Secondary battery electrolyte and application
By adding furan, carboxylic acid and thioether group additives to the sodium ion battery electrolyte, the problem of sodium precipitation in the hard carbon negative electrode is solved, the cycle stability and safety performance of the battery are improved, and a more efficient sodium ion Transmission and battery safety.
Patent Information
- Application Number
- CN202411047260.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-01
AI Technical Summary
The hard carbon anode material in sodium-ion batteries has a sodium precipitation problem, which leads to unstable battery performance and safety hazards. It is difficult to effectively solve it with existing technology.
An additive containing furans, carboxylic acids and thioether groups is used to reduce the viscosity of the electrolyte, improve the filling efficiency and conductivity of sodium ions, inhibit the precipitation of metallic sodium, and enhance the interfacial contact capability and cycle stability of the electrolyte. .
It significantly improves the cycle stability and charge and discharge efficiency of sodium-ion batteries, reduces the risk of sodium precipitation, and improves the safety performance of the battery.
Smart Images

Figure BDA0004975325930000021 
Figure BDA0004975325930000022 
Figure BDA0004975325930000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a secondary battery electrolyte and application thereof. Background Art
[0002] The complementarity between sodium-ion batteries and lithium-ion batteries shows broad application prospects in the field of grid energy storage. For sodium-ion batteries, the development of low-cost, high-performance electrode materials is the key to realizing the commercial application of sodium-ion batteries. Among various negative electrode materials, carbon-based materials are highly favored due to their abundant raw materials, simple synthesis, and low cost. But in fact, hard carbon materials are the most mature commercially applied negative electrode materials among all carbon-based materials, but their current research status is still far from large-scale industrialization.
[0003] At present, the development of hard carbon materials is mainly restricted by the unclear sodium storage mechanism and its extremely low electrode potential, low coulombic efficiency, poor cycle and rate stability and other performance reasons. When the above problems were discovered, scientific researchers had already begun to design and modify them, and the performance was significantly improved, but the battery cost rose sharply, which did not conform to the main route of low-cost energy substitution for sodium-ion batteries. Therefore, it was only reflected in journal literature and not applied to actual battery products; and in the actual test process, it was found that due to the extremely low electrode potential of hard carbon, sodium precipitation on the negative electrode surface was very serious during the battery charging and discharging process, which was directly related to the low coulombic efficiency, unstable cycle and poor rate performance mentioned earlier. Although it has been verified that the precipitated sodium metal and lithium metal are in different forms and no obvious sodium dendrites will be produced in the short term, it is also a big challenge to the long-term battery performance and safety performance. Therefore, inhibiting sodium precipitation is the main idea to solve the use of hard carbon negative electrodes in lithium-ion batteries at this stage.
[0004] At present, sodium precipitation is mainly suppressed through the following two ways: ① Negative electrode modification, by using two-dimensional materials / soft and hard carbon coating to improve the electronic conductivity of hard carbon, or reducing the particle size of carbon negative electrode materials, etc.; however, the preparation process of two-dimensional materials / soft and hard carbon coating is complex, the consistency is poor, and the electronic conductivity of the hard carbon negative electrode itself is good, and the electronic conductivity is often not the decisive factor for sodium precipitation. ② Optimize the composition of the electrolyte, by using solvents with good low-temperature performance in the electrolyte, the conductivity of the electrolyte is improved, while the SEI membrane impedance is reduced, and the sodium ion transmission kinetics are accelerated. The existing electrolyte solutions are mainly focused on optimizing the solvent system, reducing the viscosity of the formula system without affecting the ionic conductivity, improving the ion mobility, and reducing the sodium precipitation problem caused by large polarization under low temperature conditions. This type of solution is a direct application of the lithium-ion battery system solution, the main problems of which are: ① The negative electrode of the sodium-ion battery system mainly uses hard carbon rather than graphite. The sodium storage method of hard carbon and graphite is different. Improving the ionic conductivity of the system cannot effectively solve the sodium precipitation of the hard carbon negative electrode; ② There are few solutions for using additives in the electrolyte system to improve material performance. Therefore, providing an electrolyte that can effectively solve the sodium precipitation problem of the carbon negative electrode in the sodium ion battery has become a problem to be solved. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide a secondary battery electrolyte and application. The electrolyte provided by the present invention can inhibit sodium precipitation of the hard carbon negative electrode and improve the safety performance of the battery.
[0006] The present invention provides a secondary battery electrolyte, comprising an additive, wherein the additive has a structure shown in Formula I:
[0007]
[0008] In formula I, R1 is hydrogen; R2 and R3 are independently selected from H or methyl, and R2 and R3 are not hydrogen at the same time.
[0009] Preferably, the additive is selected from one or more of the following compounds:
[0010]
[0011] Preferably, the preparation method of the additive comprises the following steps:
[0012] A) reacting reactant RX with reactant RY in the presence of a catalyst to obtain a reaction product PX;
[0013] B) reacting the reaction product PX with hydrogen peroxide in the presence of an alkaline agent to produce an additive having a structure shown in Formula I;
[0014] Among them, the structure of the reactant RX is R1 is hydrogen; R2 and R3 are independently selected from H, methyl, and R2 and R3 are not hydrogen at the same time;
[0015] The structure of the reactant RY is
[0016] Reaction product PX R1 is hydrogen; R2 and R3 are independently selected from H and methyl, and R2 and R3 are not hydrogen at the same time.
[0017] Preferably, in step A), the equivalent ratio of the reactant RX to the reactant RY is 1:(1-10);
[0018] The equivalent ratio of the reactant RX to the catalyst is 1:(0.01-0.02);
[0019] The catalyst is selected from rhenium heptoxide;
[0020] The reaction temperature is 0 to 30° C. and the reaction time is 1 to 3 hours.
[0021] Preferably, in step B), the concentration of the hydrogen peroxide is 30%;
[0022] The reaction equivalent ratio of the reaction product PX to hydrogen peroxide is 1:(2-5);
[0023] The alkaline agent is selected from sodium hydroxide or potassium carbonate;
[0024] The reaction equivalent ratio of the reaction product PX to the alkaline reagent is 1:(0.2-1);
[0025] The reaction temperature is divided into three stages. The reaction product PX is mixed with an alkaline reagent at room temperature, and then hydrogen peroxide is added at a temperature of -5°C to 5°C. After the addition of hydrogen peroxide, the reaction temperature is 20 to 50°C, and the reaction time is 1h to 6h.
[0026] Preferably, the additive is added to the electrolyte in an amount of 1 wt% to 5 wt%.
[0027] Preferably, the electrolyte further comprises an electrolyte salt and a non-aqueous organic solvent.
[0028] Preferably, the electrolyte salt is selected from at least one of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium perchlorate, sodium tetrafluoroborate, sodium difluorophosphate, and sodium difluorooxalatoborate;
[0029] The non-aqueous organic solvent is selected from one or more of organic ester solvents, C1-10 alkyl ether solvents, cyclic ether solvents, sulfone solvents, and dinitrile solvents.
[0030] Preferably, the electrolyte further comprises other types of additives, and the other types of additives are selected from vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, vinyl sulfate, vinyl disulfate, propylene sulfate, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, 2,4-butane sultone, phenyl methanesulfonate, methylene disulfonate, N-phenylbis(trifluoromethanesulfonyl)imide, triallyl phosphate, tris(trimethylsilane) ) phosphate, trimethyl phosphite, triphenyl phosphite, tetramethylmethylene diphosphate, propargyl phosphate, (2-allylphenoxy)trimethylsilane, tris(trimethylsilyl)borate, 1,3,5-triallyl isocyanurate, isocyanoethyl methacrylate, hexamethylene diisocyanate, p-phenylene diisocyanate, 2,4-toluene diisocyanate, 1,3,6-hexanetrinitrile, 1,2-bis(cyanoethoxy)ethane or one or more of ethoxypentafluorocyclotriphosphazene.
[0031] The present invention also provides a secondary battery comprising the above electrolyte.
[0032] Compared with the prior art, the present invention provides a secondary battery electrolyte, including an additive, wherein the additive has a structure shown in Formula I, wherein R1 is hydrogen; R2 and R3 are independently selected from H or methyl, and R2 and R3 are not hydrogen at the same time. The present invention adds an additive to the electrolyte of a secondary battery, wherein the additive is an additive for inhibiting sodium precipitation of a hard carbon negative electrode and improving safety performance. Due to the presence of furan and carboxylic acid groups, the electrolyte can reduce viscosity and improve wettability at the initial stage of addition, so that the electrolyte can still have good interface contact ability and ion transmission performance at low temperature; the carboxylic acid group contained therein can increase the binding energy with sodium ions in the electrolyte at high voltage, alleviate the filling rate of sodium ions in hard carbon defect pores at low potential, reduce non-underpotential deposition behavior, and inhibit the precipitation of metallic sodium; the cyclic ether group contained therein can improve the orientation effect of sodium ions, so that sodium ions can be uniformly filled into the defect pores of the hard carbon negative electrode, so as not to cause oversaturation and precipitation of sodium in some areas at a high rate, thereby improving the high rate charge and discharge performance; the thioether group therein can enhance the complexing ability of sodium ions, improve the ionic conductivity and temperature width range of the electrolyte, and optimize the performance of the battery interface film during the battery cycle process, reduce the growth of the battery DCR, and have a high improvement on the overall battery performance and stability. Since the present invention solves the problem of sodium precipitation at the negative electrode, the cycle stability and charge and discharge efficiency are greatly improved. Sodium precipitation is also the main cause of battery fire safety problems. Therefore, the additive provided by the present invention improves the safety performance of the battery to a certain extent. DETAILED DESCRIPTION
[0033] The present invention provides a secondary battery electrolyte, comprising an additive, wherein the additive has a structure shown in Formula I:
[0034]
[0035] In formula I, R1 is hydrogen; R2 and R3 are independently selected from H or methyl, and R2 and R3 are not hydrogen at the same time.
[0036] In some embodiments of the present invention, the additive is selected from one or more of the following compounds:
[0037]
[0038] In the present invention, the preparation method of the additive comprises the following steps:
[0039] A) reacting reactant RX with reactant RY in the presence of a catalyst to obtain a reaction product PX;
[0040] B) reacting the reaction product PX with hydrogen peroxide in the presence of an alkaline agent to produce an additive having a structure shown in Formula I;
[0041] Among them, the structure of the reactant RX is R1 is hydrogen; R2 and R3 are independently selected from H, methyl, and R2 and R3 are not hydrogen at the same time;
[0042] The structure of the reactant RY is
[0043] Reaction product PX R1 is hydrogen; R2 and R3 are independently selected from H and methyl, and R2 and R3 are not hydrogen at the same time.
[0044] The present invention first reacts reactant RX with reactant RY in the presence of a catalyst to obtain a reaction product PX, and the reaction formula is as follows:
[0045]
[0046] Specifically, the reactant RX is dissolved in the solvent I at room temperature, and then the reactant RY and the catalytic agent are added and mixed to react to obtain the reaction product PX.
[0047] In the present invention, the solvent I used in step A) and the solvent II used in step B) are all subjected to a redistillation step or a molecular sieve to remove water before use in the reaction to obtain a dry reaction solvent, the indicator of the dry reaction solvent is benzophenone and sodium wire, the molecular sieve is selected from one of 4A, 5A, and 13X molecular sieves, and the water content in the solvent is required to be less than 1ppm; preferably, the molecular sieve is 5A or 13X.
[0048] The solvent I is one of dichloromethane, chloroform, ethyl acetate, acetone, and 2-butanone; preferably, the solvent I is dichloromethane.
[0049] The equivalent ratio of the reactant RX to the reactant RY is 1:(1-10), and can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, or any value between 1:(1-10), preferably any value between 1:(2-4);
[0050] The equivalent ratio of the reactant RX to the catalyst is 1:(0.01-0.02), which can be 1:0.01, 1:0.012, 1:0.014, 1:0.015, 1:0.016, 1:0.018, 1:0.02, or any value between 1:(0.01-0.02);
[0051] The catalyst is selected from rhenium heptoxide;
[0052] The reaction temperature is 0 to 30° C., and can be 0, 5, 10, 15, 20, 25, 30, or any value between 0 and 30° C., preferably room temperature. In the present invention, the room temperature is defined as 20 to 30° C. The reaction time is 1 to 3 hours, and can be 1, 1.5, 2, 2.5, 3, or any value between 1 and 3 hours.
[0053] Next, after obtaining the reaction product PX, the reaction product PX is reacted with hydrogen peroxide in the presence of an alkaline reagent to produce an additive having a structure shown in Formula I.
[0054] Among them, the reaction formula is as follows:
[0055]
[0056] Specifically, under normal temperature conditions, reactants PX and alkaline reagents are added to solvent II and mixed, and then hydrogen peroxide is added after cooling. After the addition is completed, the temperature of the reaction system is increased to react to obtain an additive having a structure shown in formula I.
[0057] Wherein, the concentration of the hydrogen peroxide is 30%;
[0058] The reaction equivalent ratio of the reaction product PX to hydrogen peroxide is 1:(2-5), which can be 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, or any value between 1:(2-5), preferably any value between 1:(3-4);
[0059] The alkaline agent is selected from sodium hydroxide or potassium carbonate;
[0060] The reaction equivalent ratio of the reaction product PX to the alkaline reagent is 1:(0.2-1), which can be 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1.0, or any value between 1:(0.2-1), preferably any value between 1:(0.5-1);
[0061] The solvent II in step 3 is one of N,N-dimethylformamide, acetone, 2-butanone, toluene and 1,4-dioxane; preferably, the solvent II is N,N-dimethylformamide.
[0062] The temperature of the reaction is divided into three stages. The reaction product PX is mixed with an alkaline reagent at room temperature, and then the temperature is reduced and hydrogen peroxide is added. The cooling temperature is -5°C to 5°C, which can be -5°C, -4°C, -3°C, -2°C, -1°C, 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, or any value between -5°C and 5°C, preferably 0°C. After the addition of hydrogen peroxide, the temperature for the reaction is increased to 20 to 50°C, which can be 20, 25, 30, 35, 40, 45, 50, or any value between 20 and 50°C, preferably any value between 30 and 40°C. The reaction time is 1h to 6h, which can be 1, 2, 3, 4, 5, 6, or any value between 1h and 6h, preferably any value between 2 to 4h.
[0063] In the present invention, the additive is added to the electrolyte in an amount of 1wt% to 5wt%, which may be 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, or any value between 1wt% and 5wt%.
[0064] In the electrolyte provided by the present invention, the additive used as a diluent reduces the viscosity of the electrolyte under low temperature conditions without affecting the electrolyte's own melting and boiling points, ion conductivity and other properties, thereby ensuring the ion transmission dynamics under low temperature conditions.
[0065] Among them, the carboxyl functional group in the additive can increase the binding energy with sodium ions at high voltage, alleviate the filling rate of sodium ions in hard carbon defects at low potential, reduce non-under-electrodeposition behavior, and inhibit the precipitation of metallic sodium on the negative electrode surface. At the same time, the cyclic ether group will enhance the orientation of sodium ions, so that sodium ions can be evenly filled into the defective pores of the hard carbon negative electrode, so as not to cause oversaturation and precipitation of sodium in some areas at a large rate. As an electrolyte additive, it contains thioether groups, which can enhance the complexing ability of sodium ions, improve the ionic conductivity and temperature range of the electrolyte, and optimize the performance of the battery interface film during the battery cycle process, reduce the growth of the battery DCR, and have a high improvement in the overall battery performance and stability.
[0066] In the present invention, the electrolyte solution further includes an electrolyte salt and a non-aqueous organic solvent.
[0067] Wherein, the electrolyte salt is selected from sodium hexafluorophosphate (NaPF 6 ), sodium bis(fluorosulfonyl)imide (NaFSI), sodium perchlorate (NaClO 4 ), sodium tetrafluoroborate (NaBF 4 ), sodium difluorophosphate (NaPO 2 F 2 ), sodium difluorooxalate borate (NaODFB);
[0068] The non-aqueous organic solvent is selected from one or more of organic ester solvents, C1-10 alkyl ether solvents, cyclic ether solvents, sulfone solvents, and dinitrile solvents.
[0069] Further, the organic ester is at least one of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, 1,4-butyrolactone, methyl formate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate and ethyl butyrate; the C 1-10 The alkyl ether is at least one of dimethyl ether, diethyl ether and methyl ethyl ether; the dinitriles are at least one of adiponitrile, succinonitrile and glutaronitrile; and the sulfones are at least one of dimethyl sulfoxide and cyclopentane sulfone.
[0070] Further, the electrolyte also includes other types of additives, and the other types of additives are selected from vinylene carbonate, ethylene carbonate, fluoroethylene carbonate, vinyl sulfate, vinyl disulfate, propylene sulfate, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, 2,4-butane sultone, phenyl methanesulfonate, methylene disulfonate, N-phenylbis(trifluoromethanesulfonyl)imide, triallyl phosphate, tris(trimethylsilyl)sulfonate, The invention can be one or more of (1,3,6-hexanetrinitrile, 1,2-bis(cyanoethoxy)ethane or ethoxypentafluorocyclotriphosphazene.
[0071] In some specific embodiments of the present invention, the electrolyte comprises:
[0072] 8 wt% to 25 wt% of an electrolyte salt;
[0073] 60 wt% to 90 wt% of a non-aqueous organic solvent;
[0074] 1wt% to 5wt% of additives.
[0075] Among them, the addition amount of electrolyte salt in the electrolyte can be 8wt%, 10wt%, 12wt%, 14wt%, 15wt%, 16wt%, 18wt%, 20wt%, 22wt%, 24wt%, 25wt%, or any value between 8wt% and 25wt%, preferably any value between 13wt% and 15wt%.
[0076] The addition amount of the non-aqueous organic solvent can be 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, 85wt%, 90wt%, or any value between 60wt% and 90wt%, preferably any value between 74wt% and 90wt%.
[0077] The present invention also provides a secondary battery, comprising the above electrolyte. Further, the secondary battery also comprises a positive electrode, a negative electrode and a separator.
[0078] The positive electrode material in the positive electrode is selected from sodium manganate, sodium copper iron manganate, sodium nickel iron manganate, sodium copper nickel iron manganate, sodium iron phosphate, sodium vanadium phosphate or composite sodium iron phosphate, preferably sodium nickel iron manganate.
[0079] Furthermore, the negative electrode active material in the negative electrode is selected from biomass-based hard carbon, asphalt-based hard carbon or resin-based hard carbon. Preferably, the negative electrode active material is biomass-based hard carbon.
[0080] Furthermore, the diaphragm is selected from polypropylene (PP), polyethylene (PE) and glass fiber diaphragm.
[0081] The present invention provides a secondary battery electrolyte, comprising an additive, wherein the additive has a structure shown in Formula I, wherein R1 is hydrogen; R2 and R3 are independently selected from H or methyl, and R2 and R3 are not hydrogen at the same time. The present invention adds an additive to the electrolyte of a secondary battery, wherein the additive is an additive for inhibiting sodium precipitation of a hard carbon negative electrode and improving safety performance. Due to the presence of furan and carboxylic acid groups, the electrolyte can reduce viscosity and improve wettability at the initial stage of addition, so that the electrolyte can still have good interface contact ability and ion transmission performance at low temperature; the carboxylic acid group contained therein can increase the binding energy with sodium ions in the electrolyte at high voltage, alleviate the filling rate of sodium ions in hard carbon defect pores at low potential, reduce non-underpotential deposition behavior, and inhibit the precipitation of metallic sodium; the cyclic ether group contained therein can improve the orientation effect of sodium ions, so that sodium ions can be uniformly filled into the defect pores of the hard carbon negative electrode, so as not to cause oversaturation and precipitation of sodium in some areas at a high rate, thereby improving the high rate charge and discharge performance; the thioether group therein can enhance the complexing ability of sodium ions, improve the ionic conductivity and temperature width range of the electrolyte, and optimize the performance of the battery interface film during the battery cycle process, reduce the growth of the battery DCR, and have a high improvement on the overall battery performance and stability. Since the present invention solves the problem of sodium precipitation at the negative electrode, the cycle stability and charge and discharge efficiency are greatly improved. Sodium precipitation is also the main cause of battery fire safety problems. Therefore, the additive provided by the present invention improves the safety performance of the battery to a certain extent.
[0082] In order to further understand the present invention, the secondary battery electrolyte and applications provided by the present invention are described below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0083] Preparation Example 1 (Reactant RX 1 The methyl group is in the proximal position)
[0084]
[0085] Add 10 g (1 eq, 0.0979 mol) of 3-methyl-2-tetrahydrofuran alcohol with a purity of 99% to a reaction bottle with a thermometer, then add 50 mL of dichloromethane after dehydration with a 5A molecular sieve, stir thoroughly to dissolve, weigh 14.32 g (2 eq, 0.196 mol) of nucleophilic reagent 2-mercaptoacetonitrile and add it to the reaction system, control the temperature of the reaction system to room temperature, add 0.5 g (0.01 eq, 0.001 mol) of rhenium oxide catalyst, control the reaction temperature to 20 ° C, stop the reaction after 1 hour of reaction, and distill the reaction system under reduced pressure. The residual brown viscous substance is added to silica gel particles and separated on a chromatographic column. The eluent ratio is ethyl acetate: ether = 1:1.2. After purification, 11.1 g of substance PX is obtained. 1 , the yield was 72% and the purity was 99%.1 H NMR (300 MHz, CDCl 3 )δ4.79(s,1H),3.80(d,2H),3.56(s,2H),2.2(dd,2H),1.92(m,2H),0.88(d,3H).TOF-MS(ESI)m / z calcd for C 7 H 11 NOS:157.23;[M+H] + found:157.19.
[0086] Add the substance PX prepared in the previous step into the reaction bottle with a thermometer 1 10g (1eq, 0.0636mol), then add 50mL of N,N-dimethylformamide after removing water with 5A molecular sieve, stir and dissolve thoroughly, weigh 1.27g (0.5eq, 0.0318mol) of sodium hydroxide and add it to the reaction system to stir and create an alkaline environment, then lower the temperature of the reaction system to 0°C, add 21.63g (3eq, 0.191mol) of 30wt% hydrogen peroxide to the system and control the temperature of the system at 30°C, stir and react for 2h, and quench the reaction with sodium bisulfite after the reaction is completed. The reaction system is distilled under reduced pressure, the residue is extracted with tri-filter methane, the extract is concentrated again and separated by column chromatography, the eluent ratio is ethyl acetate: methanol = 1:3, and 7.5g of substance M is obtained after purification. 1 , the yield was 67% and the purity was 99%. 1 H NMR (400MHz, d6- DMSO)δ12.04(s,1H),4.79(s,1H),3.81(d,2H),3.38(s,2H),2.25(dd,2H),1.95(m,1H),0.88(d,3H).TOF-MS(ESI)m / z calcd for C 7 H 12 O 3 S:176.23;[M+H] + found:176.34.
[0087] Preparation Example 2 (Reactant RX 2 The methyl group is in the meta position)
[0088]
[0089] Add 10 g (1 eq, 0.0979 mol) of 4-methyl-2-tetrahydrofuran alcohol with a purity of 99% to a reaction bottle with a thermometer, then add 50 mL of dichloromethane after dehydration with a 5A molecular sieve, stir thoroughly to dissolve, weigh 21.48 g (3 eq, 0.294 mol) of nucleophilic reagent 2-mercaptoacetonitrile and add it to the reaction system, control the temperature of the reaction system to room temperature, add 0.5 g (0.01 eq, 0.001 mol) of rhenium oxide catalyst, control the reaction temperature to 25 ° C, stop the reaction after 1 hour of reaction, and distill the reaction system under reduced pressure. The residual brown viscous substance is added to silica gel particles and separated on a chromatographic column. The eluent ratio is ethyl acetate: ether = 1:1.2. After purification, 11.9 g of substance PX is obtained. 1 , the yield was 77% and the purity was 99%. 1 H NMR (300 MHz, CDCl 3 )δ4.79(s,1H),3.81(d,2H),3.56(s,2H),2.25(dd,2H),1.95(m,1H),0.81(d,3H).TOF-MS(ESI)m / z calcd for C 7 H 11 NOS:157.23;[M+H] + found:157.07.
[0090] Add the substance PX prepared in the previous step into the reaction bottle with a thermometer 2 10g (1eq, 0.0636mol), then add 50mL of N,N-dimethylformamide after removing water with 5A molecular sieve, stir and dissolve thoroughly, weigh 6.15g (0.7eq, 0.0445mol) of potassium carbonate and add it to the reaction system to stir and create an alkaline environment, then lower the temperature of the reaction system to 0°C, add 28.87g (4eq, 0.255mol) of 30wt% hydrogen peroxide to the system and control the system temperature at 35°C, stir and react for 3h, after the reaction is completed, quench the reaction with sodium bisulfite, distill the reaction system under reduced pressure, extract the residue with three-filter methane, concentrate the extract again and separate it by column chromatography, the eluent ratio is ethyl acetate: methanol = 1:3, and 8.18g of substance M is obtained after purification. 1 , the yield was 73% and the purity was 99%. 1 H NMR (400MHz, d6- DMSO)δ12.04(s,1H),4.79(s,1H),3.81(d,2H),3.38(s,2H),2.25(dd,2H),1.95(m,1H),0.81(d,3H).TOF-MS(ESI)m / z calcd for C 7H 12 O 3 S:176.23;[M+H] + found:176.22.
[0091] Preparation Example 3 (Reactant RX 3 The dimethyl groups are located at the ortho and meta positions respectively)
[0092]
[0093] Add 10 g (1 eq, 0.0861 mol) of 3,4-dimethyl-2-tetrahydrofuran alcohol with a purity of 99% to a reaction bottle with a thermometer, then add 50 mL of dichloromethane after removing water from a 5A molecular sieve, stir thoroughly to dissolve, weigh 25.17 g (4 eq, 0.344 mol) of nucleophilic reagent 2-mercaptoacetonitrile and add it to the reaction system, control the temperature of the reaction system to room temperature, add 0.42 g (0.01 eq, 0.0086 mol) of rhenium oxide catalyst, control the reaction temperature to 30 ° C, stop the reaction after 1 hour of reaction, and distill the reaction system under reduced pressure. The residual brown viscous substance is added to silica gel particles and separated on a chromatographic column. The eluent ratio is ethyl acetate: ether = 1:1.2. After purification, 9.7 g of substance PX is obtained. 1 , the yield was 66% and the purity was 99%. 1 H NMR (300 MHz, CDCl 3 )δ4.69(s,1H),3.86(d,2H),3.56(s,2H),2.12(m,1H),1.86(m,1H),0.88(d,6H).TOF-MS(ESI)m / z calcd for C 8 H 13 NOS:171.26;[M+H] + found:171.89.
[0094] Add the substance PX prepared in the previous step into the reaction bottle with a thermometer 310g (1eq, 0.0584mol), then add 50mL of N,N-dimethylformamide after removing water from 5A molecular sieve, stir and dissolve thoroughly, weigh 8.07g (1eq, 0.0584mol) of potassium carbonate and add it to the reaction system to stir and create an alkaline environment, then lower the temperature of the reaction system to 0°C, add 19.86g (3eq, 0.175mol) of 30wt% hydrogen peroxide to the system and control the system temperature at 40°C, stir and react for 4h, and quench the reaction with sodium bisulfite after the reaction is completed. The reaction system is distilled under reduced pressure, the residue is extracted with tri-filter methane, the extract is concentrated again and separated by column chromatography, the eluent ratio is ethyl acetate: methanol = 1:3, and 8.8g of substance M is obtained after purification. 1 , the yield was 79% and the purity was 99%. 1 H NMR (400MHz, d6- DMSO)δ12.33(s,1H),4.69(s,1H),3.86(d,2H),3.40(s,2H),2.12(m,1H),1.86(m,1H),0.88(d,6H).TOF-MS(ESI)m / z calcd for C 8 H 14 O 3 S:190.26; [M+H] + found:190.33.
[0095] Preparation Example 4
[0096] Preparation of standard electrolyte for sodium ion batteries:
[0097] In full N 2 In a glove box, propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were uniformly mixed at a mass ratio of PC:EMC:DEC=3:5:2, and sodium hexafluorophosphate (NaPF 6 ) to a molar concentration of 1 mol / L to obtain a standard electrolyte.
[0098] Comparative Example 1
[0099] The standard electrolyte was used as the electrolyte of Comparative Example 1.
[0100] Example 1
[0101] In the standard electrolyte, add 1wt% of M prepared in Example 1 1 , and obtain the electrolyte of the embodiment.
[0102] Example 2
[0103] In the standard electrolyte, add 1wt% of M prepared in Example 22 , and obtain the electrolyte of the embodiment.
[0104] Example 3
[0105] In the standard electrolyte, add 1wt% of M prepared in Example 3 3 , and obtain the electrolyte of the embodiment.
[0106] Example 4
[0107] In the standard electrolyte, add 3wt% of M prepared in Example 1 1 , and obtain the electrolyte of the embodiment.
[0108] Example 5
[0109] In the standard electrolyte, add 3wt% of M prepared in Example 2 2 , and obtain the electrolyte of the embodiment.
[0110] Example 6
[0111] In the standard electrolyte, 3 wt% of M prepared in Example 3 was added. 3 , and obtain the electrolyte of the embodiment.
[0112] Example 7
[0113] In the standard electrolyte, add 5wt% of M prepared in Example 1 1 , and obtain the electrolyte of the embodiment.
[0114] Example 8
[0115] In the standard electrolyte, add 5wt% of M prepared in Example 2 2 , and obtain the electrolyte of the embodiment.
[0116] Example 9
[0117] In the standard electrolyte, 5 wt% of M prepared in Example 3 was added. 3 , and obtain the electrolyte of the embodiment.
[0118] Comparative Example 2
[0119] 1 wt % of vinylene carbonate (VC), an existing unsaturated carbonate additive, was added to the standard electrolyte to obtain a comparative electrolyte.
[0120] Comparative Example 3
[0121] 1 wt % of fluoroethylene carbonate (FEC), an existing fluorocarbonate additive, was added to the standard electrolyte to obtain a comparative electrolyte.
[0122] Comparative Example 4
[0123] 1 wt % of the existing sulfone additive sulfolane was added to the standard electrolyte to obtain a comparative electrolyte.
[0124] Comparative Example 5
[0125] 1 wt % of the existing ether additive 18-crown ether-6 was added to the standard electrolyte to obtain a comparative electrolyte.
[0126] Comparative Example 6
[0127] 3 wt % of vinylene carbonate (VC), an existing unsaturated carbonate additive, was added to the standard electrolyte to obtain a comparative electrolyte.
[0128] Comparative Example 7
[0129] 3 wt % of fluoroethylene carbonate (FEC), an existing fluorocarbonate additive, was added to the standard electrolyte to obtain a comparative electrolyte.
[0130] Comparative Example 8
[0131] 3 wt % of the existing sulfone additive sulfolane was added to the standard electrolyte to obtain a comparative electrolyte.
[0132] Comparative Example 9
[0133] 3 wt % of the existing ether additive 18-crown ether-6 was added to the standard electrolyte to obtain a comparative electrolyte.
[0134] Comparative Example 10
[0135] 5 wt % of vinylene carbonate (VC), an existing unsaturated carbonate additive, was added to the standard electrolyte to obtain a comparative electrolyte.
[0136] Comparative Example 11
[0137] 5 wt % of fluoroethylene carbonate (FEC), an existing fluorocarbonate additive, was added to the standard electrolyte to obtain a comparative electrolyte.
[0138] Comparative Example 12
[0139] 5 wt % of the existing sulfone additive sulfolane was added to the standard electrolyte to obtain a comparative electrolyte.
[0140] Comparative Example 13
[0141] 5 wt % of the existing ether additive 18-crown ether-6 was added to the standard electrolyte to obtain a comparative electrolyte.
[0142] After preparing the above-mentioned comparative sodium electrolyte, the viscosity and shelf moisture content were tested, and finally the following table was summarized.
[0143] Table 1 Comparison of sodium electrolyte viscosity
[0144] Comparative Example Viscosity / cP Comparative Example Viscosity / cP Comparative Example 1 4.32 Comparative Example 2 4.34 Example 1 3.95 Comparative Example 3 4.64 Example 2 3.88 Comparative Example 4 4.27 Example 3 3.75 Comparative Example 5 3.94 Example 4 4.01 Comparative Example 6 4.56 Example 5 3.94 Comparative Example 7 4.78 Example 6 3.89 Comparative Example 8 4.67 Example 7 4.12 Comparative Example 9 4.32 Example 8 4.02 Comparative Example 10 4.72 Example 9 3.96 Comparative Example 11 4.89 Comparative Example 12 4.54 Comparative Example 13 4.81
[0145] Application Example 1
[0146] Preparation of sodium battery soft pack: weigh the active material Na in the dry room 0.9 Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 O 2 , conductive carbon black and binder PVDF (5wt% PVDF solution prepared with NMP as solvent), with a mass ratio of 95:2.5:2.5, dissolved with NMP as solvent, prepared into slurry, and then evenly coated on aluminum current collector, dried and passed through a roller press to prepare pole sheet core, cut and dried to obtain the positive pole sheet of soft-pack battery; at the same time, weigh the negative electrode active material hard carbon (biomass-based), conductive carbon black, sodium carboxymethyl cellulose (CMC), and binder SBR, with a mass ratio of 94:2:2:2, used deionized water as solvent, prepared into slurry, and then evenly coated on aluminum current collector, dried and passed through a roller press to prepare pole sheet core, cut and dried to obtain the negative pole sheet of soft-pack battery; finally, the battery is semi-encapsulated according to the ratio of positive pole sheet: negative pole sheet = 12:13, and dried.
[0147] The electrolyte used in the prepared soft-pack battery is a solution of sodium hexafluorophosphate (1 mol / L) in propylene carbonate (PC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DEC) (mass ratio of 3:5:2), and 1 wt% of the electrolyte additive M provided in Preparation Example 1 of the present invention is added. 1 The negative electrode of the battery uses a metal lithium sheet and the isolation membrane uses a PE film.
[0148] Application Example 2
[0149] The difference between Application Example 2 and Application Example 1 is that 1 wt% of the electrolyte additive M prepared in Preparation Example 2 of the present invention is added. 2 , the rest of the parameters and steps remain the same as in Application Example 1.
[0150] Application Example 3
[0151] The difference between Application Example 3 and Application Example 1 is that 1 wt% of the electrolyte additive M prepared in Preparation Example 3 of the present invention is added. 3 , the rest of the parameters and steps remain the same as in Application Example 1.
[0152] Application Example 4
[0153] The difference between Application Example 4 and Application Example 1 is that 3 wt % of the electrolyte additive M prepared in Preparation Example 1 of the present invention is added. 1 , the rest of the parameters and steps remain the same as in Application Example 1.
[0154] Application Example 5
[0155] The difference between Application Example 5 and Application Example 1 is that 3 wt % of the electrolyte additive M prepared in Preparation Example 2 of the present invention is added. 2 , the rest of the parameters and steps remain the same as in Application Example 1.
[0156] Application Example 6
[0157] The difference between Application Example 6 and Application Example 1 is that 3 wt % of the electrolyte additive M prepared in Preparation Example 3 of the present invention is added. 3 , the rest of the parameters and steps remain the same as in Application Example 1.
[0158] Application Example 7
[0159] The difference between Application Example 7 and Application Example 1 is that 5 wt% of the electrolyte additive M prepared in Preparation Example 1 of the present invention is added. 1 , the rest of the parameters and steps remain the same as in Application Example 1.
[0160] Application Example 8
[0161] The difference between Application Example 8 and Application Example 1 is that 5 wt% of the electrolyte additive M prepared in Preparation Example 2 of the present invention is added. 2 , the rest of the parameters and steps remain the same as in Application Example 1.
[0162] Application Example 9
[0163] The difference between Application Example 9 and Application Example 1 is that 5 wt% of the electrolyte additive M prepared in Preparation Example 3 of the present invention is added. 3 , the rest of the parameters and steps remain the same as in Application Example 1.
[0164] Comparative application example 1
[0165] The only difference between Comparative Application Example 1 and Application Example 1 is that 1 wt % of the existing unsaturated carbonate additive vinylene carbonate is added, and the other parameters and steps are consistent with those in Application Example 1.
[0166] Comparative Application Example 2
[0167] The only difference between Application Example 2 and Application Example 1 is that 1 wt % of the existing fluorocarbonate additive fluoroethylene carbonate is added, and the other parameters and steps are consistent with those in Application Example 1.
[0168] Comparative Application Example 3
[0169] The only difference between Application Example 3 and Application Example 1 is that 1 wt % of the existing sulfone additive sulfolane is added, and the other parameters and steps are consistent with those in Application Example 1.
[0170] Comparative Application Example 4
[0171] The only difference between Application Example 4 and Application Example 1 is that 1 wt % of the existing ether additive 18-crown ether-6 is added, and the other parameters and steps are consistent with those in Application Example 1.
[0172] Comparative Application Example 5
[0173] The only difference between Comparative Application Example 5 and Application Example 1 is that 3 wt % of the existing unsaturated carbonate additive vinylene carbonate is added, and the other parameters and steps are consistent with those in Application Example 1.
[0174] Comparative Application Example 6
[0175] The only difference between Application Example 6 and Application Example 1 is that 3 wt % of the existing fluorocarbonate additive fluoroethylene carbonate is added, and the other parameters and steps are consistent with those in Application Example 1.
[0176] Comparative Application Example 7
[0177] The only difference between comparative application example 7 and application example 1 is that 3 wt % of the existing sulfone additive sulfolane is added, and the other parameters and steps are consistent with those in application example 1.
[0178] Comparative Application Example 8
[0179] The only difference between Application Example 8 and Application Example 1 is that 3 wt % of the existing ether additive 18-crown ether-6 is added, and the other parameters and steps are consistent with those in Application Example 1.
[0180] Comparative Application Example 9
[0181] The only difference between Comparative Application Example 9 and Application Example 1 is that 5 wt % of the existing unsaturated carbonate additive vinylene carbonate is added, and the other parameters and steps are consistent with those in Application Example 1.
[0182] Comparative Application Example 10
[0183] The only difference between comparative application example 10 and application example 1 is that 5 wt % of the existing fluorocarbonate additive fluoroethylene carbonate is added, and the other parameters and steps are consistent with those in application example 1.
[0184] Comparative Application Example 11
[0185] The only difference between comparative application example 11 and application example 1 is that 5 wt % of the existing sulfone additive sulfolane is added, and the other parameters and steps are consistent with those in application example 1.
[0186] Comparative Application Example 12
[0187] The only difference between Application Example 12 and Application Example 1 is that 5 wt % of the existing ether additive 18-crown ether-6 is added, and the other parameters and steps are consistent with those in Application Example 1.
[0188] Performance Testing
[0189] The button batteries obtained from Examples 1 to 3 and Comparative Application Examples 1 to 4 were tested for normal temperature (25°C) cycle (1000 cycles), low temperature (0°C) cycle, low temperature (-40°C) discharge performance, and negative electrode surface state performance after high rate (10C) charge and discharge. The specific test conditions are as follows:
[0190] ① Normal temperature cycle: At room temperature 25℃, 1.5-4.0V voltage range, 1C rate, constant current charge and discharge cycle 1000 times;
[0191] ② Low temperature cycle: In a low temperature environment of 0℃ (high and low temperature box), 1.5-4.0V voltage range, constant current charge and discharge cycle at 0.5C rate for 500 cycles;
[0192] ③ Low temperature discharge performance: At room temperature 25℃, charge the battery to 4.0V at a constant current and constant voltage rate of 1C, with a cut-off rate of 0.05C; place the fully charged battery at -40℃ for 2h, and discharge it to 1.5V at a constant current rate of 1C. ;
[0193] ④ High rate charge and discharge: Under normal temperature 25℃ environment, 1.5-4.0V voltage range, after 3 cycles of constant current charge and discharge at 10C rate, remove the battery and disassemble it to observe the negative electrode surface.
[0194] The test results are shown in Table 2 below:
[0195] Table 2 Comparison of electrochemical performance of sodium battery button cells
[0196]
[0197]
[0198] It can be clearly seen from the above data that: a) With the addition of the novel additive of the present invention, the viscosity of the existing basic electrolyte formula system can be significantly reduced, which can ensure that the battery can maintain a high dynamic performance under low temperature and high rate conditions, and improve the low temperature and rate performance of the battery (Table 1); b) It was tested in the sodium ion battery soft pack that after 1000 cycles at room temperature, the capacity retention rate was above 92.7%; the capacity retention rate of 500 cycles at low temperature (0°C) was above 87.8%; the discharge retention rate at low temperature (-40°C) was above 85.0%, and the negative electrode performance after 10C high rate charge and discharge did not show sodium precipitation, and had a high capacity retention rate after cycling; it can be seen that the multiple synergistic effects of the functional groups of the additive of the present invention jointly contributed to the excellent discharge performance and capacity retention rate of the battery; mainly due to the improvement of the main problem of sodium precipitation in the hard carbon negative electrode, a series of positive improvement results were produced, which provided ideas for the subsequent improvement of the electrolyte for the performance of the hard carbon negative electrode. However, the battery performance of the battery prepared by using the electrolyte containing the existing positive and negative electrode film-forming additives under adverse conditions such as low temperature and high rate is significantly lower than that of the battery using the additives of the present invention.
[0199] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A secondary battery electrolyte, characterized in that: Including additives, the additives have a structure shown in formula I: In formula I, R1 is hydrogen; R2 and R3 are independently selected from H or methyl, and R2 and R3 are not hydrogen at the same time.
2. The secondary battery electrolyte according to claim 1, characterized in that: The additive is selected from one or more of the following compounds:
3. The secondary battery electrolyte according to claim 1, characterized in that: The preparation method of the additive comprises the following steps: A) reacting reactant RX with reactant RY in the presence of a catalyst to obtain a reaction product PX; B) reacting the reaction product PX with hydrogen peroxide in the presence of an alkaline agent to produce an additive having a structure shown in Formula I; Among them, the structure of the reactant RX is R1 is hydrogen; R2 and R3 are independently selected from H, methyl, and R2 and R3 are not hydrogen at the same time; The structure of the reactant RY is Reaction product PX R1 is hydrogen; R2 and R3 are independently selected from H and methyl, and R2 and R3 are not hydrogen at the same time.
4. The secondary battery electrolyte according to claim 3, characterized in that: In step A), the equivalent ratio of the reactant RX to the reactant RY is 1:(1-10); The equivalent ratio of the reactant RX to the catalyst is 1:(0.01-0.02); The catalyst is selected from rhenium heptoxide; The reaction temperature is 0 to 30° C. and the reaction time is 1 to 3 hours.
5. The secondary battery electrolyte according to claim 3, characterized in that: In step B), the concentration of the hydrogen peroxide is 30%; The reaction equivalent ratio of the reaction product PX to hydrogen peroxide is 1:(2-5); The alkaline agent is selected from sodium hydroxide or potassium carbonate; The reaction equivalent ratio of the reaction product PX to the alkaline reagent is 1:(0.2-1); The reaction temperature is divided into three stages. The reaction product PX is mixed with an alkaline reagent at room temperature, and then hydrogen peroxide is added at a temperature of -5°C to 5°C. After the addition of hydrogen peroxide, the reaction temperature is 20 to 50°C, and the reaction time is 1h to 6h.
6. The secondary battery electrolyte according to claim 1, characterized in that: The additive is added in an amount of 1 wt% to 5 wt% in the electrolyte.
7. The secondary battery electrolyte according to claim 1, characterized in that: The electrolyte solution further includes an electrolyte salt and a non-aqueous organic solvent.
8. The secondary battery electrolyte according to claim 7, characterized in that: The electrolyte salt is selected from at least one of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium perchlorate, sodium tetrafluoroborate, sodium difluorophosphate, and sodium difluorooxalatoborate; The non-aqueous organic solvent is selected from one or more of organic ester solvents, C1-10 alkyl ether solvents, cyclic ether solvents, sulfone solvents, and dinitrile solvents.
9. The secondary battery electrolyte according to claim 1, characterized in that: The electrolyte also includes other types of additives, and the other types of additives are selected from vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, vinyl sulfate, vinyl disulfate, propylene sulfate, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, 2,4-butane sultone, phenyl methanesulfonate, methylene methanedisulfonate, N-phenylbis(trifluoromethanesulfonyl)imide, triallyl phosphate, tris(trimethylsilane)phosphide, One or more of ester, trimethyl phosphite, triphenyl phosphite, tetramethylmethylene diphosphate, propargyl phosphate, (2-allylphenoxy)trimethylsilane, tris(trimethylsilyl)borate, 1,3,5-triallyl isocyanurate, isocyanoethyl methacrylate, hexamethylene diisocyanate, p-phenylene diisocyanate, 2,4-toluene diisocyanate, 1,3,6-hexanetrinitrile, 1,2-bis(cyanoethoxy)ethane or ethoxypentafluorocyclotriphosphazene.
10. A secondary battery, characterized in that: The electrolyte comprising any one of claims 1 to 9.