Preparation method of nickel-based single-crystal high-temperature alloy with high structure stability and high Re content
By reasonably designing the composition and process of nickel-based single-crystal high-temperature alloys and controlling the distribution and segregation of refractory elements, the problem of TCP phase precipitation in the third generation nickel-based single-crystal high-temperature alloys is solved, and the structure stability and high-temperature performance are improved. The production cost is reduced and the performance comparable to that of the same generation of secondary alloys is achieved.
Patent Information
- Application Number
- CN202411064673.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
Separation of refractory elements in third-generation nickel-based single-crystalline high-temperature alloys leads to the precipitation of harmful topological tight-packed phases (TCP), which reduces the structural stability of the alloy and reduces the content of refractory elements, which will lead to a decrease in the high-temperature mechanical properties. The structure stability and performance of the alloy are improved without adding rare and precious elements Ru.
By rationally designing the alloy components, controlling the distribution ratio of Al, Ta, W, and Re, using empirical formulas to determine the distribution ratio of elements in the trunk and the region between dendrite, adjusting the proportion of segregation coefficients, and using vacuum induction smelting and magnetic field stirring, etc. The process reduces the segregation degree of refractory elements and improves the composition uniformity and tissue stability of the alloy.
It effectively reduces the precipitation tendency of TCP phase, improves the high-temperature structure stability and mechanical properties of the alloy, reduces production costs, and reaches the performance level of the same generation of secondary alloys without adding Ru.
Smart Images

Figure CN118957361A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-temperature alloys, and in particular relates to a method for preparing a nickel-based single crystal high-temperature alloy with high organizational stability and high Re content. Background Art
[0002] High-temperature alloys are mainly used to manufacture hot-end components of aircraft engines and gas turbines. They usually have high room temperature and high temperature strength, good oxidation resistance and thermal corrosion resistance, excellent creep and fatigue resistance, good organizational stability and reliability. Among them, single-crystal alloys prepared by directional solidification process eliminate grain boundaries, reduce the application of low-melting-point grain boundary strengthening elements, increase the initial melting temperature of the alloy, enable the alloy to be solution treated at a higher temperature, obtain a larger area of γ' phase, and greatly develop the use potential of the alloy.
[0003] At present, nickel-based single crystal high-temperature alloys have developed to the fifth generation, and the commercial application of the second-generation nickel-based single crystal high-temperature alloys has also matured. With the continuous development of engine technology and the continuous improvement of thrust-to-weight ratio, higher requirements are also placed on the performance of materials required to produce blades. Therefore, the design and application of the third-generation single crystal high-temperature alloys have become the focus of attention of the entire industry. By increasing the Re element content in the second-generation single crystal alloy to 6%, the high-temperature performance of the alloy can be further improved. On the other hand, due to the increase in the Re element content, the initial melting temperature of the alloy is increased, while also intensifying the macroscopic segregation of other elements in the interdendritic / dendritic stem area, thereby increasing the precipitation tendency of harmful topological dense phases (TCP) of the alloy under long-term high temperature conditions. The precipitation of harmful TCP phase is mainly due to the segregation of refractory elements such as W, Mo, Ta, and Re in the interdendritic or dendrite trunk regions. Once the TCP phase precipitates in the alloy during long-term service, the microstructure stability of the single crystal high-temperature alloy will decrease rapidly. Therefore, reducing the segregation degree of refractory elements in the alloy is the key to improving the long-term high-temperature microstructure stability of the alloy. However, the reduction of the content of refractory elements in the alloy is likely to lead to a decrease in the high-temperature mechanical properties of the alloy. Therefore, how to add more refractory elements to the third-generation high-temperature alloy without precipitating harmful TCP phase is a difficult point in the design of high-temperature alloys. At present, the control of the precipitation of harmful TCP phase in high-temperature alloys mainly adopts calculation methods such as the number of electronic control digits, but the basic principle of this method is that there is no segregation in the alloy and the alloy composition is completely uniform. However, in actual production, due to the segregation characteristics of the alloy elements themselves, as well as the low temperature and slow solidification rate during the solidification process, a large component segregation is also formed in the dendrite trunk / interdendritic region of the alloy. However, this segregation is difficult to completely eliminate only through subsequent heat treatment methods. Therefore, how to improve the stability of the alloy structure through alloy composition design without adding rare elements such as Ru, and achieve the performance requirements of the same generation of alloys, is the key to alloy design. In summary, there is an urgent need for a preparation method of a nickel-based single crystal high-temperature alloy that can effectively solve the problem of structural stability of nickel-based single crystal high-temperature alloys with high Re content and control production costs, while its comprehensive performance meets the requirements of alloy use. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a nickel-based single crystal high-temperature alloy with high organizational stability and high Re content in view of the deficiencies of the above-mentioned prior art. The high Re content nickel-based single crystal high-temperature alloy prepared by this method has the characteristics of excellent comprehensive performance and high organizational stability.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a nickel-based single crystal high-temperature alloy with high organizational stability and high Re content, wherein the nickel-based single crystal high-temperature alloy with high organizational stability and high Re content is made of the following raw materials by mass fraction: Cr 2.5wt%~3.5wt%, Co11.5wt%~12.5wt%, W5.5wt%~6.5wt%, Mo0.7wt%~1.3wt%, Al5.0wt%~6.0wt%, Ta7.0wt%~9.0wt%, Re4.5wt%~5.5wt%, Hf 0.005wt%~0.01wt%, and the balance is Ni;
[0006] The impurity control content requirements detected in the prepared nickel-based single crystal high-temperature alloy with high organizational stability and high Re content are O≤5ppm, S≤20ppm, C≤0.05wt%, Ti≤0.05wt%, and Nb≤0.03wt%;
[0007] The idea of designing alloy components in the present invention is: since nickel-based high-temperature alloys are mainly solidified in the form of dendrites, among the many added elements of the high-temperature alloy, their solubility in the γ matrix and γ' phase and their melting points are the main factors affecting their solidification order. Among them, W and Re have higher melting points and stronger solubility in the γ matrix, so they are mainly distributed in the dendrite trunk area where the alloy solidifies first; while Al and Ta are the main constituent elements of the γ' phase, so they are mainly distributed in the interdendritic area where the alloy solidifies later; and although Mo is mainly dissolved in the matrix and has a higher melting point, due to its lower solubility in the γ matrix, it is usually mainly distributed in the interdendritic area that solidifies later.
[0008] Therefore, the main idea of the present invention during the alloy composition design is to control the Al content in the alloy, increase the precipitation driving force of the γ' phase in the dendrite trunk of the alloy ingot during the solidification stage (dominated by the Al concentration gradient), so that the W and Re elements that are mainly concentrated in the dendrite trunk area and dissolved in the γ matrix can enter the interdendritic area more, and Ta, another main constituent element of the γ' phase, can be dissolved as much as possible in the γ' phase in the dendrite trunk area, thereby reducing the segregation degree of W, Re, and Ta in different areas, thereby achieving the purpose of homogenizing the alloy ingot.
[0009] Taking into account the solid solubility of different elements in the matrix, the composition ratio can be calculated according to the following empirical formula to determine the addition amount of W, Ta, Re, Mo, and Al in the alloy. The empirical formula is:
[0010]
[0011] In the formula, A i is the atomic percentage of added element i, R iThe distribution ratio of the i element in the dendrite trunk and interdendritic region in such high Re content cast alloy ingots is obtained based on the previous statistical results and analytical experience. The element distribution ratio involved in the patent is shown in Table 1; A Al is the atomic percentage of Al element.
[0012] Table 1 Distribution ratio of characteristic elements in the dendrite trunk and interdendritic region according to the present invention
[0013] element Al W Ta Mo Re Allocation ratio 0.462 0.547 0.458 0.286 0.562
[0014] The nickel-based single crystal high-temperature alloy with high organizational stability and high Re content has a weight ratio of 13.5%≤Al+Ti+Ta≤14.0% for the strengthening γ' phase-forming elements in the alloy, a volume fraction of 66-70% for the γ' phase, a size of 400-430 mm, and a γ collective channel width of about 40-50 mm.
[0015] The content of Cr, Co and other elements with segregation coefficient K≈1 can be increased, and the addition of elements with K≈1 can change the segregation behavior of elements with K>1, so the weight ratio of the addition of elements with K≈1 is 14.5%≤Cr+Co≤15.0%. The weight ratio of the addition of elements with K>1 such as W, Mo, Re, and Ta is 19.89%≤W+Mo+Re+Ta≤21.0%.
[0016] The total content of K>1 elements in the alloy / the total content of K≈1 elements is 0.72~0.75.
[0017] The weight ratio of K<1 element content in the alloy is 5.0%≤Al+Ti+Hf+Nb≤6.0%, and the total content of K<1 element / the total content of K>1 element in the alloy is 2.6-2.8.
[0018] The total content of impurity elements such as O and S in the alloy / K>1 The total content of elements is 1×10 -5 ~1×10 -6 .
[0019] The preparation method of the nickel-based single crystal high-temperature alloy with high organizational stability and high Re content is as follows:
[0020] S1. Co, W, Mo, Ta, Cr and Ni are sequentially loaded into a crucible for vacuum induction melting. After molten metal is purified, Re and Hf are added for the first alloying. After the first refining at 1500°C to 1600°C, Al is added to the alloy liquid for the second alloying. The temperature is adjusted to 1350°C to 1400°C for the second refining to obtain a melt.
[0021] S2. After adjusting the temperature of the melt obtained in S1 to 1470° C., a casting process is performed to obtain a nickel-based single crystal high-temperature alloy with high structural stability and high Re content.
[0022] Preferably, the first refining time in S1 is 5 min to 20 min, and the second refining time is 10 min to 30 min.
[0023] Preferably, the power outage and cooling time in S1 is 1 min to 5 min.
[0024] Preferably, during the pouring process in S2, a strong magnetic field is used to stir the semi-solid high-temperature ingot in the mold chamber, the magnetic field strength is 5T to 6T, the stirring time is 15min to 20min, the magnetic field is used to refine the grains and reduce segregation, and when the high-temperature ingot is cooled to 1330°C to 1340°C, direct current is passed through the ingot, the DC voltage is 100V to 150V, and the current is 35 to 40A, and the electric field is used to promote the diffusion of elements in the high-temperature ingot to further reduce segregation.
[0025] Preferably, after the pouring treatment in S2, when the temperature of the obtained high-temperature ingot is reduced to 850-900°C, high-purity Ar gas is introduced into the pouring chamber until the pressure gauge shows 0.4-0.8 MPa, then the Ar gas input is stopped, and after standing for 5-15 minutes, the vacuum pump group is turned on, and Ar gas is continued to be introduced at a pressure of 0.2-0.8 MPa. After 10-20 minutes, the Ar gas input is stopped, and the gate valve is opened to allow the air pressure in the pouring chamber to reach atmospheric pressure before taking it out of the furnace to obtain a nickel-based single crystal high-temperature alloy with high organizational stability and high Re content.
[0026] In order to improve the resistance to long-term creep of nickel-based single crystal high-temperature alloys while maintaining the high-temperature microstructure stability of the alloy, the present invention proposes a new alloy composition design scheme, the main concept is as follows: formulate the distribution ratio of Al, Ta, W, and Re in the alloy according to the empirical formula, design a reasonable alloy composition, and optimize the alloy composition design by adjusting the proportion of elements with different segregation coefficients, and finally obtain the third-generation nickel-based single crystal high-temperature alloy with performance that meets the requirements and has high microstructure stability. It solves the common problem of harmful TCP phase precipitation in the third-generation single crystal high-temperature alloys, provides material support for the commercial application of the third-generation alloys, and has important scientific and social significance.
[0027] Compared with the prior art, the present invention has the following advantages:
[0028] 1. The present invention reduces the segregation degree of refractory elements in the interdendritic / dendrite trunk area and the precipitation tendency of TCP phase through reasonable alloy composition design; in addition, the cooling rate of alloy ingot after pouring is accelerated during the preparation process, further improving the composition uniformity of the alloy and avoiding the inheritance of the initial TCP phase in the master alloy ingot into the casting. It can effectively improve the high-temperature structure stability of the third-generation nickel-based single crystal high-temperature alloy and improve the high-temperature performance of the alloy.
[0029] 2. In the case of not adding Ru element, the alloy of the present invention has higher organizational stability than the same generation of sub-single crystal alloys. The alloy mechanical properties are equivalent to those of the same generation of sub-single crystal alloys. The alloy has higher oxidation resistance, and the oxidation resistance reaches the oxidation resistance level. When the comprehensive performance of the alloy reaches or even exceeds that of the same generation of sub-single crystal alloys, the amount of Re element added is only 83% of that of the same generation of sub-single crystal alloys, which greatly reduces the production cost.
[0030] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the dendrite structure of the nickel-based single crystal high-temperature alloy prepared in Example 1 of the present invention.
[0032] Figure 2 This is the heat-treated microstructure of the nickel-based single crystal high-temperature alloy prepared in Example 1 of the present invention.
[0033] Figure 3 The microstructure of a nickel-based single crystal high-temperature alloy prepared in Example 1 of the present invention after long-term aging at 1100°C / 1000h.
[0034] Figure 4 The microstructure of a nickel-based single crystal high-temperature alloy prepared in Example 2 of the present invention after long-term aging at 1100°C / 1000h.
[0035] Figure 5 is the Larson-Miller curve of a typical alloy of the present invention. DETAILED DESCRIPTION
[0036] Example 1
[0037] The preparation method of the nickel-based single crystal high-temperature alloy with high organizational stability and high Re content in this embodiment is to prepare 60 kg of nickel-based single crystal high-temperature alloy ingots, feed 80 kg of materials, and cast a total of 3 alloy ingots of φ85×550 mm. The nominal chemical composition is: 2.50wt% Cr, 11.50wt% Co, 5.50wt% W, 0.70wt% Mo, 5.00wt% Al, 7.00wt% Ta, 4.50wt% Re, 0.005wt% Hf, and Ni is the balance.
[0038] The specific steps are as follows:
[0039] According to the batching points shown in Table 2, weigh pure raw materials with low impurity element content.
[0040] Table 2 Nickel-based high-temperature alloy batching points
[0041] raw materials Mass ratio, % Weighing weight, kg Cr 2.50 4.00 Co 11.50 9.20 W 5.50 4.40 Mo 0.70 0.56 Al 5.00 4.00 Ta 7.00 5.60 Re 4.50 3.60 Hf 0.005 0.004 Ni margin 48.63
[0042] Among them, the calculation formulas for elements such as Al, Ta, W, and Re are as follows:
[0043]
[0044] In the formula, A i is the atomic percentage of added element i, R i The distribution ratio of the i element in the dendrite trunk and interdendritic region in such high Re content cast alloy ingots is obtained based on the previous statistical results and analytical experience. The element distribution ratio involved in the patent is shown in Table 1; A Al is the atomic percentage of Al element.
[0045] Table 1 Distribution ratio of characteristic elements in the dendrite trunk and interdendritic region according to the present invention
[0046] element Al W Ta Mo Re Allocation ratio 0.462 0.547 0.458 0.286 0.562
[0047] The calculation result is
[0048] The preparation method of the nickel-based single crystal high-temperature alloy with high organizational stability and high Re content is as follows:
[0049] S1. Co, W, Mo, Ta, Cr and Ni are sequentially loaded into a crucible for vacuum induction melting. After molten metal is purified, Re and Hf are added for the first alloying. After the first refining at 1500°C for 20 minutes, the power is turned off and the temperature is cooled for 5 minutes. Al is then added to the alloy liquid for the second alloying. The temperature is adjusted to 1350°C to 1400°C for the second refining for 30 minutes to obtain a melt.
[0050] S2, adjusting the temperature of the melt obtained in S1 to 1470° C., and then performing a casting process to obtain a nickel-based single crystal high-temperature alloy with high structural stability and high Re content;
[0051] During the pouring process, a strong magnetic field is used in the mold room to stir the semi-solid high-temperature ingot. The magnetic field strength is 5T and the stirring time is 15 minutes. The magnetic field is used to refine the grains and reduce segregation. When the high-temperature ingot is cooled to 1330°C, direct current is passed through the ingot with a DC voltage of 100V and a current of 35A. The electric field is used to promote the diffusion of elements in the high-temperature ingot and further reduce segregation.
[0052] After the pouring treatment, when the temperature of the obtained high-temperature ingot is reduced to 850°C, high-purity Ar gas is introduced into the pouring chamber until the pressure gauge shows 0.8MPa, then the Ar gas input is stopped. After standing for 15 minutes, the vacuum pump group is turned on, and Ar gas is continued to be introduced at a pressure of 0.8MPa. After 20 minutes, the Ar gas input is stopped, and the gate valve is opened to allow the air pressure in the pouring chamber to reach atmospheric pressure before taking the ingot out of the furnace to obtain a nickel-based single crystal high-temperature alloy with high organizational stability and high Re content.
[0053] The impurity control content requirements detected in this embodiment are: O≤5ppm, S≤20ppm, C≤0.05wt%, Ti≤0.05wt%, Nb≤0.03wt%;
[0054] The impurity content of the nickel-based single crystal high-temperature alloy with high organizational stability and high Re content prepared in this embodiment meets the control requirements.
[0055] Figure 1 This is the dendritic structure of a nickel-based single crystal high-temperature alloy prepared in this embodiment. The primary dendrites of the alloy are evenly distributed, regular in shape, and the primary dendrite spacing is in line with expectations.
[0056] Figure 2 This is a heat-treated microstructure of a nickel-based single crystal high-temperature alloy prepared in this embodiment. After complete heat treatment, the cubic degree of the γ' phase is good and the size is uniform.
[0057] According to the volume of the mold shell, 5 kg of the polished mother alloy ingot was cut and the first refining temperature in the remelting process was 1550°C. Directional solidification was carried out at a crystal pulling rate of 5 mm / min. After directional solidification, when the temperature of the single crystal high-temperature alloy casting was 1250°C, the single crystal high-temperature alloy casting was taken out of the mold chamber and connected to a DC power supply with a voltage of 34 V and a current of 15 A. The processing time was 5 h, and the cooling rate of the test rod was 4.0°C / min.
[0058] The cast single crystal test rod was heat treated, and then subjected to long-term aging treatment to observe its microstructure in the heat treated and aged state. Figure 3 There is no obvious TCP phase inside the alloy, which proves that the alloy has excellent microstructural stability.
[0059] The mechanical properties of the single crystal test rod after heat treatment were tested, and the results are shown in Table 3.
[0060] Table 3 Typical mechanical properties test results of the alloy in this example
[0061]
[0062] Example 2
[0063] The method for preparing a nickel-based single crystal high-temperature alloy with high organizational stability and high Re content in this embodiment is to prepare 60 kg of a nickel-based single crystal high-temperature alloy ingot, feed 80 kg of material, and cast a total of 3 alloy ingots of φ85×550 mm, with a nominal chemical composition of 3.50 wt% Cr, 12.50 wt% Co, 6.50 wt% W, 1.30 wt% Mo, 6.00 wt% Al, 9.00 wt% Ta, 5.50 wt% Re, 0.01 wt% Hf, and Ni as the balance;
[0064] The specific steps are as follows:
[0065] (1) According to the batching points shown in Table 4, weigh pure raw materials with low impurity content.
[0066] Table 4 Nickel-based high-temperature alloy batching points
[0067] raw materials Mass ratio, % Weighing weight, kg Cr 3.50 5.60 Co 12.50 10.00 W 6.50 5.20 Mo 1.30 1.04 Al 6.00 4.80 Ta 9.00 7.20 Re 5.50 4.40 Hf 0.01 0.008 Ni margin 41.75
[0068] Among them, the calculation formulas for elements such as Al, Ta, W, and Re are as follows:
[0069]
[0070] In the formula, A i is the atomic percentage of added element i, R i The distribution ratio of the i element in the dendrite trunk and interdendritic region in such high Re content cast alloy ingots is obtained based on the previous statistical results and analytical experience. The element distribution ratio involved in the patent is shown in Table 1; A Al is the atomic percentage of Al element.
[0071] Table 1 Distribution ratio of characteristic elements involved in this patent in dendrite trunk and interdendritic region
[0072] element Al W Ta Mo Re Allocation ratio 0.462 0.547 0.458 0.286 0.562
[0073] The calculation result is
[0074] The preparation method of the nickel-based single crystal high-temperature alloy with high organizational stability and high Re content is as follows:
[0075] S1. Co, W, Mo, Ta, Cr and Ni are sequentially loaded into a crucible for vacuum induction melting. After molten metal is purified, Re and Hf are added for the first alloying. After the first refining is performed at 1600°C for 5 minutes, the power is turned off and the temperature is cooled for 1 minute. Al is then added to the alloy liquid for the second alloying. The temperature is adjusted to 1350°C for the second refining for 10 minutes to obtain a melt.
[0076] S2, adjusting the temperature of the melt obtained in S1 to 1470° C., and then performing a casting process to obtain a nickel-based single crystal high-temperature alloy with high structural stability and high Re content;
[0077] During the pouring process, a strong magnetic field is used in the mold room to stir the semi-solid high-temperature ingot. The magnetic field strength is 6T and the stirring time is 20 minutes. The magnetic field is used to refine the grains and reduce segregation. When the high-temperature ingot is cooled to 1340°C, direct current is passed through the ingot with a DC voltage of 150V and a current of 40A. The electric field is used to promote the diffusion of elements in the high-temperature ingot and further reduce segregation.
[0078] After the pouring treatment, when the temperature of the obtained high-temperature ingot is reduced to 900°C, high-purity Ar gas is introduced into the pouring chamber until the pressure gauge shows 0.4MPa and then the Ar gas input is stopped. After standing for 5 minutes, the vacuum pump group is turned on, and Ar gas is continued to be introduced at a pressure of 0.2MPa. After 10 minutes, the Ar gas input is stopped, and the gate valve is opened to allow the air pressure in the pouring chamber to reach atmospheric pressure before taking it out of the furnace to obtain a nickel-based single crystal high-temperature alloy with high organizational stability and high Re content.
[0079] The impurity control content requirements detected in this embodiment are: O≤5ppm, S≤20ppm, C≤0.05wt%, Ti≤0.05wt%, Nb≤0.03wt%;
[0080] The impurity content of the nickel-based single crystal high-temperature alloy with high organizational stability and high Re content prepared in this embodiment meets the control requirements.
[0081] According to the volume of the mold shell, 5 kg of the polished mother alloy ingot was cut and the first refining temperature in the remelting process was 1550°C. Directional solidification was carried out at a crystal pulling rate of 5 mm / min. After directional solidification, when the temperature of the single crystal high-temperature alloy casting was 1250°C, the single crystal high-temperature alloy casting was taken out of the mold chamber and connected to a DC power supply with a voltage of 34 V and a current of 15 A. The processing time was 5 h, and the cooling rate of the test rod was 4.0°C / min.
[0082] The cast single crystal test rod was heat treated, and then subjected to long-term aging treatment to observe its microstructure in the heat treated and aged state. Figure 4 There is no obvious TCP phase inside the alloy, which proves that the alloy has excellent microstructural stability.
[0083] The mechanical properties of the single crystal test rod after heat treatment were tested, and the results are shown in Table 4.
[0084] Figure 5Comparing the average values of alloy embodiments 1-2 of the present invention with the Larson-Miller curves of typical third-generation single crystal alloys, the alloy of the present invention can reach the same level as the sub-single crystal alloys of the same generation.
[0085] The mechanical properties of the single crystal test rod after heat treatment were tested, and the results are shown in Table 5.
[0086] Table 5 Typical mechanical properties test results of the alloy in this example
[0087]
[0088] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a nickel-based single crystal high-temperature alloy with high structural stability and high Re content, characterized in that: The nickel-based single crystal high-temperature alloy with high organizational stability and high Re content is made of the following raw materials in mass fraction: 2.5 wt% to 3.5 wt% of Cr, 11.5 wt% to 12.5 wt% of Co, 5.5 wt% to 6.5 wt% of W, 0.7 wt% to 1.3 wt% of Mo, 5.0 wt% to 6.0 wt% of Al, 7.0 wt% to 9.0 wt% of Ta, 4.5 wt% to 5.5 wt% of Re, 0.005 wt% to 0.01 wt% of Hf, and the balance is Ni; The impurity control content requirements detected in the prepared nickel-based single crystal high-temperature alloy with high organizational stability and high Re content are O≤5ppm, S≤20ppm, C≤0.05wt%, Ti≤0.05wt%, and Nb≤0.03wt%; The method is: S1. Co, W, Mo, Ta, Cr and Ni are sequentially loaded into a crucible for vacuum induction melting. After molten metal is purified, Re and Hf are added for the first alloying. After the first refining at 1500°C to 1600°C, Al is added to the alloy liquid for the second alloying. The temperature is adjusted to 1350°C to 1400°C for the second refining to obtain a melt. S2. After adjusting the temperature of the melt obtained in S1 to 1470°C, a casting process is performed to obtain a nickel-based single crystal high-temperature alloy with high structural stability and high Re content.
2. The method for preparing a nickel-based single crystal high-temperature alloy with high structural stability and high Re content according to claim 1, characterized in that: The time of the first refining in S1 is 5 min to 20 min, and the time of the second refining is 10 min to 30 min.
3. The method for preparing a nickel-based single crystal high-temperature alloy with high structural stability and high Re content according to claim 1, characterized in that: The power outage and cooling time in S1 is 1 min to 5 min.
4. The method for preparing a nickel-based single crystal high-temperature alloy with high structural stability and high Re content according to claim 1, characterized in that: During the pouring process in S2, a strong magnetic field is used in the casting chamber to stir the semi-solid high-temperature ingot. The magnetic field strength is 5T to 6T, and the stirring time is 15min to 20min. When the high-temperature ingot is cooled to 1330℃ to 1340℃, direct current is passed through the ingot. The DC voltage is 100V to 150V, and the current is 35 to 40A.
5. The method for preparing a nickel-based single crystal high-temperature alloy with high structural stability and high Re content according to claim 1, characterized in that: After the pouring treatment in S2, when the temperature of the obtained high-temperature ingot is reduced to 850-900°C, high-purity Ar gas is introduced into the pouring chamber until the pressure gauge shows 0.4-0.8MPa, then the Ar gas input is stopped. After standing for 5-15 minutes, the vacuum pump group is turned on, and Ar gas is continued to be introduced at a pressure of 0.2-0.8MPa. After 10-20 minutes, the Ar gas input is stopped, and the gate valve is opened to make the pressure in the pouring chamber reach atmospheric pressure before taking it out of the furnace to obtain a nickel-based single crystal high-temperature alloy with high organizational stability and high Re content.
Citation Information
Patent Citations
Re / Ru-containing monocrystal nickel-based superalloy with high temperature resistant capability and high creep resistance
CN104911407A
Third-generation nickle base monocrystal high temperature alloy with stable texture and preparation method
CN111455220A
Third-generation nickel-based single-crystal high-temperature alloy for strengthening gamma' phase and preparation method
CN111500896A
Third-generation nickel-based single-crystal high-temperature alloy and component design method and preparation method thereof
CN117037940A
Low-cost single-crystal high-temperature alloy with both structure stability and performance and preparation method
CN118389908A
Cited By
High-purity and high-stability nickel-based single crystal superalloy and preparation method thereof
CN122773181A
High-purity and high-stability nickel-based single crystal superalloy and preparation method thereof
CN122773181B