Electrolyte and lithium ion battery containing same
Through the combination of lithium salt compound and organic solvent, the problem of poor performance of lithium-ion batteries in a wide temperature range is solved, excellent cycle stability and high ion conductivity at high and low temperatures are achieved, and the application of lithium-ion batteries is broadened. field.
Patent Information
- Application Number
- CN202410702782.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-01
AI Technical Summary
Existing lithium-ion batteries are difficult to operate stably in a wide temperature range, especially under high and low temperature conditions, and existing electrolyte optimization methods cannot achieve both high and low temperature performance, resulting in increased complexity of the thermal management system and performance degradation.
Lithium salt compounding technology is used, including lithium tetrafluoroborate (LiBF4) and lithium difluoroborate borate (LiODFB) as lithium salts in the electrolyte, combined with cyclic and chain carbonates as organic solvents, and adding esters to form a film Additives to adjust the lithium salt molar concentration and solvent ratio to improve the ionic conductivity and thermal stability of the electrolyte.
It achieves excellent cycle stability of lithium-ion batteries in a wide temperature range of -40°C to 60°C, reduces the design difficulty of thermal management systems, and broadens the application fields of lithium-ion batteries.
Smart Images

Figure CN118738563A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to an electrolyte and a lithium ion battery containing the electrolyte. Background Art
[0002] In order to adapt to the use in different environments, the battery system is required to work at a temperature of -20℃~60℃. However, the optimal operating temperature range of commercial lithium-ion batteries is only 15~35℃, and it is difficult to work stably in such a wide temperature range. Therefore, it is of great significance for the application research of lithium-ion batteries to broaden the operating temperature range of lithium-ion batteries so that they can adapt to extremely harsh environments such as high or low temperatures.
[0003] At present, there are two main optimization strategies to broaden the operating temperature range of lithium-ion batteries: one is to add additional insulation / heating and cooling devices during the battery grouping process to perform thermal management on the battery pack. That is, the battery is isolated from the external environment so that the battery always operates in a more suitable temperature range. Although this solution can alleviate the adverse interference of external temperature on battery performance to a certain extent under the actual situation that the full temperature range performance of the lithium-ion battery itself is poor, and successfully apply lithium-ion batteries in some wide temperature range scenarios. However, the additional thermal management equipment will increase the complexity of the battery system, reduce the energy density and energy efficiency of the battery pack, and increase the manufacturing cost. Moreover, since the performance of the lithium-ion battery itself is very sensitive to temperature, the thermal management system must be carefully designed to ensure the consistency of the temperature of many battery cells, and avoid the attenuation of the overall performance of the battery pack caused by individual cells that deviate from the set operating temperature range, which brings great challenges to the design of the battery thermal management system. Another solution is to optimize the electrolyte system. However, the electrolyte optimization literature reported so far is limited to the study of high temperature or low temperature performance. Even if there are reports on the study of wide temperature range electrolytes, the two performances are basically studied separately and then simply superimposed. However, most electrolytes with good low-temperature performance cannot meet the requirements of high-temperature performance, and vice versa. Therefore, the current research method of simply superimposing them is difficult to obtain an electrolyte system with excellent performance in a wide temperature range.
[0004] Therefore, it is an urgent problem to be solved in this field to develop an electrolyte that has both excellent high-temperature performance and low-temperature performance, can broaden the operating temperature range of lithium-ion batteries, improve the wide-temperature performance of lithium-ion batteries, and enable lithium-ion batteries to have excellent cycle stability under both high and low temperature conditions. Summary of the invention
[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide an electrolyte and a lithium-ion battery containing the same. The electrolyte has both excellent high-temperature performance and low-temperature performance, has high ionic conductivity under both high and low temperature conditions, has good compatibility with lithium-ion batteries, broadens the operating temperature range of lithium-ion batteries, and enables lithium-ion batteries to have excellent cycle stability in a wide temperature range, thereby improving the wide temperature performance of the lithium-ion battery body, which is conducive to reducing the design difficulty of the thermal management system, and can also cooperate with the thermal management system to further broaden the operating temperature range of the lithium-ion battery, thereby broadening its application field.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides an electrolyte, comprising a lithium salt, an organic solvent and a film-forming additive; the lithium salt comprises lithium tetrafluoroborate (LiBF4) and lithium difluorooxalatoborate (LiODFB); the molar concentration of the lithium salt in the electrolyte is 0.1 to 4 mol / L; based on the total mass of the organic solvent and the film-forming additive as 100%, the mass percentage of the organic solvent in the electrolyte is 92 to 99%, and the mass percentage of the film-forming additive is 1 to 8%.
[0008] In the present invention, LiBF4 has a small charge transfer impedance, good low-temperature performance, antioxidant performance and high safety; LiODFB has good thermal stability, high solubility, and the property of forming a film at both the positive and negative electrodes, thereby improving the high-temperature performance of the battery; by compounding LiBF4 and LiODFB, the electrolyte has a wider operating temperature range, good thermal stability and high solubility, and can maintain a high ionic conductivity at low temperatures. Compared with traditional lithium salts (such as lithium hexafluorophosphate LiPF6, lithium bis(trifluoromethylsulfonyl)imide LiTFSI, etc.), it has the advantages of passivated aluminum foil and good compatibility with the positive electrode, thereby broadening the operating temperature range of the lithium-ion battery, so that the lithium-ion battery has excellent cycle stability in a wider temperature range, and the wide temperature performance of the lithium-ion battery body is improved.
[0009] In the present invention, the molar concentration of the lithium salt in the electrolyte is 0.1 to 4 mol / L, for example, it can be 0.1 mol / L, 0.2 mol / L, 0.4 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, 2 mol / L, 2.2 mol / L, 2.5 mol / L, 2.8 mol / L, 3 mol / L, 3.2 mol / L, 3.5 mol / L, 3.8 mol / L, 4 mol / L, etc.
[0010] In the present invention, the mass percentage of the organic solvent in the electrolyte is 92-99%, for example, it can be 92%, 92.2%, 92.4%, 92.6%, 92.8%, 93%, 93.2%, 93.4%, 93.6%, 93.8%, 94%, 94.2%, 94.4%, 94.6%, 94.8%, 95%, 95.2%, 95.4%, 95.6%, 95.8%, 96%, 96.2%, 96.4%, 96.6%, 96.8%, 97%, 97.2%, 97.4%, 97.6%, 97.8%, 98%, 98.2%, 98.4%, 98.6%, 98.8%, 99%, etc.
[0011] In the present invention, if the mass percentage of the organic solvent in the electrolyte is too small, the high-temperature cycle performance of the electrolyte will deteriorate and the low-temperature initial capacity will decrease; if the mass percentage is too large, the content of the film-forming additive will be reduced, and a film cannot be formed, and effective protection cannot be provided.
[0012] In the present invention, the total mass of the organic solvent and the film-forming additive is 100%.
[0013] In the present invention, the mass percentage of the film-forming additive is 1 to 8%, for example, it can be 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.8%, 4%, 4.2%, 4.5%, 4.8%, 5%, 5.2%, 5.5%, 5.8%, 6%, 6.2%, 6.5%, 6.8%, 7%, 7.2%, 7.5%, 7.8%, 8% and the like.
[0014] Preferably, the molar ratio of lithium tetrafluoroborate to lithium difluorooxalatoborate is 1:(0.1-9), wherein the specific value in (0.1-9) can be, for example, 0.1, 0.12, 0.15, 0.18, 0.2, 0.22, 0.25, 0.28, 0.3, 0.32, 0.35, 0.38, 0.4, 0.42, 0.45, 0.48, 0.5, 0.52, 0.55, 0.58, 0.6, 0.62, 0.65, 0.68, 0.7, 0.8 .72, 0.75, 0.78, 0.8, 0.82, 0.85, 0.88, 0.9, 0.95, 1, 1.2, 1.5, 1.8, 2, 2.2, 2.5, 2.8, 3, 3.2, 3.5, 3.8, 4, 4.2, 4.5, 4.8, 5, 5.2, 5.5, 5.8, 6, 6.2, 6.5, 6.8, 7, 7.2, 7.5, 7.8, 8, 8.2, 8.5, 8.8, 9, etc.; more preferably 1:(0.4~0.9).
[0015] In the present invention, the molar ratio of lithium tetrafluoroborate to lithium difluorooxalatoborate is within the above range, and the compatibility is better; if the amount of LiBF4 is too small, the low-temperature performance, antioxidant performance and safety performance are poor; if the amount is too large, the solubility is low, resulting in low ion conductivity of the electrolyte. If the amount of LiODFB is too small, the high-temperature performance is poor; if the amount is too large, the SEI film layer is thicker, resulting in increased charge transfer impedance, making its low-temperature performance poor.
[0016] Preferably, the organic solvent comprises cyclic carbonate and / or chain carbonate.
[0017] In the present invention, LiODFB has a high solubility in carbonate solvents, and the use of carbonate solvents is more conducive to the performance of the composite lithium salt.
[0018] Preferably, the cyclic carbonate includes at least one of ethylene carbonate (EC), propylene carbonate (PC) or butylene carbonate (BC), and more preferably ethylene carbonate and / or propylene carbonate.
[0019] Preferably, the volume ratio of ethylene carbonate to propylene carbonate is 1:(0.5-1.5), wherein the specific value of (0.5-1.5) can be, for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, etc.
[0020] Preferably, the linear carbonate includes at least one of ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC) or methyl propyl carbonate (MPC).
[0021] Preferably, the volume ratio of the cyclic carbonate to the linear carbonate is 1:(0.5-4), wherein the specific value of (0.5-4) can be, for example, 0.5, 0.6, 0.8, 1, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4, 3.6, 3.8, 4, etc.
[0022] Preferably, the film-forming additive comprises an ester additive.
[0023] Preferably, the ester additive includes at least one of fluoroethylene carbonate (FEC), vinylene carbonate (VC), propylene sulfite (PS), ethylene sulfite (ES), chloroethylene carbonate (CEC), vinyl vinyl sulfite (VES) or vinyl ethylene carbonate (VEC).
[0024] In the present invention, the preparation method of the electrolyte comprises: mixing a lithium salt, an organic solvent and a film-forming additive to obtain the electrolyte.
[0025] Preferably, the mixing includes premixing the organic solvent and the film-forming additive, then adding the lithium salt thereto, stirring for 10 to 15 minutes to dissolve, and mixing evenly to obtain the lithium salt.
[0026] In a second aspect, the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the electrolyte according to the first aspect.
[0027] In the present invention, the lithium-ion battery operates at a minimum temperature of ≤-40°C and a maximum temperature of ≥60°C.
[0028] Preferably, the operating temperature range of the lithium-ion battery is -40 to 60° C., for example, -30 to 60° C., -20 to 60° C., etc.
[0029] In the present invention, the lithium-ion battery also includes a positive electrode, a negative electrode and a separator; the slurry of the positive electrode includes an active material, a conductive agent and a binder; the active material includes but is not limited to LiFePO4; the conductive agent includes but is not limited to carbon black; the binder includes but is not limited to polyvinylidene fluoride; the mass ratio of the active material, the conductive agent and the binder is 8:(0.5~1.5):(0.5~1.5); the negative electrode includes a lithium sheet; the separator can be a conventional commercially available separator or a separator disclosed in the literature, including but not limited to a polypropylene separator.
[0030] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The electrolyte provided by the present invention is compounded with LiBF4 and LiODFB, so that the electrolyte has both excellent high-temperature performance and low-temperature performance, has a wider operating temperature range, and has higher ionic conductivity within the corresponding operating temperature range. Compared with traditional lithium salts (such as lithium hexafluorophosphate LiPF6, lithium bis(trifluoromethylsulfonyl)imide LiTFSI, etc.), it has good compatibility with lithium-ion batteries, broadens the operating temperature range of lithium-ion batteries, and enables lithium-ion batteries to have excellent cycle stability within a wider temperature range, improves the wide temperature performance of the lithium-ion battery body, and has low cost, thereby expanding the application field of lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a curve diagram of the change in ionic conductivity of the electrolyte provided by Examples 1 to 6 of the present invention and Comparative Examples 1 and 2 at -40 to 60°C. DETAILED DESCRIPTION
[0034] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0035] Example 1
[0036] The present embodiment provides an electrolyte, comprising an organic solvent, a film-forming additive and a lithium salt; the mass percentage of the organic solvent in the electrolyte is 95%, which is PC, EC and EMC in a volume ratio of 1:1:3; the molar concentration of the lithium salt in the electrolyte is 1 mol / L, which is LiBF4 and LiODFB in a molar ratio of 1:0.11; the mass percentage of the film-forming additive in the electrolyte is 5%, which is FEC.
[0037] This embodiment provides a method for preparing an electrolyte, which specifically includes the following steps:
[0038] PC, EC and EMC are mixed according to the formula to obtain an organic solvent; FEC is added to the organic solvent, and then a mixed lithium salt of LiBF4 and LiODFB is added thereto, and the mixture is stirred for 15 minutes and mixed evenly to obtain the electrolyte.
[0039] Example 2
[0040] This embodiment provides an electrolyte, which differs from Embodiment 1 only in that the total molar amount of the lithium salt remains unchanged, the molar ratio of LiBF4 to LiODFB is 1:0.25, and the other components, amounts and preparation methods are the same as those in Embodiment 1.
[0041] Example 3
[0042] This embodiment provides an electrolyte, which differs from Embodiment 1 only in that the total molar amount of the lithium salt remains unchanged, the molar ratio of LiBF4 to LiODFB is 1:0.43, and the other components, amounts and preparation methods are the same as those in Embodiment 1.
[0043] Example 4
[0044] This embodiment provides an electrolyte, which differs from Embodiment 1 only in that the total molar amount of the lithium salt remains unchanged, the molar ratio of LiBF4 to LiODFB is 1:0.9, and the other components, amounts and preparation methods are the same as those in Embodiment 1.
[0045] Example 5
[0046] This embodiment provides an electrolyte, which differs from Embodiment 1 only in that the total molar amount of the lithium salt remains unchanged, the molar ratio of LiBF4 to LiODFB is 1:2.33, and the other components, amounts and preparation methods are the same as those in Embodiment 1.
[0047] Example 6
[0048] This embodiment provides an electrolyte, which is different from Embodiment 1 only in that the total molar amount of the lithium salt remains unchanged, the molar ratio of LiBF4 to LiODFB is 1:9, and the other components, amounts and preparation methods are the same as those in Embodiment 1.
[0049] Example 7
[0050] This embodiment provides an electrolyte, including an organic solvent, a film-forming additive and a lithium salt; the mass percentage of the organic solvent in the electrolyte is 92.5%, which is PC, EC and DMC in a volume ratio of 1.5:1:5; the molar concentration of the lithium salt is 3 mol / L, which is LiBF4 and LiODFB in a molar ratio of 1:0.8; the mass percentage of the film-forming additive in the electrolyte is 7.5%, which is FEC, and the preparation method is the same as that in Example 1.
[0051] Example 8
[0052] This embodiment provides an electrolyte, including an organic solvent, a film-forming additive and a lithium salt; the mass percentage of the organic solvent in the electrolyte is 97%, which is PC, EC and DEC in a volume ratio of 1:1:3; the molar concentration of the lithium salt is 0.5 mol / L, which is LiBF4 and LiODFB in a molar ratio of 1:0.6; the mass percentage of the film-forming additive in the electrolyte is 3%, which is FEC, and the preparation method is the same as that in Example 1.
[0053] Example 9
[0054] This embodiment provides an electrolyte, which is different from Example 1 only in that the total mass of the organic solvent remains unchanged, including PC, EC, EMC and ethyl acetate in a mass ratio of 1:1:3:1, and other components, amounts and preparation methods are the same as those in Example 1.
[0055] Comparative Example 1
[0056] This comparative example provides an electrolyte, which is different from Example 1 only in that the total molar amount of the lithium salt remains unchanged, LiODFB is not included, and other components, amounts and preparation methods are the same as those in Example 1.
[0057] Comparative Example 2
[0058] This comparative example provides an electrolyte, which differs from Example 1 only in that the total molar amount of the lithium salt remains unchanged, LiBF4 is absent, and other components, amounts used, and preparation methods are the same as those in Example 1.
[0059] Comparative Example 3
[0060] This comparative example provides an electrolyte, which differs from Example 1 only in that LiBF4 is replaced by an equimolar amount of lithium hexafluorophosphate, and the other components, amounts and preparation methods are the same as those in Example 1.
[0061] Comparative Example 4
[0062] This comparative example provides an electrolyte, which differs from Example 1 only in that LiODFB is replaced by an equimolar amount of lithium dioxalatoborate, and the other components, amounts and preparation methods are the same as those in Example 1.
[0063] Comparative Example 5
[0064] This comparative example provides an electrolyte, which differs from Example 1 only in that the mass percentage of the organic solvent is 85%, the mass percentage of the film-forming additive is 15%, and the other component types, proportions and preparation methods are the same as those in Example 1.
[0065] Performance Testing
[0066] 1. Test of ionic conductivity
[0067] 5 mL of the electrolyte provided in Examples 1 to 6 and Comparative Examples 1 and 2 were respectively measured and injected into a polytetrafluoroethylene reagent bottle, and then placed in a high and low temperature test box after inserting a conductivity electrode. The test temperature range was: -40 to 60 ° C, and the measurement was performed every 10 ° C. At the temperature to be measured, the electrolyte was allowed to stand for 0.5 to 1 h, and then measured with a conductivity meter to obtain the ionic conductivity value of the electrolyte in the temperature range of -40 to 60 ° C. The results are as follows Figure 1 As shown, it can be seen that the electrolyte system provided by the present invention has a relatively high ionic conductivity within the temperature range of -40 to 60°C.
[0068] 2. Test of high and low temperature cycle performance of lithium-ion batteries
[0069] 100 μL of the electrolyte provided in Examples 1 to 9 and Comparative Examples 1 to 5 were respectively loaded into lithium ion half-cells to assemble lithium ion batteries; wherein the lithium sheet was used as the negative electrode, the current collector of the positive electrode was aluminum foil, the active material was LiFePO4, the conductive agent was carbon black, the binder was polyvinylidene fluoride, the mass ratio of LiFePO4 to the conductive agent and the binder was 8:1:1, and the diaphragm was a 16 mm polyethylene (PE) diaphragm. Then the CT2001A blue battery test system was used to test the cycle performance of the lithium ion battery at different temperatures at a charge and discharge rate of 1C / 1C; the test conditions were: voltage range: 2.5 to 4.2V.
[0070] The specific test results are shown in Table 1:
[0071] Table 1
[0072]
[0073]
[0074] As can be seen from Table 1, the electrolyte provided by the present invention, by compounding LiBF4 and LiODFB, enables the lithium ion battery to have a wider operating temperature range and has excellent cycle stability in the range of -20 to 60°C; at -20°C, the initial capacity of the lithium ion battery is ≥75mAh / g, and the capacity retention rate is ≥70% after 300 cycles; at 60°C, the initial capacity is ≥148mAh / g, and the capacity retention rate is ≥72% after 500 cycles.
[0075] It can be seen from Example 1 and Comparative Examples 1 and 2 that it is not the combination of LiBF4 and LiODFB, but only one of them is selected, the high temperature cycle performance of the lithium ion battery is poor or the low temperature initial capacity is low; it can be seen from Comparative Examples 3 and 4 that it is not the combination of LiBF4 and LiODFB, even if the two lithium salts are compounded, the high temperature cycle performance of the lithium ion battery is still poor or the low temperature initial capacity is low. It can be seen from Comparative Example 5 that when the organic solvent content is reduced and the film-forming additive content is increased, the high temperature cycle performance of the electrolyte deteriorates.
[0076] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. An electrolyte, characterized in that: The electrolyte comprises a lithium salt, an organic solvent and a film-forming additive; The lithium salts include lithium tetrafluoroborate and lithium difluorooxalatoborate; The molar concentration of lithium salt in the electrolyte is 0.1 to 4 mol / L; Taking the total mass of the organic solvent and the film-forming additive as 100%, the mass percentage of the organic solvent in the electrolyte is 92-99%, and the mass percentage of the film-forming additive is 1-8%.
2. The electrolyte according to claim 1, characterized in that The molar ratio of lithium tetrafluoroborate to lithium difluorooxalatoborate is 1:(0.1-9).
3. The electrolyte according to claim 1 or 2, characterized in that The organic solvent includes cyclic carbonate and / or chain carbonate.
4. The electrolyte according to claim 3, characterized in that The cyclic carbonate includes at least one of ethylene carbonate, propylene carbonate or butylene carbonate, and more preferably ethylene carbonate and / or propylene carbonate.
5. The electrolyte according to claim 4, characterized in that The volume ratio of the ethylene carbonate to the propylene carbonate is 1:(0.5-1.5).
6. The electrolyte according to claim 3, characterized in that The linear carbonate includes at least one of ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate or methyl propyl carbonate.
7. The electrolyte according to any one of claims 3 to 6, characterized in that The volume ratio of the cyclic carbonate to the chain carbonate is 1:(0.5-4).
8. The electrolyte according to any one of claims 1 to 7, characterized in that The film-forming additive includes an ester additive; Preferably, the ester additive includes at least one of fluoroethylene carbonate, vinylene carbonate, propylene sulfite, ethylene sulfite, chloroethylene carbonate, vinyl vinyl sulfite or vinyl ethylene carbonate.
9. A lithium ion battery, characterized in that: The lithium-ion battery comprises the electrolyte according to any one of claims 1 to 8.
10. The lithium ion battery according to claim 9, characterized in that: The lithium-ion battery has a minimum operating temperature of ≤-40°C and a maximum operating temperature of ≥60°C.
Citation Information
Cited By
Wide-temperature-range electrolyte for lithium ion battery and preparation method of wide-temperature-range electrolyte
CN120127215A