention provides a battery. According to an embodiment of the present invention, the battery includes the above-mentioned negative electrode plate. As a result, the battery has high capacity, excellent fast charging performance and cycle performance. It should be noted that the features and advantages described above for the negative electrode plate are also applicable to the battery and will not be repeated here.

[0060] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0061] Example 1

[0062] (1) 15 μm petroleum coke and phenolic resin were mixed in a VC mixer at a mass ratio of 90:10 for 2 h, then transferred to a push plate furnace for carbonization at 1100°C for 15 h, and then the carbonized powder was transferred to an Aixun graphitization furnace for high-temperature graphitization at 3000°C for 36 h, and hard carbon graphite particles were obtained after crushing, screening, and demagnetization;

[0063] (2) mixing hard carbon graphite particles with 5 μm silicon oxide and binder asphalt in a mass ratio of 85:10:5 for 2 h, transferring them to a vertical reactor, controlling the initial inner cavity pressure of the reactor at -0.8 MPa, and reacting at 500 °C for 8 h to obtain secondary composite particles;

[0064] (3) The secondary composite particles were mixed with 200 nm isotropic particles (solid asphalt) in a mass ratio of 90:10, and then transferred to an orbital kiln for carbonization at 1250°C for 15 h to form an outer shell layer coated with hard carbon graphite particles and silicon oxide. The thickness of the outer shell layer was 210 nm. After screening and demagnetization, a high-capacity fast-charging negative electrode material was obtained.

[0065] Example 2

[0066] (1) 12 μm needle coke and starch were mixed in a VC mixer at a mass ratio of 80:20 for 3 h, then transferred to a push plate furnace for carbonization at 1300°C for 15 h, and then the carbonized powder was transferred to an Aixun graphitization furnace for high-temperature graphitization at 3000°C for 48 h, and hard carbon graphite particles were obtained after crushing, screening, and demagnetization;

[0067] (2) mixing hard carbon graphite particles with 5 μm silicon oxide and binder asphalt in a mass ratio of 90:5:5 for 2 h, then transferring them to a vertical reactor, controlling the initial inner cavity pressure of the reactor at -0.3 MPa, and reacting at 600 °C for 12 h to obtain secondary composite particles;

[0068] (3) The secondary composite particles were mixed with 500 nm isotropic particles (solid asphalt) in a mass ratio of 92:8, and then transferred to an orbital kiln for carbonization at 1250°C for 15 h to form an outer shell layer coated with hard carbon graphite particles and silicon oxide. The thickness of the outer shell layer was 508 nm. After screening and demagnetization, a high-capacity fast-charging negative electrode material was obtained.

[0069] Example 3

[0070] (1) 12 μm petroleum coke and epoxy resin were mixed in a conical mixer at a mass ratio of 85:15 for 3 h, then transferred to a push plate furnace for carbonization at 1250°C for 15 h, and then the carbonized powder was transferred to an Aixun graphitization furnace for high-temperature graphitization at 3000°C for 48 h, and hard carbon graphite particles were obtained after crushing, screening, and demagnetization;

[0071] (2) mixing hard carbon graphite particles with 4 μm silicon oxide and binder asphalt in a mass ratio of 92:3:5 for 2 h, then transferring them to a vertical reactor, controlling the initial inner cavity pressure of the reactor at -0.3 MPa, and reacting at 600 °C for 12 h to obtain secondary composite particles;

[0072] (3) The secondary composite particles were mixed with 500 nm isotropic particles (solid asphalt) in a mass ratio of 90:10, and then transferred to an orbital kiln for carbonization at 1250°C for 15 h to form an outer shell layer coated with hard carbon graphite particles and silicon oxide. The thickness of the outer shell layer was 505 nm. After screening and demagnetization, a high-capacity fast-charging negative electrode material was obtained.

[0073] Example 4

[0074] (1) 12 μm petroleum coke, starch and glucose were mixed in a conical mixer at a mass ratio of 90:10 for 3 h, then transferred to a push plate furnace for carbonization at 1300°C for 15 h, and then the carbonized powder was transferred to an Aixun graphitization furnace for high-temperature graphitization at 3000°C for 48 h, and hard carbon graphite particles were obtained after crushing, screening and demagnetization;

[0075] (2) mixing hard carbon graphite particles with 5 μm silicon oxide and binder asphalt in a mass ratio of 82:3:15 for 2 h, then transferring them to a vertical reactor, controlling the initial inner cavity pressure of the reactor at -0.6 MPa, and reacting at 600 °C for 12 h to obtain secondary composite particles;

[0076] (3) The secondary composite particles were mixed with 400 nm isotropic particles (solid asphalt) in a mass ratio of 92:8, and then transferred to an orbital kiln for carbonization at 1250 °C for 15 h to form an outer shell layer coated with hard carbon graphite particles and silicon oxide. The thickness of the outer shell layer was 405 nm. After screening and demagnetization, a high-capacity fast-charging negative electrode material was obtained.

[0077] Comparative Example 1

[0078] The 15μm petroleum coke is transferred to an 800℃ rotary kiln for pre-carbonization, naturally cooled to room temperature, and then graphitized at 2800℃. After the mixed material is screened and demagnetized, a single-particle graphite negative electrode material is obtained, which is then mixed with a 5μm silicon-based material in a mass ratio of 95:5 to make a silicon-carbon composite material.

[0079] Comparative Example 2

[0080] 7μm needle coke and asphalt in a mass ratio of 85:15 were mixed in a VC mixer for 2 hours, then transferred to a 600℃ vertical reactor for granulation, and then the material was graphitized at 3000℃. The material was crushed and demagnetized and then mixed with asphalt in a mass ratio of 95:5, and carbonized in a 1250℃ push plate furnace to obtain secondary particle fast-charging graphite negative electrode material, which was then mixed with 5μm silicon-based material in a mass ratio of 98:2 to make a silicon-carbon composite material.

[0081] Comparative Example 3

[0082] 10μm needle coke and asphalt are mixed in a certain mass ratio of 9:1, reacted and granulated in a 600℃ drum furnace, and then the material is graphitized at 3000℃, and then sieved and demagnetized to obtain secondary particle negative electrode material, and then the secondary particle negative electrode material, 5μm silicon-based material and asphalt are mixed in a VC mixer at a mass ratio of 88:3:10 for 3h, and then transferred to a 600℃ horizontal reactor for granulation, and carbonized in a 1300℃ orbital kiln to obtain carbon-silicon secondary particle carbon-silicon composite material.

[0083] In Examples 1 to 4 and Comparative Examples 1 to 3, the prepared negative electrode material was used as the active material to prepare 2032-type button cells to evaluate the electrochemical performance of the prepared graphite negative electrode material. Among them, the metal lithium sheet was used as the counter electrode, the EC / DMC (volume ratio of 1:1) solution of 1 mol / L LiPF6 was used as the electrolyte, and the Celgard 2400 microporous base membrane was used as the diaphragm.

[0084] The performance test results of the batteries of Examples 1 to 4 and Comparative Examples 1 to 3 are shown in Table 1.

[0085] Table 1

[0086]

[0087] As can be seen from Table 1, the amount of silicon material added in Examples 1-4 is increased, and the capacity of the raw materials will tend to gradually decrease, but the initial efficiency will increase, and the cycle will also improve. In the comparative example, the addition of silicon negative electrode material will inevitably lead to a decrease in the overall material cycle performance. The comprehensive performance of the negative electrode material of the embodiment of the present application is significantly better than the comprehensive performance of the comparative example. This is because the composite method of the negative electrode material used in the present application can ensure the basic performance and solve the problem of poor cycle performance of the silicon negative electrode material to a certain extent, effectively reducing the expansion problem of silicon, improving the cycle stability of the material, and ensuring better battery performance.

[0088] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0089] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A negative electrode material, It is characterized in that include: A kernel, the kernel comprising: Hard carbon graphite particles, the hard carbon graphite particles comprising a graphite material and a porous hard carbon layer, the porous hard carbon layer coating the graphite material; silicon-based particles, the silicon-based particles being adjacent to the hard carbon graphite particles; The outer shell layer covers the inner core, and the outer shell layer includes a soft carbon layer and isotropic particles, wherein the isotropic particles are embedded in the soft carbon layer.

2. The negative electrode material according to claim 1, It is characterized in that The mass ratio of the hard carbon graphite particles to the silicon-based particles is (100-75):(10-1); Optionally, the mass ratio of the silicon-based particles to the soft carbon layer is (10-1):(15-1); Optionally, the mass ratio of the core to the isotropic particles is (100-80):(20-1); Optionally, the mass ratio of the graphite material to the porous hard carbon layer is (80-90):(20-10).

3. The negative electrode material according to claim 1 or 2, It is characterized in that The particle size of the silicon-based particles is 1 μm-10 μm; Optionally, the particle size of the isotropic particles is 100 nm to 500 nm; Optionally, the isotropic particles include at least one of mesocarbon microspheres and solid pitch; Optionally, the outer shell layer has a thickness of 100 nm to 600 nm.

4. A method for preparing the negative electrode material according to any one of claims 1 to 3, It is characterized in that include: (1) mixing a graphite material precursor and a hard carbon material precursor, performing a first carbonization treatment and then a graphitization treatment to obtain hard carbon graphite particles; (2) mixing the hard carbon graphite particles, the silicon-based material and the binder and performing negative pressure low-temperature melt granulation to obtain secondary composite particles; (3) The secondary composite particles and the isotropic fine particles are mixed and subjected to a second carbonization treatment to obtain a negative electrode material.

5. The method according to claim 4, It is characterized in that The graphite material precursor D V50 5μm~20μm; Optionally, the graphite material precursor includes at least one of petroleum coke, oil-based needle coke, coal-based needle coke, natural graphite and flake graphite; Optionally, the hard carbon material precursor includes at least one of phenolic resin, furfuryl alcohol resin, epoxy resin, polyurethane, starch and sugar organic matter.

6. The method according to claim 4, It is characterized in that In step (1), the temperature of the first carbonization treatment is 1000° C. to 1300° C., and the time of the first carbonization treatment is 10 h to 20 h; Optionally, the temperature of the graphitization treatment is 2800° C. to 3000° C., and the time of the graphitization treatment is 24 h to 48 h.

7. The method according to claim 4, It is characterized in that In step (2), the pressure of the negative pressure low-temperature melt granulation is 0 to -0.8 MPa, the temperature is 300°C to 700°C, and the granulation time is 6h to 12h; Optionally, the binder includes at least one of petroleum asphalt and coal asphalt.

8. The method according to claim 4, It is characterized in that In step (3), the temperature of the second carbonization treatment is 1200° C. to 1400° C., and the time of the second carbonization treatment is 10 h to 20 h.

9. A negative electrode sheet, It is characterized in that The negative electrode material comprises the negative electrode material described in any one of claims 1 to 3 or the negative electrode material prepared by the method described in any one of claims 4 to 8.

10. A battery, It is characterized in that Including the negative electrode sheet as described in claim 9.