Gas diffusion electrode for fuel cell
By using a carbon fiber conductive porous substrate and a microporous layer structure of fluoroalkyl chain fluororesin in the anode gas diffusion electrode of the fuel cell, the problem of carbon corrosion of the fuel cell in a fuel-deficient state is solved, and the power generation performance and power generation performance are improved. Durability and reduced costs.
Patent Information
- Application Number
- CN202380022071.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-18
- Filing Date
- 2023-02-09
- Publication Date
- 2024-10-01
AI Technical Summary
When the anode gas diffusion electrode of a fuel cell lacks fuel supply, carbon corrosion is prone to occur, resulting in reduced power generation performance. In addition, the cost of using rare metal catalysts in the existing technology is high and it is difficult to effectively inhibit carbon corrosion.
A gas diffusion electrode using a microporous layer structure composed of a carbon fiber conductive porous substrate and a fluororesin with a fluoroalkyl chain. By adjusting the specific surface area and content of carbon particles and fluororesin, the structure and resistivity of the microporous layer can be controlled. , inhibiting corrosion of carbon particles.
It effectively suppresses carbon degradation under low-temperature fuel starvation conditions, improves the long-term driving durability and power generation performance of the fuel cell, and reduces costs.
Smart Images

Figure BDA0004994934280000161 
Figure BDA0004994934280000171 
Figure BDA0004994934280000181
Abstract
Description
Technical Field
[0001] The present invention relates to a gas diffusion electrode used in a fuel cell, in particular a solid polymer fuel cell, and a fuel cell including the gas diffusion electrode. Background Art
[0002] For a solid polymer fuel cell that supplies a fuel gas containing hydrogen to an anode and an oxidizing gas containing oxygen to a cathode, and obtains an electromotive force through an electrochemical reaction occurring at both electrodes, it is generally composed of a power generation component called a stack, wherein a single cell (セル) composed of a separator, a gas diffusion electrode, a catalyst layer, an electrolyte membrane, a catalyst layer, a gas diffusion electrode, and a separator is stacked in sequence as a unit, and a plurality of single cells are stacked in series. Here, the three-layer portion of the catalyst layer, the electrolyte membrane, and the catalyst layer is called an electrolyte membrane with a catalyst layer (CCM: Catalyst Coated Membrane), and the five-layer portion including the gas diffusion electrodes arranged on both sides of the CCM is called a membrane electrode assembly (MEA: Membrane Electrode Assembly).
[0003] Gas diffusion electrodes require high gas diffusivity for diffusing the gas supplied from the separator to the catalyst layer, high drainage for discharging water generated by the electrochemical reaction to the separator, and high conductivity for extracting the generated current. Therefore, gas diffusion electrodes using a conductive porous substrate (hereinafter sometimes referred to as a "substrate") formed of conductive fibers such as carbon fibers and having a microporous layer (MPL: Micro Porous Layer) formed on the surface are widely used (Patent Documents 1 to 3).
[0004] In the operation of a normal fuel cell, the following reaction proceeds on the anode side.
[0005] H 2 →2H + +2e - (1)
[0006] In addition, the following reaction proceeds on the cathode side.
[0007] O 2 +4H + +4e - →2H 2 O (2).
[0008] Among them, part of the water generated on the cathode side sometimes penetrates the electrolyte membrane and moves to the anode side, increasing the humidity on the anode side. Moreover, when starting at low temperatures, water droplets condense and precipitate on the anode side to block the separator flow path, which sometimes hinders the supply of hydrogen. At this time, the single cell is in a fuel-deficient state and cannot continue to generate electricity. However, since other single cells in the stack other than this single cell continue to generate electricity, the fuel-deficient single cells connected in series with these power generation single cells act as a load of the fuel cell and apply a large voltage to their two poles. In this way, since a voltage in the opposite direction to that during normal power generation is applied to the two poles of the fuel-deficient single cell that is unable to generate electricity, it is usually called a reverse polarity (CR: Cell Reversal) state. At this time, the following two reactions occur on the anode side of the single cell to supply electrons.
[0009] 2H 2 O→O 2 +4H + +4e - (3)
[0010] C+2H 2 O→CO 2 +4H + +4e - (4).
[0011] Among them, reaction (3) is the electrolysis reaction of water, and reaction (4) is the electrochemical corrosion reaction of carbon. In particular, reaction (4) consumes the catalyst-supported carbon that is the constituent material of the anode catalyst layer, thereby causing serious performance degradation such as catalyst detachment and increase in contact resistance.
[0012] In this regard, there is a method that frequently monitors the voltage of each single cell constituting the stack, and if a sign of fuel deficiency is found, quickly suppresses the output, increases the hydrogen flow rate, etc., thereby avoiding the CR state. However, this method is related to the increase in the cost of the fuel cell system, so a material that suppresses the carbon corrosion reaction even in the CR state is required.
[0013] Therefore, in order to promote reaction (3) in the CR state, a method of promoting electrolysis of water is adopted. Specifically, it is known to mix iridium oxide and ruthenium oxide with platinum-supported carbon as an anode catalyst (Patent Document 4).
[0014] On the other hand, it is known that reaction (4) in the CR state proceeds not only in the anode catalyst layer but also on the carbon on the surface of the microporous layer of the anode gas diffusion electrode in contact with the anode catalyst layer. Therefore, the carbon of the anode gas diffusion electrode at the contact interface between the anode catalyst layer and the anode gas diffusion electrode also disappears, the contact resistance of the interface increases, and the power generation performance of the fuel cell unit deteriorates. In response to this, there is also a method of mixing the above-mentioned iridium oxide and ruthenium oxide in the anode gas diffusion electrode in the same way as the anode catalyst layer.
[0015] However, the materials used in these methods contain rare metals and are therefore expensive, which leads to a problem of increasing the cost of the fuel cell.
[0016] Furthermore, there is also a method of suppressing degradation by making the carbon used in the catalyst layer a highly crystalline material (Patent Document 5).
[0017] However, even in the case of carbon with good crystallinity, reaction (4) proceeds in the CR state, and thus a decrease in the cell voltage cannot be sufficiently suppressed.
[0018] Prior art literature
[0019] Patent Literature
[0020] Patent Document 1: Japanese Patent Application Publication No. 2014-011163
[0021] Patent Document 2: International Publication No. 2016 / 076132
[0022] Patent Document 3: International Publication No. 2015 / 125749
[0023] Patent Document 4: Japanese Patent Application Publication No. 2020-087644
[0024] Patent Document 5: International Publication No. 2020 / 059501 Summary of the invention
[0025] Problems to be solved by the invention
[0026] An object of the present invention is to provide a gas diffusion electrode in which carbon corrosion of an anode gas diffusion electrode of a fuel cell is suppressed from progressing and power generation performance of a single cell is not reduced even in a CR state caused by a lack of fuel supplied to the anode gas diffusion electrode.
[0027] Solutions to Solve Problems
[0028] The present invention for solving the above-mentioned problems provides the following gas diffusion electrode and fuel cell.
[0029] (1) A gas diffusion electrode comprising a conductive porous substrate containing carbon fibers as constituent materials and a microporous layer in contact with one surface of the conductive porous substrate, wherein the microporous layer contains carbon particles and a fluororesin having a fluoroalkyl chain as constituent materials, and when the specific surface area of the carbon particles is set to A (m 2 / g), the content of the carbon fine particles and the content of the fluororesin having a fluoroalkyl chain per unit volume in the microporous layer are respectively denoted as B (g / cm 3 )、C(g / cm 3 ), the value of the formula X shown below is 10 to 50,
[0030] A-30×(C / B)(Formula X).
[0031] (2) The gas diffusion electrode according to (1), wherein the value of the formula X is 10 to 28.
[0032] (3) The gas diffusion electrode according to (1) or (2), wherein the value of the formula X is 10 to 25.
[0033] (4) The gas diffusion electrode according to any one of (1) to (3), wherein the carbon particles are non-porous carbon particles.
[0034] (5) The gas diffusion electrode according to any one of (1) to (4), wherein the specific surface area of the carbon particles is 20 to 40 m 2 / g.
[0035] (6) The gas diffusion electrode according to any one of (1) to (5), wherein the melting point of the fluororesin having a fluoroalkyl chain is 200 to 300°C.
[0036] (7) The gas diffusion electrode according to any one of (1) to (6), wherein the arithmetic mean roughness of the surface on the microporous layer side of the gas diffusion electrode is 7 μm or less.
[0037] (8) A fuel cell using the gas diffusion electrode according to any one of (1) to (7) as an anode-side electrode of the fuel cell.
[0038] Effects of the Invention
[0039] The fuel cell incorporating the gas diffusion electrode of the present invention can suppress carbon degradation in the CR state under a fuel-deficient state even when started at low temperatures, so that no reduction in power generation performance is observed. Therefore, the durability of a practical vehicle during long-term driving is improved. DETAILED DESCRIPTION
[0040] The gas diffusion electrode of the present invention has a structure in which a microporous layer is formed on a conductive porous substrate. First, the conductive porous substrate will be described.
[0041] As the conductive porous substrate in the present invention, a porous substrate containing carbon fibers such as carbon fiber fabric, carbon fiber paper, carbon fiber nonwoven fabric, carbon felt, carbon paper, and carbon cloth can be used. Here, the so-called carbon paper refers to a sheet formed by bonding a carbon fiber paper with a resin carbide. Among them, carbon felt, carbon paper, and carbon cloth are preferably used due to their excellent corrosion resistance, and further, carbon paper is suitable for use due to the excellent characteristics of absorbing the dimensional change in the thickness direction of the electrolyte membrane, that is, "springiness".
[0042] As carbon fiber, polyacrylonitrile (PAN) system or pitch system, rayon system etc. can be cited. Among them, PAN system carbon fiber and pitch system carbon fiber are preferably used because of their excellent mechanical strength. In addition, natural fibers or synthetic fibers such as rayon fiber or acrylic fiber, cellulose fiber can also be mixed.
[0043] The average diameter of the single fiber of the carbon fiber is preferably 3 to 20 μm. If the average diameter is 3 μm or more, the pore diameter of the conductive porous substrate becomes larger, the drainage is improved, and overflow can be suppressed. On the other hand, if the average diameter is 20 μm or less, the water vapor diffusion becomes smaller, and drying can be suppressed. If the average diameter of the single fiber of the carbon fiber is 5 to 10 μm, these effects are improved, so it is more preferred.
[0044] The average length of the single fiber of the carbon fiber is preferably 3 to 20 mm. If the average length is 3 mm or more, the mechanical strength, electrical conductivity, and thermal conductivity of the conductive porous substrate become good. On the other hand, if the average length is 20 mm or less, the dispersibility of the carbon fiber during papermaking becomes good, and a homogeneous conductive porous substrate can be obtained. If the average length of the single fiber of the carbon fiber is 5 to 15 mm, these effects are improved, so it is more preferred.
[0045] The mass per unit area (weight per unit area) of the conductive porous substrate is preferably 20 to 50 g / m 2 If the unit area weight is 20g / m 2 On the other hand, if the weight per unit area is 50 g / m 2 If the weight per unit area of the conductive porous substrate is 30 to 40 g / m 2 , these effects are enhanced, so it is more preferred.
[0046] The weight per unit area of the conductive porous substrate can be adjusted by controlling the amount of the constituent material of the conductive porous substrate, that is, carbon fiber or resin carbide.
[0047] Conductive porous substrates are suitable for use with materials that have been waterproofed. Waterproofing is preferably performed using waterproof resins such as fluororesins with fluoroalkyl chains. As the above-mentioned fluororesins, PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene / hexafluoropropylene copolymer), PFA (tetrafluoroethylene / perfluoroalkyl vinyl ether copolymer), ETFE (tetrafluoroethylene / ethylene copolymer), PVDF (polyvinylidene fluoride), PVF (polyvinyl fluoride) etc. can be cited, but PTFE or FEP that show high waterproofness are preferred.
[0048] The amount of the waterproof resin is not particularly limited, and when the entire conductive porous substrate is set to 100 parts by mass, it is preferably 0.1 to 20 parts by mass. If it is within this range, the waterproof property can be fully exerted, and on the other hand, the waterproof resin can be inhibited from blocking the pores or resistance rise that become the gas diffusion path. In addition to the method of impregnating the conductive porous substrate in a dispersion of the waterproof resin, the method of applying the waterproof resin on the conductive porous substrate by die coating, spraying, etc. can also be applied. In addition, processing based on dry methods such as sputtering of fluororesin can also be applied. It should be noted that after the waterproof treatment, a drying process can also be added as needed, and then a heating process for wetting and spreading the waterproof resin into the substrate can be added.
[0049] In a solid polymer fuel cell, a gas diffusion electrode is required to have high gas diffusivity for diffusing the gas supplied from the separator to the catalyst and high drainage for discharging the water generated by the electrochemical reaction to the separator. Therefore, the conductive porous substrate preferably has a peak of pore diameter at 10 to 100 μm. The pore diameter and its distribution can be obtained by measuring the pore diameter distribution based on a mercury porosimeter. In order to obtain the pore diameter of the conductive porous substrate, only the conductive porous substrate can be measured, or the gas diffusion electrode after the microporous layer is formed can be measured. When measuring the gas diffusion electrode, the structure of each layer is confirmed by observing the vertical section (cross section parallel to the thickness direction) of the gas diffusion electrode with a scanning electron microscope (SEM), and the diameter of the pore part of the conductive porous substrate is roughly obtained by the SEM image. Next, while establishing a correspondence between the peaks of the multiple pore diameters obtained by the mercury porosimeter and the above-mentioned approximate values based on the SEM image, the pore diameter of the conductive porous substrate is determined.
[0050] In the present invention, the porosity of the conductive porous substrate is preferably 80 to 95%. If the porosity is 80% or more, gas diffusion is improved and power generation performance is improved. On the other hand, if the porosity is 95% or less, the mechanical strength of the conductive porous substrate is improved and the conductivity is also improved. If the porosity of the conductive porous substrate is 85 to 90%, these effects are improved, so it is more preferred. The porosity of the conductive porous substrate can be measured using a specific gravity meter or the like.
[0051] The thickness of the conductive porous substrate of the present invention is preferably 90 to 180 μm. Here, the thickness of the conductive porous substrate is the thickness when the two surfaces are clamped at a pressure of 0.15 MPa. If the thickness is 90 μm or more, the mechanical strength can be maintained and the operation in the manufacturing process is easy. In addition, the spring property becomes higher, the gas diffusion electrode can absorb the dimensional changes caused by the expansion / contraction of the electrolyte membrane during the use of the fuel cell, and the gas diffusivity in the in-plane direction becomes good, so the power generation performance is improved. On the other hand, if the thickness of the conductive porous substrate is less than 180 μm, the gas diffusivity in the vertical direction is improved, and the conductive path in the vertical direction is shortened, the conductivity becomes good, and thus the power generation performance is improved. If the thickness of the conductive porous substrate is 110 to 150 μm, these effects are improved, so it is more preferred.
[0052] Next, the microporous layer is described. In the present invention, the microporous layer is in contact with one surface of the conductive porous substrate, and the functions of the microporous layer include water management such as moisture retention of the electrolyte membrane or discharge of generated water, reduction of the interface resistance between the catalyst layer and the gas diffusion electrode, and suppression of electrolyte membrane damage caused by carbon fibers protruding from the conductive porous substrate.
[0053] The microporous layer is a layer containing carbon fine particles and a fluororesin having a fluoroalkyl chain.
[0054] In the microporous layer of the present invention, the specific surface area of the carbon particles is A (m 2 / g), the content of the carbon fine particles and the content of the fluororesin having a fluoroalkyl chain per unit volume in the microporous layer are respectively denoted as B (g / cm 3 )、C(g / cm 3 ), the value of A-30×(C / B) is 10 to 50. Preferably, it is 10 to 28, and more preferably, it is 10 to 25. Hereinafter, the calculation formula “A-30×(C / B)” is referred to as Formula X.
[0055] A-30×(C / B)(Formula X).
[0056] As described above, in the reverse polarity (CR) state, the electrochemical corrosion reaction of the carbon of the anode gas diffusion electrode shown in reaction (4) proceeds. Here, the carbon near the catalyst layer reacts most preferentially. Since the microporous layer of the gas diffusion electrode is in contact with the catalyst layer, the carbon present in the microporous layer, i.e., the carbon particles, corrode preferentially.
[0057] The inventors have found that the extent to which the surfaces of carbon particles present in the microporous layer are covered with the fluororesin having a fluoroalkyl chain affects the corrosion reaction of the carbon particles in the CR state, and that the above formula X is an indicator of the coating state of the carbon particles by the fluororesin having a fluoroalkyl chain.
[0058] If the value of formula X is 10 or more, the amount of fluororesin having a fluoroalkyl chain will not be too much, so the resistance of the gas diffusion electrode is kept low. On the other hand, if the value of formula X is 50 or less, the fluororesin having a fluoroalkyl chain covers the surface of the carbon particles, and the degradation of the carbon particles can be suppressed even in the CR state, so the degradation of the power generation performance can be suppressed. If the value of formula X is 28 or less, these effects are improved, so it is more preferred, and the value of formula X is further preferably 25 or less.
[0059] Furthermore, when porous carbon particles having pores formed inside the carbon particles are used, it becomes difficult for the fluororesin having a fluoroalkyl chain to penetrate into the pores of the carbon particles and sufficiently cover the surface of the carbon particles. Therefore, the carbon particles are preferably non-porous carbon particles having no pores formed inside.
[0060] The specific surface area of carbon particles can be measured by the BET method (JIS Z 830, ISO 9277) based on nitrogen adsorption. For example, the specific surface area of commercially available non-porous carbon particles based on the BET method is #3030B: 29 m 2 / g, #3050B: 50m 2 / g, #3230B: 200m 2 / g (all manufactured by Mitsubishi Chemical Corporation), "TOKABLACK (registered trademark)" #5500: 225m 2 / g, "TOKABLACK (registered trademark)" #4400: 50m 2 / g, "TOKABLACK (registered trademark)" #3800: 27m 2 / g (the above are manufactured by Tokai Carbon Co., Ltd.), "Vulcan (registered trademark)" 9A32: 140m 2 / g, "Vulcan (registered trademark)" XC-72: 232m 2 / g, "FCX (registered trademark)" 80: 77m 2 / g, (all manufactured by Cabot Corporation), "DENKA BLACK (registered trademark)" powdered product: 68m 2 / g, "DENKA BLACK (registered trademark)" FX35: 133m 2 / g, "DENKA BLACK (registered trademark)" HS-100: 39m 2 / g (the above are manufactured by DENKA Corporation) etc. The specific surface area of commercially available porous carbon particles by the BET method is "Blackpearls (registered trademark)" 2000: 1475 m 2 / g, (all manufactured by Cabot Corporation), "Ketjen Black (registered trademark)" EC300J: 800m 2 / g, "Ketjen Black (registered trademark)" EC600JD: 1200m 2 / g (the above are manufactured by LION SPECIALTY CHEMICALS Co., Ltd.) and the like.
[0061] Even when two or more types of carbon particles are used, the specific surface area can be obtained by calculating the total surface area and mass of all carbon particles. If the surface area is known for each particle, a known value can be used, and it can also be measured by the above-mentioned BET method.
[0062] As carbon particles, specifically, carbon black, carbon nanofiber, graphene etc. can be used. Among them, it is suitable to use cheap carbon black. In addition, carbon particles whose average crystal particle size is enlarged by heat treatment at high temperature in an inert gas are difficult to oxidize, so it is preferred.
[0063] The specific surface area of the carbon particles is preferably 20 to 40 m 2 / g. If the specific surface area of carbon particles is 20m 2 / g or more, the dispersibility of the carbon particles in the microporous layer coating liquid is improved, so a uniform microporous layer can be formed. In addition, since the moisture retention or drainage of the microporous layer is improved, the power generation performance is improved. In addition, if the specific surface area of the carbon particles is 40m 2 / g or less, the carbon corrosion reaction in the CR state of the gas diffusion electrode can be suppressed.
[0064] The content of fluororesin and carbon particles having a fluoroalkyl chain per unit volume in the microporous layer can be measured by mass spectrometry. First, the content of fluororesin having a fluoroalkyl chain in the microporous layer is determined by analyzing the degassing components when the microporous layer is heated to 1000°C in a He atmosphere to decompose and remove the resin component. Next, the content of carbon particles can be determined based on the mass of the residue after the thermal decomposition treatment. By dividing them by the volume of the microporous layer to be measured, the content per unit volume can be calculated. In addition, by analyzing the residue using the above-mentioned BET method, the specific surface area of the carbon particles can be calculated.
[0065] Furthermore, fibrous non-porous carbon particles such as carbon nanofibers form a conductive path inside the microporous layer, thereby having an effect of reducing the electrical resistance of the microporous layer.
[0066] The fluororesin having a fluoroalkyl chain contained in the above-mentioned microporous layer is the same as the fluororesin having a fluoroalkyl chain that is suitable for use when the conductive porous substrate is subjected to water-repellent treatment, and examples thereof include PTFE (polytetrafluoroethylene; melting point 327°C), FEP (tetrafluoroethylene / hexafluoropropylene copolymer; melting point 260°C), PFA (tetrafluoroethylene / perfluoroalkyl vinyl ether copolymer; melting point 305°C), ETFE (tetrafluoroethylene / ethylene copolymer; melting point 265°C), PVDF (polyvinylidene fluoride; melting point 177°C), PVF (polyvinyl fluoride; melting point 190°C), and the like.
[0067] The melting point of the fluororesin having a fluoroalkyl chain is preferably 200 to 300°C. If the melting point of the fluororesin having a fluoroalkyl chain is above 200°C, the fluororesin having a fluoroalkyl chain can be inhibited from moving together with the solvent in the drying process after the microporous layer is coated, and the fluororesin having a fluoroalkyl chain can be uniformly present inside the microporous layer. In addition, if the melting point of the fluororesin having a fluoroalkyl chain is below 300°C, during the heat treatment after the microporous layer is coated / dried, the fluororesin having a fluoroalkyl chain melts rapidly and wets and spreads into the microporous layer, thereby improving the water resistance of the microporous layer. If the melting point of the fluororesin having a fluoroalkyl chain is 230 to 270°C, these effects are enhanced, so it is more preferred. The melting point of the fluororesin having a fluoroalkyl chain can be obtained by measuring the temperature at which the substance melts when the temperature is gradually increased. For example, it can be determined by measuring the temperature showing an endothermic peak when the temperature is increased from room temperature to 400° C. at a rate of 10° C. / min in a nitrogen atmosphere using a differential scanning calorimeter.
[0068] Generally, fluororesins having fluoroalkyl chains are insoluble in water, organic solvents, etc., so when preparing a coating solution for forming a microporous layer, it is preferred to use a dispersion of fluororesins having fluoroalkyl chains processed into microparticles. Examples of dispersions of fluororesins having fluoroalkyl chains in microparticle form include "Polyflon (registered trademark)" D-210C, ND-110 (manufactured by Daikin Industries, Ltd.), 120-JRB, 31-JR (manufactured by Chemours-Mitsui Fluoroproducts Co., Ltd.), etc.
[0069] In addition, in the microporous layer of the present invention, in addition to the fluororesin having a fluoroalkyl chain, a waterproof resin such as a fluororesin without a fluoroalkyl chain and a silicone resin having a siloxane bond may also be contained. Furthermore, a thermosetting resin may also be contained. Examples of the thermosetting resin include phenolic resin, epoxy resin, acrylate resin, furan resin, and the like.
[0070] Furthermore, the microporous layer may contain microparticles of iridium oxide, ruthenium oxide, titanium oxide, etc., which promote the electrolysis of water in the reverse polarity (CR) state when hydrogen is deficient. In addition, microparticles of cerium oxide, manganese oxide, etc., which are used to deactivate hydroxide radicals generated at the anode electrode, may also be contained.
[0071] The microporous layer of the present invention preferably has a weight per unit area of 10 to 35 g / m 2 If the unit area weight of the microporous layer is 10g / m 2 The above method is preferred because it can cover the carbon fibers protruding from the surface of the conductive porous substrate, thereby preventing the carbon fibers from damaging the electrolyte membrane. In addition, it is preferred because it can reduce the contact resistance between the gas diffusion electrode and the catalyst layer and prevent the electrolyte membrane from drying. In addition, if the unit area weight of the microporous layer is 35 g / m 2 If the weight per unit area of the microporous layer is 15 to 25 g / m 2 , these effects are enhanced, so it is more preferred.
[0072] The surface of the microporous layer of the present invention preferably has few unevenness, cracks, pinholes, etc. If these defects are few and the surface is smooth, in addition to improving the durability of the microporous layer, the resistance and thermal resistance of the interface between the microporous layer and the electrolyte membrane with the catalyst layer are reduced. In addition, since the frequency of contact between the carbon particles in the microporous layer and water is reduced, the corrosion reaction of the above-mentioned carbon particles can be suppressed. The index of the smoothness of the surface of the microporous layer, i.e., the arithmetic mean roughness (Ra), is preferably less than 7μm. Ra can be measured using a laser microscope. For example, a laser microscope "VK-X3000" (made by Keyence Corporation) can be used to measure the 5mm length of the uneven profile at any part on the surface, and the average value is calculated as Ra. On the other hand, if Ra is more than 1μm, it is easy to replenish the generated water in the concave part present on the surface of the microporous layer, and the interface of the catalyst layer in contact with the surface of the microporous layer is moisturized, and the catalyst activity is improved, so it is preferred.
[0073] The thickness of the gas diffusion electrode of the present invention is preferably 90 to 200 μm. Here, the thickness of the gas diffusion electrode is the thickness when the two surfaces are clamped at a pressure of 0.15 MPa. If the thickness of the gas diffusion electrode is 90 μm or more, the mechanical strength is maintained and the handling in the manufacturing process is easy. On the other hand, if the thickness of the gas diffusion electrode is 200 μm or less, the gas diffusion property is improved and the resistance is reduced, so the power generation performance of the fuel cell is improved. If the thickness of the gas diffusion electrode is 110 to 170 μm, these effects are improved, so it is more preferred. The thickness of the gas diffusion electrode can be adjusted by appropriately adjusting the thickness of the conductive porous substrate and the microporous layer.
[0074] Next, an example of a method for producing a gas diffusion electrode according to the present invention will be described in detail.
[0075] First, a carbon fiber bundle cut to a predetermined length is untied in water to produce a uniformly dispersed carbon fiber dispersion, which is picked up and dried to produce a carbon fiber paper body. Here, the carbon fiber dispersion may contain a surfactant, a thickener, or a defoaming agent, and may also contain a water-soluble resin to maintain the shape of the carbon fiber paper body. As the water-soluble resin, polyvinyl alcohol or polyvinyl acetate may be used.
[0076] In the case of continuous papermaking in long strips, the carbon fibers can be oriented in the length direction by increasing the speed of the papermaking web, and the elastic modulus of the carbon fibers in the orientation direction becomes higher. When manufacturing a fuel cell unit, if the carbon fibers of the gas diffusion electrode are arranged in a manner orthogonal to the separator flow path, the gas diffusion electrode can be prevented from being pressed into the groove of the flow path, thereby improving drainage.
[0077] The carbon fiber paper body obtained above can also be used as the conductive porous substrate of the present invention, but in order to improve the mechanical strength and reduce the electrical resistance, it is preferred to bond the intersections between the carbon fibers with a resin carbide.
[0078] For this purpose, for example, a method can be applied in which a carbon fiber paper base is immersed in a resin composition solution and then subjected to a heat treatment to carbonize the resin component in the resin composition.
[0079] As the resin used in the resin composition solution, thermosetting resins such as phenolic resins, epoxy resins, melamine resins, and furan resins can be cited. In addition to the resin component and the solvent, the resin composition solution can also contain carbon powder or surfactants. As the carbon powder, carbon black or graphite, black lead, carbon nanotubes, carbon nanofibers, etc. can be cited.
[0080] Examples of methods for impregnating the resin composition solution include dipping, spraying, knife coating, die coating, transfer, etc. By adjusting the impregnation method, a gradient distribution of the amount of the resin composition in the thickness direction of the substrate can be formed.
[0081] Next, the substrate impregnated with the resin composition solution is dried in air at a temperature of 80°C to 150°C. Next, the thermosetting resin is cured and the surfactant and the like are decomposed and removed by heating in air at a temperature of 200°C to 300°C. At this time, the flatness of the substrate can be improved and the thickness can be adjusted by pressing both sides of the substrate with a flat plate.
[0082] Furthermore, in order to improve the conductivity of the substrate and improve long-term durability, it is preferred to carbonize the cured resin composition at a temperature of 1000° C. to 2400° C. in an inert atmosphere such as nitrogen. Here, if a pre-carbonization treatment is performed at a temperature of 300° C. to 1000° C. in an inert atmosphere before the carbonization treatment to decompose and remove impurities and to approach the crystal structure of graphite in advance, the crystallinity during the carbonization treatment is improved, and the above-mentioned performance is improved, so it is preferred.
[0083] The substrate thus obtained can have sufficient conductivity as a conductive porous substrate for a gas diffusion electrode of a fuel cell.
[0084] Furthermore, in order to improve the drainage of the conductive porous substrate, a waterproof treatment may be performed. The waterproof treatment is to immerse the substrate in a liquid containing a waterproof resin, dry it, and appropriately perform a heating treatment to wet and spread the waterproof resin to the inside of the substrate, thereby obtaining a conductive porous substrate with the waterproof resin attached to the inside. As the waterproof resin, the same resin as the fluororesin contained in the above-mentioned microporous layer can be used. In addition, a liquid obtained by diluting a dispersion of a microparticle-like waterproof resin to a specified concentration can also be used as the liquid containing the waterproof resin.
[0085] In this manner, the conductive porous substrate of the present invention can be obtained.
[0086] Next, a method for forming a microporous layer on a conductive porous substrate will be described.
[0087] The microporous layer can be formed by applying a coating solution in which carbon particles and a fluororesin having a fluoroalkyl chain are dispersed in a solvent such as water on a conductive porous substrate, and then heating the coating solution. Here, the composition ratio of the carbon particles to the fluororesin having a fluoroalkyl chain needs to be determined so that the value of the above formula X is 10 to 50.
[0088] When making a coating liquid for forming a microporous layer, if a dispersant, a thickener, etc. are added to the liquid, the dispersion stability of carbon particles and fluororesins with fluoroalkyl chains is improved, so it is preferred. As a dispersant, from the aspect of less metal components, a non-ionic surfactant is preferably used, and particularly preferably a polyoxyalkylene aryl ether "TRITON (registered trademark)" X-100 (manufactured by Nacalai Tesque Co., Ltd.) of which the dispersion stability of the coating liquid becomes higher and the surface smoothness of the obtained microporous layer is good. In addition, in order to keep the coating liquid at a high viscosity, it is effective to add a thickener. As a thickener, for example, methylcellulose, polyethylene glycol, polyvinyl alcohol, etc. can be used appropriately.
[0089] For these dispersants and thickeners, the same substance may have two functions, or raw materials suitable for each function may be selected. However, when the thickener and dispersant are selected separately, it is preferred to select a thickener that does not impair the dispersibility of the carbon particles and the dispersibility of the fluororesin having a fluoroalkyl chain.
[0090] Furthermore, if necessary, fine particles of iridium oxide, ruthenium oxide, titanium oxide, etc. for promoting electrolysis of water, and fine particles of cerium oxide, manganese oxide, etc. for inactivating radicals are added.
[0091] The above mixture is kneaded using a homogenizer, a planetary mixer, an ultrasonic disperser or the like to obtain a coating liquid for forming a microporous layer.
[0092] The coating liquid for forming the microporous layer can be applied to the conductive porous substrate using various commercially available coating devices. As the coating method, screen printing, rotary screen printing, gravure printing, gravure printing, spray coating, die coating, rod coating, doctor blade coating, roller blade coating, etc. can be used.
[0093] After the microporous layer is coated on the conductive porous substrate, the coating liquid is dried at a temperature of 60°C to 150°C, and then heated at a temperature of 250°C to 380°C to promote the decomposition and removal of additives such as dispersants and thickeners and the melting of fluororesins with fluoroalkyl chains. At this time, not only the fluororesins with fluoroalkyl chains in the microporous layer are melted, but also the waterproof resin attached to the conductive porous substrate is melted, and they wet and spread on the surface of carbon fibers, resin carbides, carbon particles, etc., which are other constituent materials. As a result, the drainage of the conductive porous substrate and the microporous layer is enhanced, so the performance of the fuel cell using it is improved.
[0094] In this way, a gas diffusion electrode having a microporous layer formed on a conductive porous substrate is obtained.
[0095] The gas diffusion electrode of the present invention is particularly preferably used as an anode electrode. The membrane / electrode assembly (MEA) is prepared by bonding the microporous layer side surface of the gas diffusion electrode of the present invention to one side surface of an electrolyte membrane (CCM) having catalyst layers on both sides, and bonding the microporous layer side surface of a separately prepared cathode gas diffusion electrode on the opposite side of the CCM. Here, the gas diffusion electrode of the present invention can also be used in the cathode gas diffusion electrode.
[0096] Furthermore, the obtained MEA is sandwiched from both sides with two separators for the anode and cathode, each of which has a gas flow path, to produce a fuel cell unit. At this time, the MEA is set to be one size smaller than the outer periphery of the two separators. If the gasket is arranged to surround the outside of the MEA, when the separator applies pressure to clamp the MEA, the MEA is fixed in a state of being compressed to an appropriate thickness. By adjusting the thickness of the gasket, the power generation unit cell ( The thickness of the MEA in the cell can be adjusted to optimize performance in accordance with the purpose of power generation.
[0097] In the flow path of the separator, an inlet / outlet for supplying hydrogen is provided on the anode side, and an inlet / outlet for supplying air is provided on the cathode side. In addition, since the separator is made of conductive materials such as stainless steel or carbon, electricity can be taken in and out by connecting electrical wiring. Furthermore, by providing a passage inside the separator for supplying circulating water, the single cell can be maintained at a specified temperature.
[0098] By preparing a set of about 200 to 500 fuel cell units thus manufactured and connecting them in series, a high voltage of 40 kV to 200 kV can be generated, and such a fuel cell stack can be used as a power source for fuel cell vehicles and the like.
[0099] Example
[0100] The present invention will be specifically described below by way of examples. The following describes methods for preparing materials used in the examples and methods for evaluating the cell performance of fuel cells.
[0101] <Method for producing conductive porous substrate>
[0102] Toray Industries, Inc. manufactured polyacrylonitrile carbon fiber "TORAYCA (registered trademark)" T300 (average fiber diameter: 7 μm) cut into 12 mm lengths, dispersed in water and continuously made into paper, and then sprayed with a 10% by mass aqueous solution of polyvinyl alcohol and dried to obtain a weight per unit area of 20 g / m 2 The amount of the polyvinyl alcohol attached was 20 parts by mass relative to 100 parts by mass of the papermaking body.
[0103] Next, a resin composition solution was prepared by mixing flaky graphite (average particle size: 5 μm), phenolic resin (a mixture of resol-type phenolic resin and novolac-type phenolic resin in a mass ratio of 1:1), and methanol in a mass ratio of 5:10:85. The resin composition solution was continuously applied by spraying on the carbon fiber paper body so that the total amount of phenolic resin and flaky graphite was 130 parts by mass relative to 100 parts by mass of carbon fibers in the substrate, and dried at 100° C. for 5 minutes.
[0104] Next, the substrate with the resin composition attached was sandwiched between upper and lower hot plates in a press molding machine and heated and compressed at 180°C for 5 minutes. Here, a release paper was placed between the substrate and the hot plate to prevent the hot plate from adhering to the substrate. In addition, spacers were arranged around the upper and lower hot plates to adjust the thickness of the substrate after heating and compression. Then, the substrate was heated at 2400°C in a heating furnace under a nitrogen atmosphere and carbonized.
[0105] Furthermore, a water-repellent resin dispersion prepared by mixing 5 parts by mass of a dispersion of PTFE fine particles ("Polyfion (registered trademark)" D-210C manufactured by Daikin Industries, Ltd.) and 95 parts by mass of ion-exchanged water was sprayed and dried at 100°C for 5 minutes to obtain a film having a thickness of 150 μm and a weight per unit area of 40 g / m at 0.15 MPa. 2 Conductive porous substrate.
[0106] <Method for measuring the arithmetic mean roughness of the gas diffusion electrode surface>
[0107] The arithmetic mean roughness (Ra) of the microporous layer side surface of the gas diffusion electrode over a length of 5 mm was measured using a laser microscope "VK-X3000" (manufactured by KEYENCE Corporation). Ra was measured at four random locations on a 30 mm x 30 mm test piece, and the average value was calculated.
[0108] <Evaluation of power generation performance>
[0109] The specified gas diffusion electrodes prepared in each embodiment / comparative example are arranged on the anode side and cathode side of the electrolyte membrane / catalyst layer integrated product (for the electrolyte membrane "GORE-SELECT (registered trademark)" manufactured by Japan GORE Contract Co., Ltd., the catalyst layer "PRIMEA (registered trademark)" manufactured by Japan GORE Contract Co., Ltd. is formed on both sides) in such a way that the microporous layer and the catalyst layer are in contact, and a membrane electrode assembly (MEA) is prepared by hot pressing at a pressure of 0.1 MPa and 130°C for 20 minutes. The MEA is installed in a single cell for a fuel cell, and hydrogen is supplied to the anode side and air is supplied to the cathode side at a temperature of 70°C for the single cell, and the pressure is 1A / cm 2 The current density is maintained for 3 hours of power generation. At this time, the fuel utilization efficiency is 70%, the air utilization efficiency is 40%, and the dew points of hydrogen on the anode side and air on the cathode side are 59°C (relative humidity: 60%) and 60°C, respectively, and then humidified and introduced into the single cell. The voltage value at the time of 3 hours is read as the power generation voltage, which is used as an indicator of power generation performance.
[0110] <Cell Reversal Tolerance (CRT)>
[0111] After the above-mentioned <Evaluation of Power Generation Performance>, the anode side was switched from hydrogen to nitrogen, and 200 mA / cm was applied to the nitrogen via a potentiostat so that the nitrogen flowed from the anode side to the cathode side. 2 The low current is applied to the single cell to put it in a reverse polarity state (reverse potential state) and measure the single cell voltage. The holding time from the start of application to the time when the single cell voltage falls below -1.5V is defined as the CRT time.
[0112] <Carbon Particles for Microporous Layer Used in Examples>
[0113] Carbon particles A: "TOKABLACK (registered trademark)" #3800 (manufactured by Tokai Carbon Co., Ltd.; specific surface area 27 m 2 / g)
[0114] Carbon particles B: "TOKABLACK (registered trademark)" #4400 (manufactured by Tokai Carbon Co., Ltd.; specific surface area 50 m 2 / g)
[0115] Carbon particles C: "DENKA Black (registered trademark)" HS-100 (manufactured by DENKA Corporation: specific surface area 39 m 2 / g)
[0116] Carbon particles D: "DENKA Black (registered trademark)" powder (manufactured by DENKA Corporation: specific surface area 68 m 2 / g)
[0117] Carbon particles E: "Vulcan (registered trademark)" 9A32 (manufactured by Cabot Corporation: specific surface area 140 m 2 / g)
[0118] Carbon particles F: "Vulcan (registered trademark)" XC-72 (manufactured by Cabot Corporation: specific surface area 232 m 2 / g).
[0119] (Example 1)
[0120] Carbon particles A were used as carbon particles, PTFE was used as a fluororesin having a fluoroalkyl chain, "TRITON (registered trademark)" X-100 (manufactured by Nacalai Tesque Co., Ltd.) of a polyoxyalkylene aryl ether system was used as a dispersant, and water was used as a dispersion medium. The mixing ratio was set to carbon particles / fluororesin having a fluoroalkyl chain / dispersant = 75 parts by mass / 25 parts by mass / 150 parts by mass, and the coating liquid for forming the microporous layer was adjusted so that the non-decomposed components (carbon particles and fluororesin having a fluoroalkyl chain) were 23% by mass relative to the total amount. Here, a dispersion liquid "Polyflon (registered trademark)" D-210C (manufactured by DAIKIN Industries Co., Ltd.) in which PTFE particles were dispersed in water was used as a supply source of PTFE. In addition, when adjusting the coating liquid, a planetary mixer was used to disperse the raw materials so that the coating liquid composition became uniform. At this time, the value of formula X was calculated to be 17.
[0121] A-30×(C / B)(Formula X).
[0122] The above-mentioned coating liquid for forming a microporous layer was applied to the conductive porous substrate produced as described in the above-mentioned <Method for producing a conductive porous substrate> using a die coater, dried at 100°C for 10 minutes, and then heated at 350°C for 10 minutes to promote the adhesion of the fluororesin having a fluoroalkyl chain and the carbon particles and to decompose and remove the dispersant, thereby producing a gas diffusion electrode. Here, the coating amount was adjusted so that the unit area weight of the microporous layer after heating would be 20 g / cm 2 It should be noted that the fluororesin having a fluoroalkyl chain was not decomposed during heating at 350° C. for 10 minutes.
[0123] The arithmetic mean roughness of the surface of the microporous layer of the obtained gas diffusion electrode was 6 μm.
[0124] Next, the obtained gas diffusion electrode was used for both anode and cathode to evaluate the power generation performance, which was 0.58 V. In addition, the CRT evaluation was performed, which showed that the retention time was 50 hours.
[0125] (Examples 2 to 14, Comparative Examples 1 to 6)
[0126] A coating liquid for forming a microporous layer was prepared in the same manner as in Example 1, except that the types and mass fractions of each component were as shown in Tables 1 to 3, and a gas diffusion electrode was obtained by coating the coating liquid on a conductive porous substrate. It should be noted that for Examples 11 to 14 and Comparative Examples 5 to 6, a dispersion liquid "Polyflon" (registered trademark) ND-110 (manufactured by DAIKIN Industries, Ltd.) in which FEP particles are dispersed in water was used as a source of FEP. The obtained gas diffusion electrode was used to evaluate the power generation performance and CRT. The results are shown in Tables 1 to 3. In addition, for Comparative Example 2, Example 1 of Patent Document 1 was used as a reference. In addition, for Comparative Example 3, Example 1 of Patent Document 2 was used as a reference, and for Comparative Example 4, Comparative Example 1 of Patent Document 3 was used as a reference.
[0127]
[0128]
[0129]
[0130] (Example 15)
[0131] Carbon particles C were used as carbon particles, PTFE was used as a fluororesin having a fluoroalkyl chain, "Emulgen" 430 (manufactured by Kao Corporation) of a polyoxyalkylene alkyl ether system was used as a dispersant A, "Unilife (registered trademark)" 70DP-950B (manufactured by NOF Corporation) was used as a dispersant B, and water was used as a dispersion medium. The mixing ratio was set to carbon particles / PTFE / dispersant A / dispersant B = 100 parts by mass / 45 parts by mass / 90 parts by mass / 90 parts by mass, and the coating liquid for forming the microporous layer was adjusted so that the non-decomposed components (carbon particles and fluororesin having a fluoroalkyl chain) were 23% relative to the total amount. Here, a dispersion liquid "Polyflon (registered trademark)" D-210C (manufactured by Daikin Industries, Ltd.) in which PTFE particles were dispersed in water was used as a supply source of PTFE. In addition, when adjusting the coating liquid, a planetary mixer was used to disperse the raw materials so that the coating liquid composition became uniform. At this time, the value of formula X is calculated to be 26.
[0132] A-30×(C / B)(Formula X).
[0133] The above-mentioned coating liquid for forming a microporous layer was applied to the conductive porous substrate produced as described in the above-mentioned <Method for producing a conductive porous substrate> using a die coater, dried at 100°C for 10 minutes, and then heated at 350°C for 10 minutes to promote the adhesion of the fluororesin having a fluoroalkyl chain and the carbon particles and to decompose and remove the dispersant, thereby producing a gas diffusion electrode. Here, the coating amount was adjusted so that the unit area weight of the microporous layer after heating would be 20 g / cm 2 It should be noted that the fluororesin having a fluoroalkyl chain was not decomposed during heating at 350° C. for 10 minutes.
[0134] The arithmetic mean roughness of the surface of the microporous layer of the obtained gas diffusion electrode was 8 μm.
[0135] Next, the obtained gas diffusion electrode was used for both anode and cathode to evaluate the power generation performance, which was 0.60 V. In addition, the CRT evaluation was performed, which showed that the retention time was 38 hours.
Claims
1. A gas diffusion electrode comprising a conductive porous substrate containing carbon fibers as a constituent material and a microporous layer in contact with one surface of the conductive porous substrate, wherein: The microporous layer comprises carbon particles and a fluororesin having a fluoroalkyl chain as constituent materials, and when the specific surface area of the carbon particles is set to A (m 2 / g), the content of the carbon fine particles and the content of the fluororesin having a fluoroalkyl chain per unit volume in the microporous layer are respectively denoted as B (g / cm 3 )、C(g / cm 3 ), the value of the formula X shown below is 10 to 50, A-30×(C / B)(Formula X).
2. The gas diffusion electrode according to claim 1, wherein: The value of the formula X is 10-28.
3. The gas diffusion electrode according to claim 1, wherein: The value of the formula X is 10-25.
4. The gas diffusion electrode according to claim 1 or 3, wherein: The carbon particles are non-porous carbon particles.
5. The gas diffusion electrode according to claim 1 or 3, wherein: The specific surface area of the carbon particles is 20 to 40 m 2 / g.
6. The gas diffusion electrode according to claim 1 or 3, wherein: The melting point of the fluororesin having a fluoroalkyl chain is 200 to 300°C.
7. The gas diffusion electrode according to claim 1 or 3, wherein: The arithmetic mean roughness of the microporous layer-side surface of the gas diffusion electrode is 7 μm or less.
8. A fuel cell using the gas diffusion electrode according to claim 1 or 3 as an anode-side electrode of the fuel cell.
Citation Information
Patent Citations
Carbon substrate for gas diffusion layer, gas diffusion layer using the same, and electrode for fuel cell including the gas diffusion layer
JP2014011163A
Anode catalyst for hydrogen deficiency resistant fuel cell
JP2020087644A
Gas diffusion electrode substrate, and membrane electrode assembly and fuel cell equipped with same
WO2015125749A1
Gas diffusion electrode base and method for producing gas diffusion electrode base
WO2016076132A1
JP特开2020/059501