Electrode and method of manufacture

By airflow grinding and classifying the H-Nb2O5 material, its particle size distribution is optimized, which solves the problem of poor electronic conductivity and capacity fading of niobium oxide in lithium-ion batteries, and achieves good battery performance at high rates.

CN118743048APending Publication Date: 2024-10-01ECHION TECH LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202380022525.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-23
Filing Date
2023-02-23
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The application of niobium oxide in lithium-ion batteries is limited by its poor electronic conductivity and capacity fading problems caused by pulverization during charge and discharge, and existing nanoscale or particle-scale engineering methods increase manufacturing complexity.

Method used

The H-Nb2O5 material is processed by airflow grinding and classification to control its particle size distribution to a D50 particle size of 2.2-15 μm and a particle size distribution span of <1.90 to form an active electrode material with optimized performance.

Benefits of technology

The capacity of H-Nb2O5 as an active electrode material is significantly improved, and it can maintain good performance even at high rates, making it suitable for high-power batteries with rapid charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004999015770000141
    Figure BDA0004999015770000141
  • Figure BDA0004999015770000171
    Figure BDA0004999015770000171
  • Figure FDA0004999015750000031
    Figure FDA0004999015750000031
Patent Text Reader

Abstract

The present invention relates to a method of manufacturing an electrode, the method comprising: providing a starting H-Nb2O5 material; subjecting the starting material to airflow milling and classification to provide a processed H-Nb2O5 material, the material having a D50 particle size and lt of 2.2 to 15 [mu] m; 1.90, a particle size distribution span (D90-D10) / D50; and forming an electrode, wherein the electrode comprises the processed H-Nb2O5 material as an active electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to electrodes comprising niobium oxide and methods for their manufacture. Such electrodes are of interest for use in metal ion batteries, such as lithium ion or sodium ion batteries, preferably as anodes in lithium ion batteries. Background Art

[0002] Lithium-ion (Li-ion) batteries are a commonly used type of rechargeable battery, and their global market is expected to grow to $200 billion by 2030. Li-ion batteries are the technology of choice for electric vehicles with multiple requirements from technical performance to environmental impact, thus providing a viable path for a green automotive industry.

[0003] A typical lithium-ion battery consists of multiple battery cells connected in series or in parallel. Each individual battery cell is usually composed of an anode (negative electrode) and a cathode (positive electrode), separated by a porous electrically insulating membrane (called a separator) and immersed in a liquid (called an electrolyte) capable of transporting lithium ions. In most systems, the electrode consists of an active electrode material - meaning that it is able to chemically react with lithium ions, thereby reversibly storing and releasing the lithium ions in a controlled manner - mixed with conductive additives (such as carbon) and polymer binders as necessary. A slurry of these components is applied in the form of a thin film on a current collector (usually a thin foil of copper or aluminum), thereby forming an electrode after drying.

[0004] In conventional Li-ion battery technology, the safety limitations of graphite anodes during battery charging have severely hampered their use in high-power electronics, automotive, and industrial applications. Various polymorphs of niobium oxides have previously been shown to be useful as lithium-ion battery materials. In 1981, Reichman and Bard (B. Reichman and AJ Bard, "The Application of Nb2O5 as a Cathode in Nonaqueous Lithium Cells", J. Electrochem. Soc., 128, 344, 1981) first demonstrated the electrochemical performance of niobium oxides as positive electrode materials in lithium-ion battery cells. Later in 1983, Cava et al. (RJ Cava, DW Murphy and SM Zahurak, "Lithium Insertion in Wadsley-Roth Phases Based on Niobium Oxide," J. Electrochem. Soc., Vol. 130, No. 12, pp. 2345-2351, 1983) studied the Wadsley-Roth phase of lithium insertion in niobium oxide. In 1994, Koshiba et al. (N. Koshiba, K. Takata, M. Nakanishi and Z. Takehara, "Evaluation of crystalline Nb2O5 as an anode of rechargeable lithium cell," Denki Kagaku, Vol. 62, No. 7, pp. 593-601, 1994) studied different niobium oxide polymorphs obtained by calcining niobium chloride at different temperatures as anode materials for lithium ion batteries. Recently, Griffith et al. (KJGriffith, ACForse, JM Griffin and CPGrey, "High-Rate Intercalation without Nanostructuring in Metastable Nb2O5 BronzePhases," J.Am.Chem.Soc., Vol. 138, No. 28, pp. 8888-8899, 2016) studied various micron-sized niobium oxide polymorphs synthesized by heating NbO2 as anode materials and found that the capacity and rate performance of the low-temperature bronze phase TT and T polymorphs are inherent properties of the bulk crystal structure.Li et al. (“A Niobium Oxide with Shear Structure and Planar Defects for High-Power Lithium Ion Batteries,” Energy Environ. Sci., 2021) prepared micron-sized H-Nb2O5 with abundant Wadsley plane defects for rapid lithium storage by adjusting the calcination temperature. They further tested the effect of particle size on the performance of well-crystallized H-Nb2O5 battery cells, and obtained smaller particle sizes by roller milling. The battery cell results showed that there was little improvement with reduced particle size. In WO2021 / 245411, niobium oxide has the general formula M1. a M2 1-a M3 b Nb 12-b O 33-c-d Q d EP0402687B1 relates to a niobium oxide powder having a T phase of >90%, a fluorine value of <1000ppm, >99.9% by weight passing through a 45μm sieve, and a BET surface area of ​​greater than 3.5m 2 / g, suitable for ceramic capacitors.

[0005] In summary, while niobium oxides do have some promising properties, they are said to have intrinsically poor electronic conductivity and suffer from capacity decay during charge and discharge due to pulverization, which limits their practical application in lithium-ion batteries. Specifically, the Wadsley-Roth H-Nb2O5 polymorph exhibits the highest specific capacity but the lowest capacity retention at high charge / discharge rates due to increased impedance (see polarization) effects. On the other hand, the low-temperature bronze-type polymorphs T-Nb2O5 and TT-Nb2O5 exhibit higher capacity retention at high charge / discharge rates, but their specific capacities are lower. As the reduced form of niobium oxides (such as NbO2) increases, the conductivity is greatly improved when the material becomes a semiconductor material, but its ability to intercalate lithium ions is lost because the material no longer has the Wadsley-Roth or bronze crystal structure type that is considered favorable. Typical approaches to address these issues rely on extensive nanoscale or particle-scale engineering, which increases the complexity of manufacturing. Therefore, there is still a need for more effective methods to optimize niobium oxides for use as active electrode materials. Summary of the invention

[0006] In a first aspect, the present invention provides a method for manufacturing an electrode, the method comprising: providing a starting H-Nb2O5 material; jet milling and classifying the starting material to provide a processed H-Nb2O5 material having a D of 2.2-15 μm;50 Particle size and particle size distribution span (D 90 -D 10 ) / D 50 ; and forming an electrode, the electrode comprising the processed H-Nb2O5 material as an active electrode material.

[0007] It has been found that processing H-Nb2O5 using airflow milling and classification to achieve specific particle size parameters provides surprising improvements when compared to using other milling methods and other particle size parameters. For example, as shown in the examples of the present invention, controlling the milling method and the particle size distribution of the processed H-Nb2O5 material has been shown to increase the capacity of H-Nb2O5 as an active electrode material, even when delithiated at high rates such as 5C and 10C. These are important results that demonstrate the advantages of the present invention in providing electrodes for use in high power batteries designed for rapid charge / discharge.

[0008] In a second aspect, the present invention provides a method of manufacturing an electrochemical cell, the method comprising manufacturing an electrode according to the method of the first aspect, and forming an electrochemical cell comprising the electrode. Preferably, the electrode forms an anode of the electrochemical cell. Preferably, the electrochemical cell is a metal ion battery, such as a lithium ion or sodium ion battery, most preferably a lithium ion battery.

[0009] The invention provides electrodes and electrochemical cells obtainable from the first and second aspects. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 . Particle size distribution of Examples 1-6

[0011] Figure 2 XRD of Examples 1-6

[0012] Figure 3 SEM images of the powders of Examples 1, 2, 5 and 6

[0013] Figure 4 : SEM images of electrodes obtained using the powders of Examples 1, 2 and 6

[0014] Figure 5 . Particle size distribution of Examples 7-9

[0015] Figure 6 SEM of the powders of Examples 7-9

[0016] Figure 7 SEM images of electrodes obtained using the powders of Examples 7-9

[0017] Figure 8 : XRD of Examples 7-9 DETAILED DESCRIPTION

[0018] The starting material used in the process is H-Nb2O5, which is a polymorph of Nb2O5 having a Wadsley-Roth crystal structure. The Wadsley-Roth crystal structure is considered to be a crystallographically non-stoichiometric MO3(ReO3) crystal structure containing a crystallographic shear, and the simplified formula is MO 3-x Therefore, these structures usually contain [MO6] octahedral subunits and other subunits in their crystal structure. The H-Nb2O5 crystal structure has an array of octahedral units arranged in a block structure with (3×4)1 and (3×5) ∞ A combination of both ReO3-like blocks. These blocks are infinitely parallel to b, and the subscripts 1 and ∞ represent block connectivity in the ac plane. Further information on the crystal structure of Nb2O5 can be found in Griffith et al., J.Am.Chem.Soc.2016, 138, 28, 8888-8899. It is well known that the crystal structure of a material can be determined by analyzing X-ray diffraction (XRD) patterns. For example, an XRD pattern obtained from a given material can be compared with a known XRD pattern to confirm the crystal structure, for example via a public database such as the ICDD crystallographic database. Rietveld analysis and Pawley analysis can also be used to determine the crystal structure of a material, particularly with respect to unit cell parameters. The crystal structure of H-Nb2O5 can be found in the ICDD crystallographic database entry JCPDS 37-1468.

[0019] The starting H-Nb2O5 material may have a phase purity of >80 wt% H-Nb2O5, >90 wt% H-Nb2O5, or >95 wt% or about 100 wt% H-Nb2O5. Phase purity refers to the proportion of Nb2O5 adopting the H-Nb2O5 crystal structure relative to Nb2O5 of other crystal structures. Phase purity can be determined by X-ray diffraction. The starting H-Nb2O5 material may be substantially pure H-Nb2O5, for example it may contain unavoidable impurities resulting from the manufacturing process. The starting H-Nb2O5 material may be doped with additional cations and / or anions, provided that the crystal structure corresponds to the H-Nb2O5 crystal structure. The term 'corresponding' may be understood to mean that the peaks in the X-ray diffraction pattern may be offset by no more than 0.5 degrees (preferably no more than 0.25 degrees, more preferably no more than 0.1 degrees) from the corresponding peaks in the reference X-ray diffraction pattern.

[0020] The starting H-Nb2O5 material can be obtained from a commercial supplier. Alternatively, the starting H-Nb2O5 material can be prepared by annealing a niobium oxide precursor (e.g., NbO2, other polymorphs of Nb2O5, Nb2O5 hydrate) at above 900°C (e.g., 1100-1300°C) in air. The formation of H-Nb2O5 can then be confirmed by XRD. The annealing time can be at least 30 minutes, or at least 1 hour. The starting material is typically obtained with a relatively large particle size that is not suitable for use as an active electrode material. For example, the starting H-Nb2O5 material can have a D of >20 μm, 25-150 μm, or 30-100 μm. 50 Particle size.

[0021] The term "particle size" refers to the equivalent spherical diameter (esd), which is the diameter of a sphere having the same volume as a given particle, wherein the particle volume is understood to include the volume of any intraparticle pores. n ” and “D n The term "D" refers to the diameter below which n% of the volume of the particle population exists. 50 ” and “D 50 "Particle size" refers to the volume-based median particle size below which 50% of the volume of the particle population exists. In the case where the material comprises primary crystallites agglomerated into secondary particles, it is understood that the particle size refers to the diameter of the secondary particles. The particle size can be determined by laser diffraction. The particle size can be determined according to ISO 13320:2009, for example using Mie theory.

[0022] The starting H-Nb2O5 material typically has a relatively low surface area. For example, the starting material may have a surface area of ​​<0.8 m 2 / g or <0.6m 2 The term "BET surface area" refers to the surface area per unit mass calculated by measuring the physical adsorption of gas molecules on a solid surface using the Brunauer-Emmett-Teller theory. For example, the BET surface area can be determined according to ISO 9277:2010.

[0023] The starting H-Nb2O5 material is subjected to jet milling and classification. Jet milling is a powder comminution technique in which the powder material is accelerated by high-pressure gas or steam and causes inter-particle collisions to reduce the particle size. Two common designs are spiral jet mills and fluidized bed jet mills. Spiral jet mills typically have a cylindrical grinding chamber in which multiple gas nozzles are present in a tangential direction. The selection of particle size is based on the aerodynamic properties of the particles and the spiral design, so that the fineness can be well controlled. Fluidized bed jet mills typically have a grinding chamber in which gas nozzles are radially arranged on the chamber wall and form a fluidized bed. Jet milling may include fluidized bed jet milling. Jet milling can be achieved without using spiral jet milling (for example, it can consist of fluidized bed jet milling).

[0024] Classification is usually achieved by air classification, for example using a centrifugal forced vortex air classifier. By controlling process parameters such as centrifugal force and suction to filter powder of a specific particle size, the desired particle size distribution can be achieved.

[0025] Other common powder comminution methods are impact milling and high shear milling. In impact milling, the powder material is milled by mechanical impact with a high-speed component, which can be gravitational energy (hammer mill) or kinetic energy (high-speed rotor / stator / pin, etc.). High shear milling consists of a rotating container or rotor, so the grinding assembly and powder material interact with shear forces to reduce particle size.

[0026] Unlike other powder comminution methods, the jet milled and classified material can be identified by SEM. Specifically, the SEM image of the material that has been jet milled and classified to the particle size parameters defined herein will be uniform, without very fine particles, and without larger particles that might be expected in the SEM images of materials pulverized by other methods. Electrodes containing the processed H-Nb2O5 material can be identified as having a uniform surface, without large cavities and large particles.

[0027] D of processed H-Nb2O5 material 50 The particle size is 2.2-15 μm; or optionally 2.5-12 μm, 3.0-10 μm or 4.0-8.0 μm.

[0028] The particle size distribution span (D 90 -D 10 ) / D 50 is <1.90; or optionally is <1.80, <1.60 or <1.50. For example, the particle size distribution span (D 90 -D 10 ) / D 50 Can be in the range of >0.2 to <1.90 or >0.5 to <1.50.

[0029] For materials processed by air jet grinding and classification, it has been found that D 50 The combination of particle size and span can improve the performance of H-Nb2O5 materials used as active electrode materials. For example, as shown in this example, the capacity is significantly improved at high delithiation rates, such as 5C and 10C, compared to alternative particle size parameters and grinding methods. In theory, the particle size and distribution of active electrode materials directly affect the performance of lithium-ion battery cells in the following aspects: 1) Conductivity. Active electrode materials with larger particle size and wide distribution lead to uneven electrodes and poor processing performance on an industrial scale through, for example, roll-to-roll coating processes, which in turn leads to poor electronic conductivity of the electrodes and unstable performance. In addition, larger particle sizes have longer lithium ion diffusion paths, thereby reducing the performance of the battery cell at high rates. 2) Side reactions. Active electrode materials with small particle sizes correspond to high specific surface areas and undergo more adverse side reactions with the electrolyte, resulting in material degradation and shortened cycle life. The inventors have found that a specified D 50 Particle size and particle size distribution span provide the best balance of these factors for H-Nb2O5. In addition, it has been found that the use of airflow grinding and classification is a particularly advantageous way to achieve these parameters. Conventional powder material size reduction techniques include impact grinding and high shear grinding. However, these two types of grinding are prone to contamination due to direct contact between the powder and the grinding media, and the particle size distribution control is poor at particle sizes <20μm. Airflow grinding and classification avoid these problems, and by controlling processing parameters (such as centrifugal force and suction), the desired particle size parameters can be easily obtained. Therefore, it has been found that when the combination of particle size parameters is achieved by airflow grinding and classification, the performance of H-Nb2O5 as an active electrode material can be unexpectedly improved.

[0030] Another definition of the particle size distribution span is (D 95 -D5) / D 50 The particle size distribution span of processed H-Nb2O5 materials (D 95 -D5) / D 50 It can be <2.50, <2.25 or <2.0. For example, the particle size distribution span (D 95 -D5) / D 50 Can be in the range of >0.3 to <2.50 or >0.6 to <2.0.

[0031] D of processed H-Nb2O5 material 10 The particle size is >0.7μm, 1.0-8.0μm or 1.5-4.0μm. 90 The particle size may be <30 μm, 4.5-20 μm or 5.5-15 μm. The processed H-Nb2O5 material may have a particle size of >0.7 μm. 2 / g, or 1-20m 2 / g, or 0.8-2.50m 2 / g of BET surface area.

[0032] It is preferred to maintain the H-Nb2O5 crystal structure after airflow milling and classification. Therefore, the starting H-Nb2O5 material may have a phase purity of >80wt% H-Nb2O5, >90wt% H-Nb2O5, or >95wt% or about 100wt% H-Nb2O5. The processed H-Nb2O5 material may be substantially pure H-Nb2O5. The relative intensities of the characteristic peaks of the H-Nb2O5 crystal structure may change somewhat after airflow milling and classification, which may be due to the introduction of defects into the crystal structure during the milling process. The intensity ratio of the peak at about 23.7°2θ to the peak at about 24.4°2θ in the XRD pattern of the processed H-Nb2O5 material may be in the range of 0.7-1.3 or 0.8-1.2.

[0033] The processed H-Nb2O5 material forms an electrode so that the processed H-Nb2O5 material is an active electrode material. An active electrode material may be understood as a material that is capable of chemically reacting with lithium ions to reversibly store and release lithium ions in a controlled manner. The electrode is typically in the form of an electrode composition that is in electrical contact with a current collector. The current collector is typically a metal foil, such as copper or aluminum foil. The electrode may be made by forming a slurry of the processed H-Nb2O5 material and a solvent. The slurry may contain at least one other component selected from a binder, a conductive additive, a different active electrode material, and a mixture thereof. The slurry may be deposited onto the current collector and the solvent removed to form an electrode composition on the current collector. Further steps may be implemented as appropriate, such as heat treatment for curing any binder and / or calendering of the electrode layer. For example, the solvent may be removed by, for example, drying at a temperature of 30-100°C. The electrode may be calendered to 2-3.5 or 2.3-2.9 gcm- 3 The electrode composition may form a layer having a thickness in the range of 5 μm to 2 mm, preferably 5 μm to 1 mm, preferably 5 μm to 500 μm, preferably 5 μm to 200 μm, preferably 5 μm to 100 μm, preferably 5 μm to 50 μm.

[0034] Alternatively, the slurry can be formed into a self-supporting film or mat containing the active electrode material, for example by casting the slurry onto a suitable casting template, removing the solvent, and then removing the casting template. The resulting film or mat is in the form of a cohesive, self-supporting mass that can then be bonded to a current collector by known methods.

[0035] Optionally, the processed H-Nb2O5 material forms at least 10 wt%, 50 wt% or 75 wt% of the total active electrode material in the electrode. The processed H-Nb2O5 material may form the only active anode material in the electrode.

[0036] The electrode composition may further comprise at least one other component selected from the group consisting of a binder, a conductive additive, a different active electrode material, and mixtures thereof. For example, based on the total dry weight of the anode composition, an electrode composition comprises about 92 wt % of processed H-Nb2O5 material, about 5 wt % of a conductive additive (e.g., carbon black), and about 3 wt % of a binder (e.g., poly(vinylidene fluoride)).

[0037] Examples of suitable binders include polyvinylidene fluoride and its copolymers (PVDF), polytetrafluoroethylene (PTFE) and its copolymers, polyacrylonitrile (PAN), poly(methyl)methacrylate or poly(butyl)methacrylate, polyvinyl chloride (PVC), polyvinyl formal, polyetheramide, polymethacrylic acid, polyacrylamide, polyitaconic acid, polystyrene sulfonic acid, polyacrylic acid (PAA) and its alkali metal salts, modified polyacrylic acid (mPAA) and its alkali metal salts, cellulose-based polymers, carboxymethyl cellulose (CMC), modified carboxymethyl cellulose (mCMC), sodium carboxymethyl cellulose (Na-CMC), polyvinyl alcohol (PVA), alginates and their alkali metal salts, nitrile rubber (NBR), hydrogenated forms of NBR (HNBR), styrene-butadiene rubber (SBR) and polyimide. The binder may be present in the electrode composition in an amount of 0-30% by weight, or 0.1-10% by weight, or 0.1-5% by weight based on the total dry weight of the electrode composition.

[0038] Conductive additives are preferably inactive materials, which are included to improve the conductivity between active electrode materials and between active electrode materials and current collectors. Conductive additives can be appropriately selected from graphite, carbon black, carbon fiber, vapor grown carbon fiber (VGCF), carbon nanotubes, graphene, acetylene black, ketjen black, metal fibers, metal powders and conductive metal oxides. Preferred conductive additives include carbon black and carbon nanotubes. Based on the total dry weight of the electrode composition, the conductive additive can be present in the electrode composition at 0-20 weight %, 0.1-10 weight % or 0.1-5 weight %.

[0039] The processed H-Nb2O5 material may be present in the electrode composition at 100-50 wt%, 99.8-80 wt%, or 99.8-90 wt%, based on the total dry weight of the electrode composition. When the active electrode material is present at 100 wt% of the electrode composition, the active electrode material may form a solid-state electrode.

[0040] When a different active anode material is present in addition to the processed H-Nb2O5 material, it may be selected from lithium titanium oxide, titanium niobium oxide, oxides comprising niobium and at least one other cation, graphite, hard carbon, soft carbon, silicon, doped forms thereof and mixtures thereof.

[0041] The processed H-Nb2O5 material may be further processed after jet milling and classification and before forming an electrode. For example, the processed H-Nb2O5 material may be coated with carbon, for example to improve its surface electronic conductivity and / or prevent reaction with the electrolyte. The processed H-Nb2O5 material may be coated with aluminum oxide, zirconium oxide, oxides comprising niobium and at least one other cation, organic or inorganic fluorides, organic or inorganic phosphates, titanium oxides, lithiated forms thereof, and mixtures thereof.

[0042] The present invention includes the method of the first aspect, but omits the step of forming an electrode comprising a processed H-Nb2O5 material as an active electrode material. For example, the present invention includes a method of making an active electrode material, the method comprising: providing a starting H-Nb2O5 material; and jet milling and classifying the starting material to provide a processed H-Nb2O5 material having a D of 2.2-15 μm. 50 Particle size and particle size distribution span (D 90 -D 10 ) / D 50 The processed H-Nb2O5 material can then be used as an active electrode material when forming an electrode. The present invention also includes the processed H-Nb2O5 material obtained by this method.

[0043] The electrodes may be incorporated into an electrochemical cell. Preferably, the electrochemical cell comprises an electrode as an anode, a cathode and an electrolyte disposed between the anode and the cathode. The electrochemical cell is preferably a metal ion battery, such as a lithium ion battery or a sodium ion battery, most preferably a lithium ion battery.

[0044] Electrochemical cells may be configured to have an N / P ratio > 1, where N / P is defined as:

[0045]

[0046] Area loading (mgcm -2 ) is the dry loading of the electrode composition without considering the current collector.

[0047] The active fraction (wt %) is the percentage of the dry electrode composition that is active material.

[0048] First lithiation / delithiation capacity (mAhg -1) is the specific capacity at C / 10 at 25°C for the first lithiation cycle of the anode or the first delithiation cycle of the cathode measured on an equivalent half-cell with a lithium metal counter electrode. An equivalent half-cell may be understood as utilizing the same electrode composition deposited at the same areal loading and activity fraction as a full cell.

[0049] The charge rate of a battery cell is usually expressed as a "C-rate". A 1C charge rate means the charge current that fully charges the battery cell in 1 hour, and a 10C charge means the battery is fully charged in 1 / 10 of an hour (6 minutes). The C-rate can be defined based on the reversible capacity of the battery cell within the appropriate voltage limit, for example, for a battery cell that exhibits 1.0 mAh cm in the voltage range of 1.2-3.15 V, the ... -2 Capacity of the battery cell, 1C-rate corresponds to an applied 1.0 mA cm -2 of current density.

[0050] The first lithiation / delithiation capacity was measured on an equivalent half-cell. For the anode, the first constant current C / 10 lithiation (discharge, negative current) capacity (relative to Li / Li+) at 25°C was measured. For the cathode, the first constant current C / 10 delithiation (charge, positive current) capacity (relative to Li / Li+) at 25°C was measured.

[0051] N / P may be >1-2, or 1.01-1.5, or preferably 1.05-1.3. Alternatively, N / P may be ≤1, or <1, ​​such as 0.7-0.95.

[0052] The cathode comprises an active cathode material, which may be selected from LiNi 1-x M x Nickel-based layered oxides of the O2 type (where M = Co, Mn, Al), such as NMC (lithium nickel manganese cobalt oxide), NCA (lithium cobalt aluminum oxide), and LCO (lithium cobalt oxide); and LNMO (lithium nickel manganese oxide) (e.g. LiNi 0.5 Mn 1.5 O4). Active cathode materials are widely available from commercial suppliers. The active cathode materials may be doped with additional cations and / or anions.

[0053] The choice of active electrode material may affect the appropriate voltage range, including for determining the first lithiation / delithiation capacity. For example, the appropriate voltage range may be LNMO: 5.2-3V, with an upper cutoff of 5.2V; NCA, NMC and LCO: 4.5-2.7V, with an upper cutoff of 4.5V; processed H-Nb2O5 materials: 3-0V, with a lower cutoff of 0V. A narrower range may be LNMO: 5-3V, with an upper cutoff of 5V; NCA, NMC and LCO: 4.3-2.7V, with an upper cutoff of 4.3V; processed H-Nb2O5 materials: 3V-1.0V, with a lower cutoff of 1.0V.

[0054] An appropriate voltage range may be determined empirically. For example, the voltage profile is related to changes in the energy state of the anode and cathode materials associated with the removal or insertion of electrons and ions. The cutoff voltage of the battery cell may be selected to fall before a specific inflection point in the voltage profile, corresponding to a rise in the energy state of one or both electrodes exceeding a critical level that causes the crystal structure to decay to a lower energy structure at a rate that is significantly detrimental to the performance of the battery cell. The absolute voltage at which this occurs is a function of the electrode potentials of the two electrodes, but can be calculated by using a common reference electrode and does not need to be determined experimentally for a well-established family of materials with reliable standard electrochemical behavior.

[0055] The cathode active material is preferably in particulate form, for example having a D in the range of 0.1-100 μm, or 0.5-50 μm, or 1-20 μm. 50 Particle size.

[0056] The electrolyte may include any material suitable for metal ion battery operation, preferably lithium ion battery operation. For example, the electrolyte may be a non-aqueous solution (e.g., an organic electrolytic solution). The electrolyte may include one or more non-aqueous solvents and a salt at least partially dissolved in the solvent. For example, the solvent may include an organic solvent such as ethylene carbonate (EC) and / or other carbonate-based solvents, or butyrates, or acetates, or mixtures thereof. The solvent may include 1M LiPF6 dissolved in an aprotic solvent mixture, such as a 1:1 mixture by weight of ethylene carbonate and other carbonate-based solvents or butyrates or acetates. Salts suitable for use in the present invention include LiPF6, LiSbF6, LiBF4, LiTFSI, LiFSI, LiAlCl4, LiAsF6, LiClO4, LiGaCl4, LiC(SO2CF3)3, LiN(CF3SO2)2, Li(CF3SO3), LiB(C6H4O2)2, LiBOB (lithium bis(oxalato)borate) and LiDFOB (lithium difluoro(oxalato)borate). Suitable low viscosity solvents (e.g., organic solvents) for the electrolyte may include, but are not limited to, ethyl methyl carbonate (EMC), dioxolane (DOL), ethyl acetate (EA); propylene acetate (PA); butyl acetate (BA); methyl butyrate (MB); ethyl butyrate (EB); dimethyl carbonate (DMC); diethyl carbonate (DEC); 1,2-dimethoxyethane (DME); tetrahydrofuran (THF); methyl acetate (MA); diethylene glycol dimethyl ether (DGL); triethylene glycol dimethyl ether; tetraethylene glycol dimethyl ether; cyclic carbonates; cyclic esters; cyclic amides; propylene carbonate (PC); methylpropyl carbonate (MPC); acetonitrile; dimethyl sulfoxide (DMS); dimethylformamide; dimethylacetamide; γ-butyrolactone (GBL); and N-methylpyrrolidone (NMP); and various mixtures or combinations thereof.

[0057] Example

[0058] Example 1 was obtained from a commercial supplier. It was ground to obtain Examples 2-9.

[0059] Examples 2, 3 and 7-9 were made by fluid bed jet milling with wheel classification (Alpine Fluid Bed Opposed Jet Mill AFG 100 for Examples 2 and 7-9 and AFG 200 for Example 3).

[0060] Example 2 was milled at 4.5 bar pressure with a 2.5 mm nozzle diameter. The classifier speed was set at 6000 rpm.

[0061] Example 3 was milled at 6 bar pressure with a 5 mm nozzle diameter. The classifier speed was set at 6000 rpm.

[0062] Example 4: Grinding by spiral airflow (MC 100). The venturi pressure was set to 9 bar and the ring pressure was set to 8 bar. This example was not classified.

[0063] Example 5 was prepared by rolling ball milling with zirconium oxide balls in a 5L PTFE jar. The ball diameters were 5 mm and 1 mm. The material to ball ratio was 10:1. The rolling speed was 400 rpm. The milling time for 5A was 4 hours, and the milling time for 5B was 12 hours.

[0064] Example 6 was made by impact milling using a continuous milling process (Retsch ZM200 impact mill). The milling speed was set at 18000 rpm.

[0065] Example 7 was milled at 5 bar pressure with a nozzle diameter of 2.5 mm. The classifier speed was set at 8000 rpm.

[0066] Example 8 was milled at 4 bar pressure with a nozzle diameter of 2.5 mm. The classifier speed was set at 10000 rpm.

[0067] Example 9 was milled at 4 bar pressure with a nozzle diameter of 2.5 mm. The classifier speed was set at 3000 rpm.

[0068] The particle size distribution of the samples was measured using a Horiba Partica LA-960 and a dry dispenser ( Figure 1 and Figure 5 and Table 1).

[0069] The surface area was measured by BET surface area analysis using N2 at 77.35 K on a BELSORP-miniX instrument (Table 2).

[0070] Table 1. Particle size

[0071]

[0072] *Compare

[0073] Table 2. Surface area

[0074] Example 1* Example 2 Example 4* Example 5A* <![CDATA[BET surface area (m 2 / g)]]> 0.57 1.23 2.24 1.39

[0075] Material characterization

[0076] The phase purity of the samples was analyzed using a Rigaku Miniflex powder X-ray diffractometer in the 2θ range (10°-70°) at a scanning rate of 1° / min. Figure 2 and Figure 8 and Table 3).

[0077] Example 1 was obtained as the starting H-Nb2O5 material with a phase purity of 100 wt% as determined by XRD. The XRD patterns of all ground samples (2-9) showed that the purity was maintained after grinding. Some differences in the relative intensities of the two characteristic peaks at about 23.7° and about 24.4° 2θ were observed, which may be due to the different degrees of defects introduced into the H-Nb2O5 crystal structure.

[0078] Table 3. Intensity ratio of the peak at about 23.7° to the peak at about 24.4°

[0079] Example Strength ratio 1* 1.13 2 0.86 3 1.18 4* 1.25 5* 0.82 6* 1.05 7 0.96 8* 0.96 9* 1.12

[0080] SEM results ( Figure 3 and Figure 6 ) shows that Example 1 has the most spherical particles and the largest particle size. The surface of these particles is composed of sintered primary particles. Example 2 shows particles with the most uniform particle size. All particles in the SEM are less than 15μm. Compared with Example 2, the particles in Example 5 show a much wider particle size distribution, with the largest particles being about 25μm and the smallest particles being less than 1μm. Example 6 shows the second largest particle size among the four examples imaged, with some particles being about 25μm and unground particles present. Example 7 shows particles of uniform particle size under SEM, with all particles being less than 12μm. Example 8 shows a wide distribution of particle sizes, with particles greater than 20μm and less than 10μm. Example 9 shows that most of the particles are large, with occasional particles less than 5μm. These results are consistent with the particle size distribution results obtained by laser diffraction shown in Table 1.

[0081] When the electrode is made ( Figure 4 and Figure 7 ), powders with large particle sizes cannot provide uniform electrode surfaces. Excessive polymer binders and large cavities (e.g., Example 1) exist on the electrode surface, thereby impairing conductivity, or large particles make the surface uneven (e.g., Example 6), thereby impairing the life of the battery cell. The electrodes prepared by Examples 8 and 9 showed uneven surfaces with large cavities. In contrast, the electrode surfaces of Examples 2 and 7 were uniform and free of large particles.

[0082] Electrochemical characterization

[0083] The charging rate of a Li-ion battery cell is usually expressed as a "C-rate". A 1C charging rate means the charging current that fully charges the battery cell in 1 hour, and a 10C charge means that the battery is fully charged in 1 / 10 of an hour (6 minutes). The C-rate here is defined based on the reversible capacity of the anode observed within the voltage limit applied in its second cycle delithiation, that is, within the voltage limit of 1.1-3.0V, the anode exhibits 1.0mAh cm -2 Capacity, 1C rate corresponds to an applied 1.0 mA cm -2 In typical materials as described herein, this corresponds to about 215 mA / g active material.

[0084] Electrochemical tests were performed in a semi-button cell (CR2032 size) for analysis. In the semi-button cell test, the active material was tested in an electrode relative to a Li metal electrode to evaluate its basic performance. In the following examples, the active material composition to be tested was combined with N-methylpyrrolidone (NMP), carbon black (SuperP) acting as a conductive additive, and poly(vinylidene fluoride) (PVDF) binder, and mixed using a laboratory-scale centrifugal planetary mixer to form a slurry. The non-NMP composition of the slurry was 92 wt% active material, 5 wt% conductive additive, 3 wt% binder. The slurry was coated on an Al foil current collector by blade coating until 69-75 g m -2 The electrode was then calendered to a loading of 2.5–2.7 g cm at 80 °C. -3 density to achieve a target porosity of 32-37%. The electrodes were punched into the desired size and combined with a separator (Celgard porous polypropylene / polyethylene), Li metal and electrolyte (1.3M LiPF6 in ethyl carbonate / diethyl carbonate) in a steel button cell housing and sealed under pressure. The cells were then cycled between 1.1-3.0V at a low current rate (C / 10) at 23°C to achieve 2 full cycles of lithiation and delithiation. After this, the performance of the cells was tested at increasing current densities. During these tests, the cells were cycled asymmetric at 23°C with slow lithiation (C / 5) followed by increasing delithiation rates (e.g., 1C, 5C, 10C) to probe capacity retention at high rates.

[0085] The data of 3-5 battery cells prepared from the same electrode coating were averaged and the error is represented by the standard deviation. Therefore, these data represent a reliable study that shows that the materials according to the present invention achieve improvements compared to previous materials. These data are shown in Table 4a and Table 4b. The first cycle coulombic efficiency is defined as the percentage of the capacity of the first lithiation step returned in the first delithiation step, and the formed capacity is defined as the capacity of the second delithiation step.

[0086] Table 4a. Electrochemical data of Examples 1-6

[0087]

[0088] Table 4b. Electrochemical data of Examples 7-9

[0089] (mAh / g) Example 7 Example 8* Example 9* Cycle 1 CE 96.8(0.3)% 98.4(3.5)% 97.9(2.2)% Formation capacity 215.8(3.9) 217.2(2.1) 216.5(3.9) 0.5C 206.3(1.6) 202.6(2.6) 201.6(3.6) 1C 200.9(1.6) 194.7(2.4) 195.0(3.7) 2C 198.1(1.6) 188.9(2.2) 190.5(3.8) 5C 195.2(1.7) 181.6(1.9) 184.0(3.6) 10C 191.2(1.24) 165.9(16.0) 174.1(2.7)

[0090] discuss

[0091] Compared to the starting material of Example 1, Examples 2, 3 and 7, which were jet milled and classified according to the present invention, were found to provide improved capacity at all delithiation rates when incorporated into electrodes. Notably, compared to Example 4 (jet milled but not classified, and therefore having a higher particle size distribution span), Examples 5A and 5B (tumbling ball milling), Example 6 (impact milling), Example 8 (jet milled and classified, but having a higher particle size distribution span) and Example 9 (jet milled and classified, but having a higher D 50 Compared to the niobium oxide active electrode materials with different particle sizes, Examples 2, 3 and 7 provide improved capacity at all delithiation rates. The improvement provided by the present invention is particularly evident at a high delithiation rate of 10C, an important result that demonstrates the utility of the present invention in providing niobium oxide active electrode materials for high power applications.

Claims

1. A method for manufacturing an electrode, the method comprising: Providing a starting H-Nb2O5 material; The starting material is jet milled and classified to provide a processed H-Nb2O5 material having a D of 2.2-15 μm. 50 Particle size and particle size distribution span (D 90 -D 10 ) / D 50 ; as well as An electrode is formed comprising the processed H-Nb2O5 material as an active electrode material.

2. The method of claim 1, wherein the processed H—Nb2O5 material has a particle size distribution span (D Span) of <2.50, <2.25 or <2.

0. 95 -D5) / D 50 .

3. A method as claimed in any one of the preceding claims, wherein the processed H-Nb2O5 material has a particle size distribution span (D Span) of <1.80, <1.60 or <1.

50. 90 -D 10 ) / D 50 .

4. The method of any one of the preceding claims, wherein the processed H-Nb2O5 material has a D of 2.5-12 μm, 3.0-10 μm or 4.0-8.0 μm. 50 Particle size.

5. The method of any one of the preceding claims, wherein the processed H-Nb2O5 material has a D>0.7 μm, 1.0-8.0 μm or 1.5-4.0 μm. 10 Particle size.

6. A method as claimed in any one of the preceding claims, wherein the processed H-Nb2O5 material has a D<30 μm, 4.5-20 μm or 5.5-15 μm. 90 Particle size.

7. A method as claimed in any one of the preceding claims, wherein the processed H-Nb2O5 material has a molecular weight of >0.7 m 2 / g, or 1-20m 2 / g, or 0.8-2.50m 2 / g of BET surface area.

8. A method as claimed in any one of the preceding claims, wherein the starting H-Nb2O5 material has a D of >20 μm, 25-150 μm or 30-100 μm. 50 Particle size.

9. The method of any of the preceding claims, wherein the starting H-Nb2O5 material has a phase purity of >80 wt% H-Nb2O5, >90 wt% H-Nb2O5, or is substantially pure H-Nb2O5.

10. The method of any one of the preceding claims, wherein the intensity ratio of the peak at about 23.7° 2θ to the peak at about 24.4° 2θ in the XRD pattern of the processed H—Nb2O5 material is in the range of 0.7-1.3 or 0.8-1.

2.

11. The method according to any one of the preceding claims, wherein the jet milling comprises, comprises or consists of fluidized bed jet milling or spiral jet milling.

12. A method as claimed in any preceding claim, wherein the classifying is achieved by a centrifugal forced vortex air classifier.

13. The method of any of the preceding claims, wherein forming the electrode comprises forming a slurry of the processed H-Nb2O5 material in a solvent, depositing the slurry on a current collector, and removing the solvent.

14. The method of claim 13, wherein the slurry comprises at least one additional component selected from the group consisting of a binder, a conductive additive, a different active electrode material, and mixtures thereof.

15. A method as claimed in any preceding claim, wherein the processed H-Nb2O5 material is coated with carbon prior to forming the electrode.

16. A method as claimed in any one of the preceding claims, wherein the processed H-Nb2O5 material forms at least 10 wt%, 50 wt% or 75 wt% of the total active electrode material in the electrode.

17. A method as claimed in any preceding claim, wherein the processed H-Nb2O5 material is the only active electrode material in the electrode.

18. The method of any preceding claim, further comprising forming an electrochemical cell comprising the electrode.

19. The method of claim 18, wherein the electrochemical cell comprises the electrode as an anode, a cathode, and an electrolyte disposed between the anode and the cathode.

20. The method of claim 19, wherein the electrochemical cell is configured to have an N / P ratio > 1, wherein N / P is defined as: in: Area loading (mgcm -2 ) is the dry loading of the electrode composition, ignoring the current collector; Active fraction (wt %) is the percentage of the dry electrode composition that is active material; First lithiation / delithiation capacity (mAhg -1 ) is the specific capacity at C / 10 at 25°C for the first lithiation cycle of the anode or the first delithiation cycle of the cathode measured on an equivalent half-cell with a lithium metal counter electrode.

21. The method of claim 19, wherein the electrochemical cell is configured to have an N / P ratio of ≤ 1, wherein N / P is defined as: in: Area loading (mgcm -2 ) is the dry loading of the electrode composition, ignoring the current collector; Active fraction (wt %) is the percentage of the dry electrode composition that is active material; First lithiation / delithiation capacity (mAhg -1 ) is the specific capacity at C / 10 at 25°C for the first lithiation cycle of the anode or the first delithiation cycle of the cathode measured on an equivalent half-cell with a lithium metal counter electrode.

22. The method of any one of claims 18-21, wherein the electrochemical cell is a metal ion battery, such as a lithium ion battery or a sodium ion battery, or wherein the electrochemical cell is a lithium ion battery.

23. An electrode obtainable by the method according to any one of claims 1 to 17.

24. An electrochemical cell obtainable by the method according to any one of claims 18 to 22.

Citation Information

Cited By

  • Battery cell, battery device, and electric device

    CN119153758A

  • Battery cell, battery device, and electric device