Positive electrode material, electrochemical device, and electronic device

By introducing nitrate ions and chloride ions into the cathode material of lithium-ion batteries, the solvation structure and film-forming effect of the electrolyte are controlled, which solves the problems of cracks and expansion during the cycle of the cathode material and improves the Coulombic efficiency and cycle performance of the battery.

CN118743053APending Publication Date: 2024-10-01DONGGUAN AMPEREX TECH
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202380021032.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-10-20
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode materials are prone to cracks during cycling, leading to problems such as cycle life decay and gas expansion, affecting the performance of electrochemical devices.

Method used

Introduce nitrate ions and chloride ions into the cathode material to regulate the solvation structure and film-forming effect of the electrolyte to form a thinner and denser interface film, improve the first Coulombic efficiency and high-temperature cycle performance of the electrochemical device, and reduce thickness expansion Rate.

Benefits of technology

By introducing nitrate ions and chloride ions, the first Coulombic efficiency and high-temperature cycle performance of lithium-ion batteries are significantly improved, the thickness expansion rate is reduced, the cycle life of the battery is extended, and the structural stability is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743053A_ABST
    Figure CN118743053A_ABST
Patent Text Reader

Abstract

The invention provides a positive electrode material which comprises nitrate ions and chloride ions, and based on the mass of the positive electrode material, the mass percentage content of the nitrate ions is 0.01%-0.2%, and the mass percentage content of the chloride ions is 0.05%-1.0%. The invention also provides an electrochemical device and an electronic device comprising the positive electrode material. The positive electrode material can improve the cycling stability, the first-circle coulombic efficiency and the high-temperature storage performance of an electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage technology, and in particular to positive electrode materials and electrochemical devices and electronic devices comprising the positive electrode materials. Background Art

[0002] As people pay more and more attention to the demand for clean energy, lithium-ion batteries play an extremely important role in it. As one of the key factors affecting the performance of lithium-ion batteries, the research on lithium-ion battery positive electrode materials has always attracted much attention.

[0003] However, the lithium-ion positive electrode materials that have been commercialized are prone to cracking during the cycle process, leading to problems such as cycle life degradation and gas production expansion. Summary of the invention

[0004] Based on the defects of the prior art, the present application introduces nitrate ions and chloride ions into the positive electrode material to improve the first coulombic efficiency and high-temperature cycle performance of the electrochemical device and reduce the thickness expansion rate.

[0005] In a first aspect, the present application provides a positive electrode material, which comprises nitrate ions and chloride ions, wherein, based on the mass of the positive electrode material, the mass percentage of nitrate ions is 0.01% to 0.2%, and the mass percentage of chloride ions is 0.05% to 1.0%. The nitrate ions and chloride ions in the present application can work together to regulate the electrolyte solvation structure and film-forming effect, so that a thinner, denser and more stable interface film is formed on the positive electrode surface and the negative electrode surface, respectively, thereby improving the first coulomb efficiency and high temperature cycle performance of the electrochemical device, and reducing the thickness expansion rate.

[0006] In some embodiments, based on the mass of the positive electrode material, the mass percentage of nitrate ions is 0.015% to 0.1%, and the mass percentage of chloride ions is 0.25% to 0.5%. Meeting the above ranges can enable the electrochemical device to obtain better first coulombic efficiency, high temperature cycle performance and thickness expansion rate.

[0007] In some embodiments, the ratio of the mass percentage of chloride ions to the mass percentage of nitrate ions is Z, and Z satisfies: 2≤Z≤15. When the chloride ions and nitrate ions are within this ratio range, the solvation structure of the electrolyte is regulated to have a better film-forming effect.

[0008] In some embodiments, the unit cell parameter a of the positive electrode material satisfies

[0009] In some embodiments, the unit cell parameter c of the positive electrode material satisfies

[0010] When the unit cell parameters of the positive electrode material are within the above range, the Li-O interlayer spacing of the positive electrode material is larger, thereby further improving the kinetic performance of the positive electrode material.

[0011] In some embodiments, 4.95≤c / a≤5.0. Meeting the above range can further improve the first coulombic efficiency and high temperature cycle performance of the electrochemical device, and further reduce the thickness expansion rate.

[0012] In some embodiments, the X-ray diffraction spectrum of the positive electrode material has diffraction peaks in the ranges of 17.5° to 19.0°, 35.5° to 38.5°, and 43.0° to 44.5°. The positive electrode material having the above characteristics can further improve the first coulombic efficiency and high temperature cycle performance of the electrochemical device, and further reduce the thickness expansion rate.

[0013] In some embodiments, the positive electrode material includes a lithium transition metal oxide, the lithium transition metal oxide includes a T element, and the T element includes at least one of Ni, Co, or Mn. The positive electrode material satisfying the above conditions can further improve the first coulombic efficiency and high temperature cycle performance of the electrochemical device, and further reduce the thickness expansion rate.

[0014] In some embodiments, based on the molar amount of the T element in the lithium transition metal oxide, the molar percentage of the Ni element is greater than or equal to 50%. The positive electrode material having the above characteristics can further improve the first coulombic efficiency and high temperature cycle performance of the electrochemical device, and further reduce the thickness expansion rate.

[0015] In some embodiments, the molar percentage of the Mn element is less than or equal to 50% based on the molar amount of the T element in the lithium transition metal oxide; and / or, the molar percentage of the Co element is less than or equal to 50% based on the molar amount of the T element. The positive electrode material having the above characteristics can further improve the first coulombic efficiency and high temperature cycle performance of the electrochemical device, and further reduce the thickness expansion rate.

[0016] In some embodiments, the mass percentage of Li element is greater than or equal to 5% based on the mass of lithium transition metal oxide. The positive electrode material having the above characteristics can further improve the first coulombic efficiency and high temperature cycle performance of the electrochemical device, and further reduce the thickness expansion rate.

[0017] In some embodiments, the lithium transition metal oxide further comprises at least one of the group consisting of Na element, R element and Q element, and the molar amount of Na element in the lithium transition metal oxide is n Na , the molar amount of Ni element is n Ni , the molar amount of Co element is n Co , the molar amount of Mn element is n Mn, the molar amount of element R is n R , the molar amount of element Q is n Q , the total molar amount of element T is n T , where 0≤n Na / n T ≤0.2, 0.5≤n Ni / n T ≤1,0≤n Co / n T ≤0.5, 0≤n Mn / n T ≤0.5, 0≤n R / n T ≤0.3, 0.00014≤n Q / n T ≤0.03, R element includes at least one of Ca, Sr, Ba, Al, Fe, B, Mg, Si, S, Ti, Cr, Fe, Cu, Zn, Ga, Zr, Mo, W, Nb, In, Sn, Pb, Sb, Ce, La, Ta or Hf, and Q element includes at least one of F, Cl, Br, I, N or P. The R element can support the transition metal layer, thereby improving the structural stability of the positive electrode material. The Q element regulates the electrolyte solvent structure to form a thinner, denser and more stable interface layer (CEI) film on the positive electrode surface.

[0018] The present application also provides a method for preparing the aforementioned positive electrode material, which comprises the following steps: 1) mixing a precursor with an optional sodium source and an optional R element source, introducing a first atmosphere, and calcining at a first temperature for a first time; 2) cooling to room temperature under a second atmosphere, and treating to obtain a first product; 3) mixing the first product obtained in step 2) with a lithium source, introducing a first atmosphere, and reacting at a second temperature, and keeping the temperature for a second time; 4) cooling to room temperature under a third atmosphere, and treating to obtain a second product; 5) mixing the second product obtained in step 4) with a lithium source, introducing a third atmosphere, and reacting at a second temperature, and keeping the temperature for a second time. The precursor comprises an element T, and the element T comprises at least one of Ni, Co and Mn. The element R comprises at least one of Ca, Sr, Ba, Al, Fe, B, Mg, Si, S, Ti, Cr, Fe, Cu, Zn, Ga, Zr, Mo, W, Nb, In, Sn, Pb, Sb, Ce, La, Ta and Hf. The element Q comprises at least one of F, Cl, Br, I, N and P.

[0019] In some embodiments, the first atmosphere is selected from air.

[0020] In some embodiments, the second atmosphere is selected from an inert gas or an inert gas and H 2At least one of the mixed gases; wherein the inert gas is selected from N 2 , Ar or He.

[0021] In some embodiments, the third atmosphere is selected from air, an inert gas, or a mixture of air and an inert gas; wherein the inert gas is selected from N 2 , Ar or He.

[0022] In some embodiments, the first temperature is 700° C. to 1200° C.; and the first time is 10 h to 48 h.

[0023] In some embodiments, the second temperature is 300° C. to 600° C.; and the second time is 4 h to 24 h.

[0024] In some embodiments, the third temperature is 100° C. to 300° C.; and the third time is 1 h to 5 h.

[0025] In some embodiments, the cooling rate in step 2) is 5°C / min to 30°C / min.

[0026] In some embodiments, the heating rate in step 3) is 5°C / min to 30°C / min.

[0027] In some embodiments, the cooling rate in step 4) is 20°C / min to 50°C / min.

[0028] In some embodiments, the cooling rate in step 6) is 5°C / min to 30°C / min.

[0029] In some embodiments, based on an inert gas and H 2 The total volume of the mixed gas, inert gas and H 2 In the mixed gas, H 2 The volume percentage is less than or equal to 20%.

[0030] In some embodiments, the precursor includes a hydroxide of a T element.

[0031] In some embodiments, the lithium source includes at least one of lithium carbonate, lithium nitrate, lithium chloride, or lithium hydroxide.

[0032] In some embodiments, the sodium source includes at least one of a carbonate or a hydroxide of the element sodium.

[0033] In some embodiments, the source of the R element includes an oxide of the R element.

[0034] In some embodiments, the source of the Q element includes at least one of an ammonium salt or a lithium salt of the Q element.

[0035] In some embodiments, when an electrode including the above-mentioned positive electrode material is assembled into a button cell with lithium metal, and the button cell is charged and discharged at a current of 0.01C in a voltage range of 2.8V to 4.5V, the voltage capacity differential dQ / dV curve obtained has a first oxidation peak and a first reduction peak in the range of 4.2V to 4.5V. The peak voltage of the first oxidation peak is Vo1, the peak voltage of the first reduction peak is Vr1, and |Vo1-Vr1|≤0.1V. This indicates that the positive electrode material has a reversible charge and discharge capacity in the high voltage range of 4.2V to 4.5V, so that the positive electrode material has a higher energy density and good structural stability.

[0036] In some embodiments, the positive electrode and lithium metal are assembled into a button cell, and when the button cell is charged and discharged at a current of 0.01C in a voltage range of 2.8V to 4.5V, the voltage capacity differential dQ / dV curve obtained has a second oxidation peak and a second reduction peak in the range of 3.6V to 4.0V. The peak voltage of the second oxidation peak is Vo2, the peak voltage of the second reduction peak is Vr2, and |Vo2-Vr2|≤0.1V. The positive electrode material having the above characteristics can further improve the first coulomb efficiency and high temperature cycle performance of the electrochemical device, and further reduce the thickness expansion rate.

[0037] In some embodiments, when the button cell is charged and discharged at a current of 0.1C in a voltage range of 2.8V to 4.5V, the discharge curve in the obtained voltage-capacity curve has a platform in the range of 4.2V to 4.5V. This indicates that the positive electrode material can have a reversible discharge capacity in the high voltage range of 4.2V to 4.5V, and the electrochemical device can obtain better first coulomb efficiency, high temperature cycle performance and thickness expansion rate.

[0038] In some embodiments, when the button cell is charged and discharged at a current of 0.1C in a voltage range of 2.8V to 4.5V, the capacity of the discharge curve in the range of 4.2V to 4.5V is Q1, and the capacity of the discharge curve in the range of 3.0V to 4.5V is Qt, satisfying: 0.2≤Q1 / Qt≤0.3. At this time, the capacity of the positive electrode material in the high voltage range of 4.2V to 4.5V is higher, so that the positive electrode material has a higher energy density.

[0039] In a second aspect, the present application further provides an electrochemical device, which includes the positive electrode material of the first aspect or the positive electrode material prepared according to the preparation method of the first aspect.

[0040] In some embodiments, the electrochemical device further comprises an electrolyte, the electrolyte comprising a boron-containing additive, the boron-containing additive comprising LiBOB, LiDFOB, LiBF 4At least one of the following. The boron-containing additive in the electrolyte works together with the nitrate ions and chloride ions introduced by the positive electrode material to regulate the electrolyte solvation structure, improve the conductivity of the electrolyte, thereby reducing the resistance inside the battery, and forming a more stable SEI film on the surface of the negative electrode, thereby improving the interface stability and thermal stability of the battery. This can further improve the first coulomb efficiency and high-temperature cycle performance of the electrochemical device and reduce the thickness expansion rate.

[0041] In some embodiments, the mass percentage of the boron-containing additive is 0.1% to 2% based on the mass of the electrolyte. The mass percentage of the boron-containing additive in the above range is more conducive to improving the first coulombic efficiency and high temperature cycle performance of the electrochemical device and reducing the thickness expansion rate.

[0042] In a third aspect, the present application provides an electronic device comprising the electrochemical device of the second aspect.

[0043] Beneficial effects:

[0044] The present invention introduces nitrate ions (NO 3 - ) and chloride ions (Cl - ), NO 3 - and Cl - The combined effects of the two regulate the electrolyte solvation structure and film-forming effect, so that a thinner, denser and more stable interface (CEI) film is formed on the positive electrode surface. 3 - It can act as a film-forming additive on the negative electrode surface and stabilize the solid electrolyte interface (SEI) film. The positive electrode material can improve the first coulomb efficiency and high-temperature cycle performance of the electrochemical device and reduce the thickness expansion rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] The following will briefly describe the drawings necessary for describing the embodiments of the present application or the prior art to facilitate the description of the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, drawings of other embodiments can still be obtained based on the structures illustrated in these drawings.

[0046] Figure 1 The XRD patterns of the positive electrode material powders of Comparative Example 1 and Example 1.

[0047] Figure 2 The voltage-capacity curves of button batteries of Comparative Example 1 and Example 1 are shown.

[0048] Figure 3 The voltage capacity differential dQ / dV curves of the button-type batteries of Comparative Example 1 and Example 1 are shown. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical scheme and advantages of the present application clearer, the technical scheme of the present application will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The relevant embodiments described herein are illustrative and are used to provide a basic understanding of the present application. The embodiments of the present application should not be interpreted as limiting the present application.

[0050] For simplicity, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.

[0051] In the description herein, unless otherwise specified, “above” and “below” include the number.

[0052] Unless otherwise specified, the terms used in this application have the commonly known meanings generally understood by those skilled in the art. Unless otherwise specified, the numerical values ​​of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).

[0053] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0054] In the description of this article, it should also be noted that the terms "first", "second", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.

[0055] In a first aspect, the present application provides a positive electrode material comprising nitrate ions and chloride ions, wherein, based on the mass of the positive electrode material, the mass percentage of the nitrate ions is 0.01% to 0.2%, and the mass percentage of the chloride ions is 0.05% to 1.0%.

[0056] The present invention introduces nitrate ions (NO 3 - ) and chloride ions (Cl - ), NO 3 - and Cl - The combined effect of regulating the electrolyte solvation structure and film-forming effect enables a thinner, denser and more stable interface (CEI) film to be formed on the cathode surface. 3 - It can act as a film-forming additive on the negative electrode surface and stabilize the solid electrolyte interface (SEI) film. The positive electrode material can improve the first coulomb efficiency and high-temperature cycle performance of the electrochemical device and reduce the thickness expansion rate.

[0057] In some embodiments, based on the mass of the positive electrode material, the mass percentage of nitrate ions is 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20% or the range of any two of these values. In some embodiments, the mass percentage of nitrate ions is 0.015% to 0.1%.

[0058] In some embodiments, based on the mass of the positive electrode material, the mass percentage of chloride ions is 0.05%, 0.10%, 0.15%, 0.20%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50%, 0.55%, 0.60%, 0.65%, 0.70%, 0.75%, 0.80%, 0.85%, 0.90%, 0.95%, 1.0% or any two of these values. In some embodiments, the mass percentage of chloride ions is 0.25% to 0.5%.

[0059] In some embodiments, the mass percentage ratio of chloride ions to nitrate ions is Z, and Z satisfies: 2≤Z≤15. In some embodiments, Z can be 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or a range consisting of any two of these values. When chloride ions and nitrate ions are within this ratio, the solvation structure of the electrolyte can be regulated to have a better film-forming effect. The above numerical values ​​can be obtained by conventional testing methods in the art, such as ion chromatography.

[0060] In some embodiments, the unit cell parameter a of the positive electrode material satisfies In some embodiments, the unit cell parameter c of the positive electrode material satisfies In some embodiments, 4.95≤c / a≤5.0.

[0061] In some embodiments, a can be Or a range consisting of any two of these values.

[0062] In some embodiments, c can be Or a range consisting of any two of these values. When the unit cell parameter c of the positive electrode material is within the above range, the Li-O interlayer spacing of the positive electrode material is larger, thereby improving the kinetic performance of the positive electrode material.

[0063] In some embodiments, c / a may be 4.95, 4.96, 4.97, 4.98, 4.99, 5.00, or a range consisting of any two of these values.

[0064] In some embodiments, the X-ray diffraction pattern of the positive electrode material has diffraction peaks in the ranges of 17.5° to 19.0°, 35.5° to 38.5°, and 43.0° to 44.5°.

[0065] In some embodiments, the positive electrode material includes a lithium transition metal oxide, the lithium transition metal oxide includes a T element, and the T element includes at least one of Ni, Co or Mn. In some embodiments, based on the molar amount of the T element in the lithium transition metal oxide, the molar percentage of the Ni element is greater than or equal to 50%. In some embodiments, based on the molar amount of the T element in the lithium transition metal oxide, the molar percentage of the Ni element in the lithium transition metal oxide is less than or equal to 98%. For example, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 98% or a range consisting of any two of these values.

[0066] In some embodiments, based on the molar amount of the T element in the lithium transition metal oxide, the molar percentage of the Mn element is less than or equal to 50%, for example, 0.5%, 1%, 5%, 10%, 20%, 30%, 40%, 50%, or a range consisting of any two of these values.

[0067] Based on the molar amount of the T element, the molar percentage of the Co element is less than or equal to 50%, for example, 0.5%, 1%, 5%, 10%, 20%, 30%, 40%, 50% or a range consisting of any two of these values.

[0068] In some embodiments, the mass percentage of the Li element is greater than or equal to 5% based on the mass of the lithium transition metal oxide.

[0069] In some embodiments, the positive electrode material includes Li element and other metal elements, and the other metal elements may include at least one of the group consisting of Na element, T element or R element. The ratio of the molar amount of Li element to the total molar amount of the other metal elements is greater than 0.5 and less than 2.

[0070] In some embodiments, the ratio of the molar amount of Li element to the sum of the molar amounts of other metal elements is 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0 or a range consisting of any two of these values.

[0071] In some embodiments, the lithium transition metal oxide further comprises at least one of the group consisting of Na element, R element and Q element, and the molar amount of Na element in the lithium transition metal oxide is n Na , the molar amount of Ni element is n Ni , the molar amount of Co element is n Co , the molar amount of Mn element is n Mn , the molar amount of element R is n R , the molar amount of element Q is n Q , the total molar amount of element T is n T , where 0≤n Na / n T ≤0.2, 0.5≤n Ni / n T ≤1,0≤n Co / n T ≤0.5, 0≤n Mn / n T ≤0.5, 0≤n R / n T ≤0.3, 0.00014≤n Q / n T≤0.03, R element includes at least one of Ca, Sr, Ba, Al, Fe, B, Mg, Si, S, Ti, Cr, Fe, Cu, Zn, Ga, Zr, Mo, W, Nb, In, Sn, Pb, Sb, Ce, La, Ta or Hf, and Q element includes at least one of F, Cl, Br, I, N or P. The R element can support the transition metal layer, thereby improving the structural stability of the positive electrode material. The Q element regulates the electrolyte solvent structure to form a thinner, denser and more stable interface layer (CEI) film on the positive electrode surface.

[0072] The present application also provides a method for preparing the aforementioned positive electrode material, which comprises the steps of:

[0073] 1) mixing a precursor with an optional sodium source and an optional R element source, introducing the precursor into a first atmosphere, and calcining the precursor for a first time at a first temperature;

[0074] 2) cooling the temperature to room temperature under the condition of introducing the second atmosphere, and treating to obtain the first product;

[0075] 3) mixing the first product obtained in step 2) with a lithium source, introducing the first atmosphere, reacting at a second temperature, and keeping the temperature for a second time;

[0076] 4) cooling the temperature to room temperature under the condition of introducing the third atmosphere, and treating to obtain the second product;

[0077] 5) mixing the second product obtained in step 4) with a lithium source and an optional Q element source, introducing the first atmosphere, and calcining at a third temperature for a third time;

[0078] 6) cooling to room temperature and treating to obtain a positive electrode material; the precursor comprises element T, element T comprises at least one of Ni, Co or Mn; element R comprises at least one of Ca, Sr, Ba, Al, Fe, B, Mg, Si, S, Ti, Cr, Fe, Cu, Zn, Ga, Zr, Mo, W, Nb, In, Sn, Pb, Sb, Ce, La, Ta or Hf; element Q comprises at least one of F, Cl, Br, I, N or P.

[0079] In some embodiments, the first atmosphere is selected from air.

[0080] In some embodiments, the second atmosphere is selected from an inert gas or an inert gas and H 2 At least one of the mixed gases; wherein the inert gas is selected from N 2 , Ar or He.

[0081] In some embodiments, the third atmosphere is selected from air, an inert gas, or a mixture of air and an inert gas; wherein the inert gas is selected from N 2, Ar or He.

[0082] In some embodiments, the first temperature is 700°C to 1200°C; the first time is 10h to 48h. In some embodiments, the first temperature can be 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, or a range consisting of any two of these values. In some embodiments, the first time can be 10h, 12h, 16h, 18h, 24h, 36h, 48h, or a range consisting of any two of these values.

[0083] In some embodiments, the second temperature is 300°C to 600°C; the second time is 4h to 24h. In some embodiments, the second temperature can be 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, or a range consisting of any two of these values. In some embodiments, the second time can be 4h, 6h, 8h, 10h, 12h, 16h, 18h, 24h, or a range consisting of any two of these values.

[0084] In some embodiments, the third temperature is 100°C to 300°C; the third time is 1h to 5h. In some embodiments, the third temperature can be 100°C, 150°C, 200°C, 250°C, 300°C, or a range consisting of any two of these values. In some embodiments, the third time can be 1h, 2h, 3h, 4h, 5h, or a range consisting of any two of these values.

[0085] In some embodiments, the cooling rate in step 2) is 5°C / min to 30°C / min. In some embodiments, the cooling rate can be 5°C / min, 10°C / min, 15°C / min, 20°C / min, 25°C / min, 30°C / min, or a range consisting of any two of these values.

[0086] In some embodiments, the heating rate in step 3) is 5°C / min to 30°C / min. In some embodiments, the heating rate can be 5°C / min, 10°C / min, 15°C / min, 20°C / min, 25°C / min, 30°C / min, or a range consisting of any two of these values.

[0087] In some embodiments, the cooling rate in step 4) is 20°C / min to 50°C / min. In some embodiments, the cooling rate can be 20°C / min, 25°C / min, 30°C / min, 35°C / min, 40°C / min, 45°C / min, 50°C / min, or a range consisting of any two of these values.

[0088] In some embodiments, the cooling rate in step 6) is 5°C / min to 30°C / min. In some embodiments, the cooling rate can be 5°C / min, 10°C / min, 15°C / min, 20°C / min, 25°C / min, 30°C / min, or a range consisting of any two of these values.

[0089] In some embodiments, based on an inert gas and H 2 The total volume of the mixed gas, inert gas and H 2 In the mixed gas, H 2 The volume percentage is less than or equal to 20%. In some embodiments, based on the inert gas and H 2 The total volume of the mixed atmosphere, inert gas and H 2 H in mixed atmosphere 2 The volume percentage can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% or a range consisting of any two of these values.

[0090] In some embodiments, the precursor includes a hydroxide of element T. Element T includes at least one of Ni, Co, or Mn.

[0091] In some embodiments, the lithium source includes at least one of lithium carbonate, lithium nitrate, lithium chloride, or lithium hydroxide.

[0092] In some embodiments, the sodium source includes at least one of a carbonate or a hydroxide of the element sodium.

[0093] In some embodiments, the source of the R element includes an oxide of the R element.

[0094] In some embodiments, the source of the Q element includes at least one of an ammonium salt or a lithium salt of the Q element.

[0095] In some embodiments, an electrode including the positive electrode material in the present application is assembled with lithium metal into a button cell, and when the button cell is charged and discharged at a current of 0.01C in a voltage range of 2.8V to 4.5V, the voltage capacity differential dQ / dV curve obtained has a first oxidation peak and a first reduction peak in the range of 4.2V to 4.5V. The peak voltage of the first oxidation peak is Vo1, the peak voltage of the first reduction peak is Vr1, and |Vo1-Vr1|≤0.1V. It shows that the positive electrode material has a reversible charge and discharge capacity in the high voltage range of 4.2V to 4.5V, so that the positive electrode material has a high energy density and good structural stability. In some embodiments, |Vo1-Vr1| can be 0.1V, 0.09V, 0.08V, 0.07V, 0.06V, 0.05V, 0.04V, 0.03V, 0.02V, 0.01V, or a range consisting of any two of these values.

[0096] In some embodiments, an electrode including the positive electrode material in the present application is assembled with lithium metal into a button cell, and when the button cell is charged and discharged at a current of 0.01C in a voltage range of 2.8V to 4.5V, the voltage capacity differential dQ / dV curve obtained has a second oxidation peak and a second reduction peak in the range of 3.6V to 4.0V. The peak voltage of the second oxidation peak is Vo2, the peak voltage of the second reduction peak is Vr2, and |Vo2-Vr2|≤0.1V. In some embodiments, |Vo2-Vr2|≤0.1V can be 0.1V, 0.09V, 0.08V, 0.07V, 0.06V, 0.05V, 0.04V, 0.03V, 0.02V, 0.01V, or a range consisting of any two of these values.

[0097] In some embodiments, when the button cell is charged and discharged at a current of 0.1C in a voltage range of 2.8V to 4.5V, the discharge curve in the obtained voltage capacity curve has a platform in the range of 4.2V to 4.5V, indicating that the positive electrode material can have a reversible discharge capacity in the high voltage range of 4.2V to 4.5V.

[0098] In some embodiments, when the button battery is charged and discharged at a current of 0.1C in the voltage range of 2.8V to 4.5V, the capacity of the discharge curve in the range of 4.2V to 4.5V is Q1, and the capacity of the discharge curve in the range of 3.0V to 4.5V is Qt, satisfying: 0.2≤Q1 / Qt≤0.3. At this time, the capacity of the positive electrode material in the high voltage range of 4.2V to 4.5V is higher, so that the positive electrode material has a higher energy density. In some embodiments, Q1 / Qt can be 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30 or a range consisting of any two of these values.

[0099] In a second aspect, the present application further provides an electrochemical device, which includes a positive electrode, wherein the positive electrode includes a positive electrode material layer, and the positive electrode material layer includes the positive electrode material described above.

[0100] In some embodiments, the positive electrode material layer also includes a conductive agent and a binder. In some embodiments, the binder includes, but is not limited to: polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber or acrylic (ester) styrene-butadiene rubber, etc. In some embodiments, the conductive agent includes, but is not limited to: carbon-based materials, metal-based materials, conductive polymers and mixtures thereof. In some embodiments, the carbon-based material is selected from graphite, carbon black, acetylene black, Ketjen black, carbon nanotubes, carbon fibers, graphene or any combination thereof. In some embodiments, the metal-based material is selected from metal powder, metal fiber, copper, nickel, aluminum or silver. In some embodiments, the conductive polymer is a polyphenylene derivative.

[0101] In some embodiments, the positive electrode further includes a positive electrode current collector, which may be a metal foil or a composite current collector. For example, aluminum foil may be used. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymer substrate.

[0102] The electrochemical device of the present application further comprises a negative electrode, which comprises a negative electrode material layer and a negative electrode current collector.

[0103] In some embodiments, the negative electrode material layer includes a negative electrode active material, a conductive agent and a binder. In some embodiments, the negative electrode active material may include a material that reversibly intercalates / deintercalates lithium ions, lithium metal, lithium metal alloy or transition metal oxide. In some embodiments, the negative electrode active material includes at least one of a carbon material or a silicon material, the carbon material includes at least one of graphite and hard carbon, and the silicon material includes at least one of silicon, silicon oxide, silicon carbon compound or silicon alloy. In some embodiments, the binder may include various binder polymers. In some embodiments, the binder includes polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, sodium carboxymethyl cellulose, polyvinyl pyrrolidone, polyvinyl ether, polytetrafluoroethylene, polyhexafluoropropylene or styrene-butadiene rubber. In some embodiments, the conductive agent may use any conductive material as long as it does not cause chemical changes. In some embodiments, the conductive agent includes at least one of conductive carbon black, acetylene black, carbon nanotubes, Ketjen black, carbon fiber or graphene.

[0104] In some embodiments, the negative electrode current collector may be copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, or a combination thereof.

[0105] In some embodiments, the electrochemical device further comprises an electrolyte, the electrolyte comprising a boron-containing additive, the boron-containing additive comprising LiBOB, LiDFOB, LiBF 4 , C 4 BLiO 8 At least one of the following. The boron-containing additive in the electrolyte works together with the nitrate ions and chloride ions introduced by the positive electrode material to regulate the electrolyte solvation structure, improve the conductivity of the electrolyte, thereby reducing the resistance inside the battery, and forming a more stable SEI film on the surface of the negative electrode, thereby improving the interface stability and thermal stability of the battery. This can further improve the first coulomb efficiency and high-temperature cycle performance of the electrochemical device and reduce the thickness expansion rate. The boron-containing additive is preferably LiBOB and / or LiDFOB.

[0106] In some embodiments, based on the mass of the electrolyte, the mass percentage of the boron-containing additive is 0.1% to 2%. In some embodiments, the mass percentage of the boron-containing additive is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0% or a range consisting of any two of these values. Too high a mass percentage of the boron-containing additive will significantly increase the impedance of the battery. In some embodiments, the mass percentage of the boron-containing additive is 1.0% to 2.0%.

[0107] In some embodiments, the electrolyte further includes a non-aqueous solvent, and the non-aqueous solvent may be a carbonate compound, a carboxylate compound, an ether compound, other organic solvents, or a combination thereof.

[0108] The carbonate compound may be a linear carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound or a combination thereof.

[0109] Examples of the above-mentioned linear carbonate compounds are dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC) and combinations thereof. Examples of cyclic carbonate compounds are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) and combinations thereof. Examples of fluorocarbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate and combinations thereof.

[0110] Examples of the above carboxylic acid ester compounds are methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanoic acid lactone, valerolactone, mevalonolactone, caprolactone and combinations thereof.

[0111] Examples of the above ether compound are dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, and combinations thereof.

[0112] Examples of the above other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate and phosphoric acid esters and combinations thereof.

[0113] According to some embodiments of the present application, in the electrochemical device, a separator is provided between the positive electrode and the negative electrode to prevent short circuit. The material and shape of the separator used in the embodiments of the present application are not particularly limited, and it can be any technology disclosed in the prior art. In some embodiments, the separator includes a polymer or inorganic substance formed by a material that is stable to the electrolyte of the present application. For example, the separator may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer includes at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film can be selected. A surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer can be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. The inorganic layer includes inorganic particles and a binder, and the inorganic particles include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The binder includes at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. The polymer layer includes a polymer, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride or poly (vinylidene fluoride-hexafluoropropylene).

[0114] According to some embodiments of the present application, the electrochemical device of the present application includes, but is not limited to: all kinds of primary batteries or secondary batteries. In some embodiments, the electrochemical device is a lithium secondary battery. In some embodiments, the lithium secondary battery includes, but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0115] In a third aspect, the electronic device of the present application may be any device using the electrochemical device of the second aspect of the present application.

[0116] In some embodiments, the electronic device includes, but is not limited to: laptop computers, pen-type computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries or lithium-ion capacitors, etc.

[0117] Examples and Comparative Examples

[0118] Hereinafter, the present application will be described in more detail with reference to Examples and Comparative Examples, but the present application is not limited to these Examples unless departing from the gist of the present application.

[0119] 1. Preparation of positive electrode materials

[0120] Comparative Example 1

[0121] In this comparative example, the synthesis of the positive electrode material is:

[0122] Step 1: Prepare NiSO according to the element molar ratio of Ni:Mn=50:50 4 、MnSO 4 The mixed solution was mixed with a precipitant (NaOH solution) and a complexing agent (ammonia water) to react, and the precursor Ni was obtained by controlling the reaction time to 60 hours, the ammonia concentration to 1 mol / L, and the pH value to 12.2. 0.5 Mn 0.5 (OH) 2 ;

[0123] Step 2: Grind and mix the nickel-manganese precursor and lithium carbonate in the above step 1 in a certain proportion, calcine at 800°C in an air atmosphere for 20 hours, cool to room temperature at a rate of 10°C / min, and finally crush and sieve to obtain the positive electrode material.

[0124] Comparative Example 2

[0125] In this comparative example, the synthesis of the positive electrode material is:

[0126] Step 1: Prepare NiSO according to the element molar ratio of Ni:Mn=50:50 4 、MnSO 4 The mixed solution was mixed with a precipitant (NaOH solution) and a complexing agent (ammonia water) to react, and the precursor Ni was obtained by controlling the reaction time to 60 hours, the ammonia concentration to 1 mol / L, and the pH value to 12.2. 0.5 Mn 0.5 (OH)2 ;

[0127] Step 2: Grind and mix the nickel-manganese precursor and sodium carbonate in the above step 1 in a molar ratio of 1:0.525, calcine in a dry air atmosphere at 800°C for 20 hours, introduce a second mixed gas (specific composition see Table 1) and cool to room temperature at a rate of 10°C / min, and obtain a first product by crushing and sieving;

[0128] Step 3, the first product obtained in step 2 is fully mixed with a lithium source (a mixture of lithium hydroxide and lithium nitrate in a molar ratio of 5:5) (an excess of a mixture of lithium hydroxide and lithium nitrate, an element molar ratio of Li:TM>6), and then heated to 400°C at a rate of 10°C / min in a dry air atmosphere and kept at a constant temperature for 8 hours, a third mixed gas (Ar / air mixed gas) is introduced and cooled to room temperature at a rate of 30°C / min, and the positive electrode material is obtained after washing with deionized water, drying, and sieving.

[0129] Example 1

[0130] In this embodiment, the positive electrode material is synthesized as follows:

[0131] Step 1: Prepare NiSO according to the element molar ratio of Ni:Mn=50:50 4 、MnSO 4 The mixed solution was mixed with a precipitant (NaOH solution) and a complexing agent (ammonia water) to react, and the precursor Ni was obtained by controlling the reaction time to 60 hours, the ammonia concentration to 1 mol / L, and the pH value to 12.2. 0.5 Mn 0.5 (OH) 2 ;

[0132] Step 2: Grind and mix the nickel-manganese precursor and sodium carbonate in the above step 1 in a molar ratio of 1:0.525, calcine in a dry air atmosphere at 800°C for 20 hours, introduce a second mixed gas (specific composition see Table 1) and cool to room temperature at a rate of 10°C / min, and obtain a first product by crushing and sieving;

[0133] Step 3, the first product obtained in step 2 is fully mixed with a lithium source (a mixture of lithium hydroxide and lithium nitrate in a molar ratio of 5:5) (an excess of a mixture of lithium hydroxide and lithium nitrate, an element molar ratio of Li:TM>6), and then heated to 400°C at a rate of 10°C / min in a dry air atmosphere and kept at a constant temperature for 8h, a third mixed gas (Ar / air mixed gas) is introduced and cooled to room temperature at a rate of 30°C / min, and a second product is obtained by washing with deionized water, drying, and sieving;

[0134] Step 4: Grind and mix the second product obtained in step 3 with a certain proportion of lithium nitrate and lithium chloride, calcine in an air atmosphere at 200° C. for 2 h, cool to room temperature at a rate of 10° C. / min, and finally crush and sieve to obtain the positive electrode material.

[0135] Example 2-3

[0136] The positive electrode material preparation method provided in Examples 2-3 can refer to Example 1, except that:

[0137] In order to obtain positive electrode materials with different sodium contents, the constant temperature and constant temperature time are changed in step 3. The constant temperature and constant temperature time of Example 2 are 370° C. and 6 h, respectively, and the constant temperature and constant temperature time of Example 3 are 340° C. and 5 h, respectively.

[0138] Embodiment 4-9

[0139] The positive electrode material preparation method provided in Examples 4-9 can refer to Examples 1-3, except that:

[0140] In step 2, different proportions of calcium oxide are doped. Among them, the molar ratio of calcium oxide to precursor in Examples 4-6 is M CaO / 前驱体 =0.011:1, the molar ratio of calcium oxide to precursor in Examples 7-9 is M CaO / 前驱体 =0.023:1.

[0141] Examples 10-15

[0142] The positive electrode material preparation methods provided in Examples 10-15 can refer to Examples 1-3, except that:

[0143] In step 2, different proportions of nano-magnesium oxide are doped. The molar ratio of nano-magnesium oxide to the precursor in Examples 10-12 is M MgO / 前驱体 =0.012:1, the molar ratio of nano-magnesium oxide to the precursor in Example 13-15 is M MgO / 前驱体 =0.023:1.

[0144] Examples 16-17

[0145] The method for preparing the positive electrode material provided in Examples 16-17 is the same as that in Example 1.

[0146] Table 1 shows the volume percentages of nitrogen and hydrogen in the second mixed gas, the unit cell parameter a, the unit cell parameter c, c / a, Cl in Comparative Examples 1-2 and Examples 1-15. - Based on the mass percentage of the positive electrode material, NO 3 - Based on the mass percentage of the positive electrode material and Cl - The mass percentage of NO3 - The ratio Z of the mass percentage content.

[0147] Table 1

[0148]

[0149] Note: The percentage of each component in the mixed gas is the volume percentage

[0150] 2. Preparation method of button battery:

[0151] Examples 1-15 and Comparative Examples 1-2

[0152] The positive electrode slurry is prepared from a certain weight ratio (1.5:1.5:97) of binder polyvinylidene fluoride (PVDF), conductive agent conductive carbon black (SuperP) and polyimide @ positive electrode active material. The viscosity of the positive electrode slurry is adjusted to about 3000mPa·s to about 6000mPa·s, and the mixed slurry is evenly coated on aluminum foil with a single layer thickness of 200μm and double layer coating; after drying, it is rolled to form the required electrode, and the humidity of the electrode processing and transportation environment is 45%. Among them, the surface density of the coated electrode is 14mg / cm 2 The positive electrode sheet was obtained by drying and punching into a 14 mm diameter disc to prepare a single-sided positive electrode sheet. The isolation film was punched into a 18 mm disc; the negative electrode used was a lithium metal sheet with a diameter of 18 mm; LiPF was added to a solvent mixed with propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) (weight ratio 1:1:1). 6 The electrolyte solution is obtained by mixing uniformly, wherein based on the volume of the electrolyte solution, LiPF 6 The mass concentration is 12.5%. Move the positive electrode sheet, diaphragm paper, negative electrode sheet (lithium sheet), electrolyte, battery shell and other accessories into the glove box (the water content must be less than 10ppm); assemble the battery and inject the electrolyte in the following stacking order from bottom to top: negative electrode shell> flat gasket> metal lithium sheet + appropriate amount of electrolyte> a layer of diaphragm paper + appropriate amount of electrolyte> positive electrode sheet + appropriate amount of electrolyte> flat gasket> shrapnel> positive electrode shell; package on the packaging machine to obtain button batteries.

[0153] Example 16

[0154] The positive electrode slurry is prepared from a certain weight ratio (1.5:1.5:97) of binder polyvinylidene fluoride (PVDF), conductive agent conductive carbon black (SuperP) and polyimide @ positive electrode active material. The viscosity of the positive electrode slurry is adjusted to about 3000mPa·s to about 6000mPa·s, and the mixed slurry is evenly coated on aluminum foil with a single layer thickness of 200μm and double layer coating; after drying, it is rolled to form the required electrode, and the humidity of the electrode processing and transportation environment is 45%. Among them, the surface density of the coated electrode is 14mg / cm 2 The positive electrode sheet was obtained by drying and punching into a 14 mm diameter disc to prepare a single-sided positive electrode sheet. The isolation film was punched into a 18 mm disc; the negative electrode used was a lithium metal sheet with a diameter of 18 mm; LiPF was added to a solvent mixed with propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) (weight ratio 1:1:1) respectively. 6 and LiBOB are uniformly mixed to obtain an electrolyte, wherein, based on the volume of the electrolyte, LiPF 6 The mass concentration is 12.5%, and the mass percentage of LiBOB is 1% based on the mass of the electrolyte. Move the positive electrode sheet, diaphragm paper, negative electrode sheet (lithium sheet), electrolyte, battery shell and other accessories into the glove box (the water content must be less than 10ppm); assemble the battery and inject the electrolyte in the stacking order from bottom to top: negative electrode shell> flat gasket> metal lithium sheet + appropriate amount of electrolyte> a layer of diaphragm paper + appropriate amount of electrolyte> positive electrode sheet + appropriate amount of electrolyte> flat gasket> shrapnel> positive electrode shell; package on the packaging machine to obtain a button battery.

[0155] Embodiment 17

[0156] The positive electrode slurry is prepared from a certain weight ratio (1.5:1.5:97) of binder polyvinylidene fluoride (PVDF), conductive agent conductive carbon black (SuperP) and polyimide @ positive electrode active material. The viscosity of the positive electrode slurry is adjusted to about 3000mPa·s to about 6000mPa·s, and the mixed slurry is evenly coated on aluminum foil with a single layer thickness of 200μm and double layer coating; after drying, it is rolled to form the required electrode, and the humidity of the electrode processing and transportation environment is 45%. Among them, the surface density of the coated electrode is 14mg / cm 2 The positive electrode sheet was obtained by drying and punching into a 14 mm diameter disc to prepare a single-sided positive electrode sheet. The isolation film was punched into a 18 mm disc; the negative electrode used was a lithium metal sheet with a diameter of 18 mm; LiPF was added to a solvent mixed with propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) (weight ratio 1:1:1) respectively. 6 and LiDFOB are mixed evenly to obtain an electrolyte, wherein based on the volume of the electrolyte, LiPF 6The mass concentration is 12.5%, and the mass percentage of LiDFOB is 0.4% based on the mass of the electrolyte. Move the positive electrode sheet, diaphragm paper, negative electrode sheet (lithium sheet), electrolyte, battery shell and other accessories into the glove box (the water content must be less than 10ppm); assemble the battery and inject the electrolyte in the stacking order from bottom to top: negative electrode shell> flat gasket> metal lithium sheet + appropriate amount of electrolyte> a layer of diaphragm paper + appropriate amount of electrolyte> positive electrode sheet + appropriate amount of electrolyte> flat gasket> shrapnel> positive electrode shell; package on the packaging machine to obtain button batteries.

[0157] 3. Preparation method of lithium-ion battery:

[0158] Examples 1-15 and Comparative Examples 1-2

[0159] (1) Preparation of positive electrode

[0160] The positive electrode slurry is prepared by mixing a binder polyvinylidene fluoride (PVDF), a conductive agent conductive carbon black (SuperP) and a positive electrode active material in a certain weight ratio (1.5:1.5:97). The viscosity of the positive electrode slurry is adjusted to about 3000mPas to about 6000mPas, and the mixed slurry is evenly coated on the aluminum foil, with a single layer thickness of 40μm and double layer coating; dried, cold pressed, and then cut and welded to obtain the positive electrode. The humidity of the electrode processing and transportation environment is 45%, and the surface density of the coated electrode is 14mg / cm 2 The positive electrode was placed in a constant temperature and constant humidity environment to compare the hygroscopicity of the battery. After placement, the positive electrode was assembled with the graphite negative electrode into a 3.5Ah soft-pack battery for battery performance testing.

[0161] (2) Preparation of negative electrode

[0162] Artificial graphite, styrene-butadiene rubber and sodium carboxymethyl cellulose (CMC) were mixed with deionized water in a mass ratio of 96:2:2 and stirred evenly to obtain a negative electrode slurry. The negative electrode slurry was coated on a 12 μm thick copper foil. After drying, cold pressing, cutting and welding of the tabs, a negative electrode was obtained.

[0163] (3) Preparation of electrolyte

[0164] In a dry argon environment, LiPF was added to a solvent mixed with propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) (weight ratio 1:1:1). 6 The electrolyte solution is obtained by mixing uniformly, wherein based on the volume of the electrolyte solution, LiPF 6 The mass concentration is 12.5%.

[0165] (4) Preparation of isolation membrane

[0166] A polyethylene (PE) porous polymer film is used as the isolation membrane.

[0167] Preparation of lithium-ion batteries

[0168] Stack the positive electrode, separator and negative electrode in order, so that the separator is between the positive electrode and the negative electrode to play an isolating role. Wind to obtain a bare cell. Place the bare cell in an outer package, inject electrolyte and package. After the formation, degassing, trimming and other process flows, a lithium-ion battery is obtained.

[0169] Example 16

[0170] The preparation method of the lithium ion battery provided in Example 16 can refer to Example 1, except that:

[0171] (3) Preparation of electrolyte

[0172] In a dry argon environment, LiPF was added to a solvent mixed with propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) (weight ratio 1:1:1). 6 and LiBOB are uniformly mixed to obtain an electrolyte, wherein, based on the volume of the electrolyte, LiPF 6 The mass concentration is 12.5%, and based on the mass of the electrolyte, the mass percentage of LiBOB is 1%.

[0173] Embodiment 17

[0174] The preparation method of the lithium ion battery provided in Example 17 can refer to Example 1, except that:

[0175] In a dry argon environment, LiPF was added to a solvent mixed with propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) (weight ratio 1:1:1). 6 and LiDFOB are mixed evenly to obtain an electrolyte, wherein based on the volume of the electrolyte, LiPF 6 The mass concentration of LiDFOB is 12.5%, and based on the mass of the electrolyte, the mass percentage of LiDFOB is 0.4%.

[0176] Test Method

[0177] 1.XRD test

[0178] The positive electrode material was tested by X-ray powder diffractometer (XRD, instrument model: Bruker D8 ADVANCE) to obtain the half-width of the diffraction peaks of (101), (104), and (003) crystal planes; the target material was Cu Kα; the voltage and current were 40KV / 40mA, and the scanning angle range was 10° to 70°.

[0179] 2. 85℃ storage thickness expansion test

[0180] The lithium-ion soft-pack battery was charged at 0.5C to 4.45V at 25°C, and then charged at a constant voltage of 4.45V to 0.05C. The thickness of the lithium-ion battery at this time was measured with a micrometer and recorded as H11. The lithium-ion battery was then placed in an 85°C oven for 12 hours. After 12 hours, the thickness of the lithium-ion battery was measured with a micrometer and recorded as H12.

[0181] Thickness expansion ratio (%) of the lithium-ion battery after storage at 85° C. for 12 hours = (H12 −H11) / H11×100%.

[0182] 3. 45℃ Cyclic Capacity Retention Test

[0183] The lithium-ion soft-pack battery was placed in a 45°C constant temperature box and allowed to stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature; the lithium-ion battery that reached a constant temperature was charged to 4.35V at a constant current of 1.5C at 45°C, and then charged to 0.02C at a constant voltage of 4.35V; it was allowed to stand for 5 minutes, and then discharged to 2.8V at a constant current of 4C, and allowed to stand for 5 minutes. The discharge capacity of this test was recorded as the first cycle discharge capacity; this charge and discharge cycle was repeated 300 times, and the discharge capacity of the 300th cycle of the test battery was recorded as the 300th cycle discharge capacity.

[0184] The capacity retention rate (%) of a lithium-ion battery after 300 cycles at 45° C. = 300th cycle discharge capacity / first cycle discharge capacity×100%.

[0185] 4.Q1 / Qt test

[0186] Using an electrochemical workstation, the discharge curve of the lithium-ion button battery in the voltage range of 2.8V to 4.5V and at a rate of 0.1C was tested and obtained. The capacity in the voltage range of 4.2V to 4.5V was calculated to be Q1, and the capacity in the voltage range of 3.0V to 4.5V was Qt.

[0187] 5. First cycle coulomb efficiency test

[0188] The lithium-ion soft-pack battery is charged to 4.35V at a current of C / 5, and then discharged to 2.75V at a current of C / 5. The ratio of the discharge capacity to the rated capacity is the first-cycle coulombic efficiency.

[0189] 6. Power cycle retention rate

[0190] Charge the button cell to 4.5V at 25°C with a current of C / 5. Discharge the fully charged button cell to 2.8V at a current of C / 5. This cycle is recorded as the first cycle. Repeat the operation for 50 cycles. After the 50th cycle of discharge, record the discharge capacity as Q50. Calculate the cycle retention rate based on the button cell rated capacity Qn and the 50th cycle discharge capacity Q50: Cycle retention rate = (Q50 / Qn) × 100%.

[0191] Test Results

[0192] Table 2-1

[0193]

[0194] Table 2-2

[0195] Serial number First-cycle Coulomb efficiency Thickness expansion rate at 85℃ storage 45℃ cycle capacity retention rate Comparative Example 1 85% 40% 50% Comparative Example 2 89% 27% 68% Example 1 91% 12% 88% Example 2 92% 10% 89% Example 3 91% 8% 91% Example 4 91% 5% 89% Example 5 91% 6% 92% Example 6 90% 6% 91% Example 7 91% 5% 91% Example 8 92% 4% 92% Example 9 90% 4% 93% Example 10 90% 8% 91% Embodiment 11 90% 7% 90% Example 12 91% 7% 92% Embodiment 13 92% 6% 92% Embodiment 14 90% 9% 90% Embodiment 15 91% 5% 91% Example 16 93% 2% 94% Embodiment 17 91% 4% 91%

[0196] Comparison of the data of Examples 1-15 and Comparative Examples 1-2 shows that the positive electrode material is introduced with NO 3 - and Cl - Afterwards, the performance data of lithium-ion batteries, such as the charge cycle retention rate, first cycle coulomb efficiency, 85℃ storage thickness expansion rate, and 45℃ cycle capacity retention rate, were significantly improved, indicating that the NO 3 - and Cl - Under the combined effect, the electrolyte solvation structure and film-forming effect can be regulated to form a thinner, denser and more stable interface (CEI) film on the positive electrode surface. 3 - It also acts as a film-forming additive on the negative electrode surface, stabilizes the solid electrolyte interface (SEI) film, thereby improving the first cycle coulomb efficiency and high temperature cycle performance of the lithium-ion battery, and reducing the cycle expansion rate. It can be seen from the data shown in Examples 16-17 and Example 1 that after adding boron-containing additives to the electrolyte, the performance data of the lithium-ion battery such as the charge cycle retention rate, 85°C storage thickness expansion rate, and 45°C cycle capacity retention rate are further improved and optimized, achieving better results, indicating that the boron-containing additives in the electrolyte and the NO introduced by the positive electrode material 3 - and Cl - The combined effect further regulates the solvation structure, improves the conductivity of the electrolyte, reduces the resistance inside the battery, and forms a more stable SEI film on the surface of the negative electrode, further improving the interface stability and cycle thermal stability of the electrochemical device. It can also be seen from the data shown in Example 1 and Comparative Example 2 that the positive electrode material lacks NO 3 - and Cl -When the battery is charged, the cycle retention rate, first-cycle coulomb efficiency, high-temperature cycle performance and cycle expansion rate of lithium-ion batteries decrease significantly.

[0197] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.

Claims

1. A positive electrode material, characterized in that: The positive electrode material comprises nitrate ions and chloride ions, wherein, based on the mass of the positive electrode material, the mass percentage of the nitrate ions is 0.01% to 0.2%, and the mass percentage of the chloride ions is 0.05% to 1.0%.

2. The positive electrode material according to claim 1, wherein Based on the mass of the positive electrode material, the mass percentage of the nitrate ions is 0.015% to 0.1%, and the mass percentage of the chloride ions is 0.25% to 0.5%.

3. The positive electrode material according to claim 1, wherein The ratio of the mass percentage of the chloride ions to the mass percentage of the nitrate ions is Z, 2≤Z≤15.

4. The positive electrode material according to claim 1, wherein The unit cell parameter a and the unit cell parameter c of the positive electrode material satisfy at least one of the following conditions: (1) (2) (3)4.95≤c / a≤5.

0.

5. The positive electrode material according to claim 1, wherein The X-ray diffraction spectrum of the positive electrode material has diffraction peaks in the ranges of 17.5° to 19.0°, 35.5° to 38.5°, and 43.0° to 44.5°.

6. The positive electrode material according to claim 1, wherein The positive electrode material includes a lithium transition metal oxide, the lithium transition metal oxide includes a T element, the T element includes at least one of Ni, Co or Mn, and the lithium transition metal oxide satisfies at least one of the following conditions: (1) Based on the molar amount of the T element, the molar percentage of the Ni element is greater than or equal to 50%; (2) Based on the molar amount of the T element, the molar percentage of the Mn element is less than or equal to 50%; (3) Based on the molar amount of the T element, the molar percentage of the Co element is less than or equal to 50%; (4) Based on the mass of the lithium transition metal oxide, the mass percentage of Li element is greater than or equal to 5%; (5) The lithium transition metal oxide further comprises at least one of the group consisting of Na element, R element and Q element, and the molar amount of Na element in the lithium transition metal oxide is n Na , the molar amount of Ni element is n Ni , the molar amount of Co element is n Co , the molar amount of Mn element is n Mn , the molar amount of element R is n R , the molar amount of element Q is n Q , the molar amount of element T is n T , where 0≤n Na / n T ≤0.2, 0.5≤n Ni / n T ≤1,0≤n Co / n T ≤0.5, 0≤n Mn / n T ≤0.5, 0≤n R / n T ≤0.3, 0.00014≤n Q / n T ≤0.03, the R element includes at least one of Ca, Sr, Ba, Al, Fe, B, Mg, Si, S, Ti, Cr, Fe, Cu, Zn, Ga, Zr, Mo, W, Nb, In, Sn, Pb, Sb, Ce, La, Ta or Hf, and the Q element includes at least one of F, Cl, Br, I, N or P.

7. The positive electrode material according to claim 1, wherein When an electrode including the positive electrode material is assembled into a button battery with lithium metal, and the button battery is charged and discharged at a current of 0.01C in a voltage range of 2.8V to 4.5V, the obtained voltage capacity differential dQ / dV curve has a first oxidation peak and a first reduction peak in the range of 4.2V to 4.5V, and the voltage capacity differential dQ / dV curve has a second oxidation peak and a second reduction peak in the range of 3.6V to 4.0V.

8. The positive electrode material according to claim 7, wherein The positive electrode material satisfies at least one of the following conditions: (1) The peak voltage of the first oxidation peak is Vo1, the peak voltage of the first reduction peak is Vr1, |Vo1-Vr1|≤0.1V; (2) The peak voltage of the second oxidation peak is Vo2, the peak voltage of the second reduction peak is Vr2, |Vo2-Vr2|≤0.1V; (3) When the button battery is charged and discharged at a current of 0.1C in the voltage range of 2.8V to 4.5V, the discharge curve in the obtained voltage-capacity curve has a platform in the range of 4.2V to 4.5V; (4) When the button battery is charged and discharged at a current of 0.1C in the voltage range of 2.8V to 4.5V, the capacity of the discharge curve in the range of 4.2V to 4.5V is Q1, and the capacity of the discharge curve in the range of 3.0V to 4.5V is Qt, and 0.2≤Q1 / Qt≤0.

3.

9. An electrochemical device comprising the positive electrode material according to any one of claims 1 to 8.

10. The electrochemical device according to claim 9, wherein: The electrochemical device further includes an electrolyte, wherein the electrolyte includes a boron-containing additive, and the boron-containing additive includes at least one of LiBOB, LiDFOB, and LiBF4.

11. The electrochemical device according to claim 10, wherein: Based on the mass of the electrolyte, the mass percentage of the boron-containing additive is 0.1% to 2%.

12. An electronic device comprising the electrochemical device according to any one of claims 9 to 11.

Citation Information

Cited By

  • Positive electrode material and preparation method thereof, electrochemical device and electronic device

    CN119542410A

  • Positive electrode material, positive electrode sheet, and secondary battery

    WO2026052148A1

  • Positive electrode material and battery

    WO2026057095A1

  • Positive electrode material, positive electrode sheet and battery

    WO2026103952A1

  • Positive electrode sheet and electrochemical device

    WO2026112827A1