Magnetic nano-hybridized uricase with adjustable activity as well as preparation method and application of magnetic nano-hybridized uricase
Through the amide bond connection of magnetic nanohybrid uricase and the control of alternating magnetic field, the reversible control of uricase activity is achieved, which solves the problem of uncontrolled activity of uricase in treating gout, improves the therapeutic effect and safety, and efficiently ablates MSU crystals. , relieve joint inflammation.
Patent Information
- Application Number
- CN202410820379.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-08
AI Technical Summary
The activity of existing uricase in treating gout is uncontrolled, making it difficult to balance efficacy and safety, resulting in fluctuations in uric acid levels and toxic side effects.
A magnetic nanohybrid uricase with controllable activity is used to connect the amide bond of uricase with a carboxylated vortex magnetic ferric oxide nanoring, and an alternating magnetic field is used to control the activity of CAT enzyme to achieve reversible activity of uricase. control.
By driving the activity of CAT nanozyme through magnetic heat, the external magnetic field can activate or silence uricase, effectively maintain uric acid at normal levels, avoid fluctuations, improve the efficacy and safety of gout treatment, efficiently ablate MSU crystals, and relieve joint inflammation.
Smart Images

Figure CN118743754A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of pharmaceutical preparations, and in particular relates to a magnetic nano-hybrid uricase with adjustable activity, and a preparation method and application thereof. Background Art
[0002] Gout is a common arthritis disease caused by abnormal uric acid metabolism. With the development of refined life, the number of gout patients in my country has exceeded 80 million, and is still growing at an annual rate of 9.7%. It is estimated that the number of gout patients will reach 240 million in 2030, which is a health warning that cannot be ignored. Gout is characterized by persistent hyperuricemia, deposition of monosodium urate (MSU) crystals in the periarticular structures, causing synovial inflammation and severe pain, which seriously threatens the health of contemporary Chinese people.
[0003] In recent years, catalytic therapy that intervenes in uric acid metabolism levels by supplementing uricase has become an emerging strategy for the treatment of gout. For example, Pegloticase is currently the only protease drug approved by the FDA (Food and Drug Administration) for the treatment of chronic refractory gout. It can catalyze uric acid to convert it into more water-soluble allantoin and excrete it with urine, which can more quickly reduce uric acid levels and dissolve MSU crystals. In order to improve the therapeutic effect of uricase, many studies have co-loaded UOX (urate oxidase) and CAT enzyme (catalase) into nano-delivery systems to improve the stability of enzyme molecules and reduce the toxic side effects of H2O2 through cascade catalysis, or encapsulate enzyme molecules with cell membranes to further prolong their retention time in the body and enhance their activity.
[0004] However, after these catalysts reach the human body, their activity is uncontrolled, making it difficult to balance safety and effectiveness: if the activity is too low, the efficacy is insufficient; if the activity is too high, it will overreact and cause toxic side effects such as hypouricemia. Therefore, how to control the activity of uricase in the body on demand and reversibly is an urgent problem to be solved in order to achieve precise gout treatment. Summary of the invention
[0005] In order to solve the above problems existing in the prior art, the present invention provides an activity-regulatable magnetic nano-hybrid uricase and a preparation method and application thereof. The technical problem to be solved by the present invention is achieved by the following technical solutions:
[0006] The present invention provides a method for preparing a magnetic nano-hybrid uricase with adjustable activity, comprising:
[0007] S1: taking a predetermined amount of carboxylated vortex magnetic ferroferric oxide nanorings, adding morpholineethanesulfonic acid solution, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride solution and N-hydroxysuccinimide solution in sequence, reacting sufficiently to activate the carboxyl groups on the surface of the carboxylated vortex magnetic ferroferric oxide nanorings, and obtaining vortex magnetic ferroferric oxide nanorings after carboxyl group activation;
[0008] S2: adding a predetermined amount of phosphate buffered saline solution, urate oxidase and deionized water to the vortex magnetic ferroferric oxide nanoring after the carboxyl group activation, and reacting them sufficiently so that the carboxyl group on the surface of the vortex magnetic ferroferric oxide nanoring is connected to the amino group on the surface of the urate oxidase in the form of an amide bond;
[0009] S3: After the reaction is completed, the reaction solution is centrifuged and washed to obtain the activity-regulatable magnetic nano-hybrid uricase.
[0010] In one embodiment of the present invention, the mass ratio of the carboxylated vortex magnetic ferroferric oxide nanoring to the uricase is (1:0.1) to (1:10).
[0011] In one embodiment of the present invention, the S1 includes:
[0012] A predetermined amount of carboxylated vortex magnetic ferroferric oxide nanorings is placed in a centrifuge tube;
[0013] Selecting predetermined amounts of morpholineethanesulfonic acid powder, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride powder and N-hydroxysuccinimide powder and respectively proportioning them into solutions, wherein the mass ratio of the ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride powder to the N-hydroxysuccinimide powder is 1:1.5, and the pH value of the proportioned morpholineethanesulfonic acid solution is 6, and the concentration is 25 mmol / L;
[0014] Adding morpholineethanesulfonic acid solution, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride solution and N-hydroxysuccinimide solution into the centrifuge tube in sequence, shaking and reacting at room temperature for 10 to 40 minutes to activate the carboxyl groups on the surface of the carboxylated vortex magnetic ferrosoferric oxide nanorings;
[0015] Magnetic separation technology is used to separate the carboxyl-activated vortex magnetic ferroferric oxide nanoring liquid, and the mixed solution of morpholineethanesulfonic acid, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride and N-hydroxysuccinimide in the upper layer is discarded to obtain the carboxylated vortex magnetic ferroferric oxide nanoring after carboxyl activation.
[0016] In one embodiment of the present invention, the S2 includes:
[0017] Adding a predetermined amount of phosphate buffered saline solution, urate oxidase and deionized water to the vortex magnetic ferrosoferric oxide nanorings after carboxyl activation, and ultrasonically dispersing to form a dispersed solution, wherein the concentration of the added phosphate buffered saline solution is 0.1 mol / L;
[0018] The dispersed solution is placed on a shaker and reacted at 4-25° C. for 1-5 hours, so that the carboxyl groups on the surface of the vortex magnetic ferroferric oxide nanorings after carboxyl group activation are connected to the amino groups on the surface of the urate oxidase in the form of amide bonds.
[0019] In one embodiment of the present invention, the preparation method further comprises: regulating the CAT enzyme activity in the activity-regulatable magnetic nanohybrid uricase by an alternating magnetic field.
[0020] In one embodiment of the present invention, the alternating magnetic field has a frequency of 100 kHz to 1 MHz and a magnetic field strength of 0 to 500 Oe.
[0021] Another aspect of the present invention provides an activity-regulatable magnetic nanohybrid uricase, which is prepared by the preparation method described in any one of the above embodiments, and the magnetic nanohybrid uricase comprises a composite material of carboxylated vortex magnetic ferroferric oxide nanorings and uricase oxidase.
[0022] In one embodiment of the present invention, the size of the carboxylated vortex magnetic ferroferric oxide nanorings is 40 to 300 nm.
[0023] In one embodiment of the present invention, in the magnetic nanohybrid uricase, the mass ratio of the carboxylated vortex magnetic ferroferric oxide nanoring and the uricase oxidase is 0.1:10, and the carboxylated vortex magnetic ferroferric oxide nanoring and the uricase oxidase are connected via an amide bond.
[0024] Another aspect of the present invention provides an application of an activity-regulatable magnetic nanohybrid uricase in maintaining uric acid homeostasis, ablating MSU crystals, and alleviating gouty joint damage and inflammation.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] In the magnetic nanohybrid uricase with adjustable activity of the present invention, the magnetic induction heat mediated by Fe3O4 NR can drive the CAT nanozyme of Fe3O4 NR to produce oxygen to activate uricase, and realize the reversible regulation of the alternating magnetic field on the uric acid-lowering treatment process of Fe3O4 NR@UOX. As a gentle and non-invasive regulation method, magnetic heat can repeatedly activate and shut down the activity of Fe3O4 NR@UOX through an external magnetic field. When the uric acid level is high, the magnetic field is turned on to reduce the uric acid to a normal level, and then the magnetic field is turned off to silence the enzyme activity, which can effectively maintain the uric acid at a normal level and avoid the toxic side effects caused by excessively high, too low or drastic fluctuations in uric acid levels. In addition, Fe3O4 NR@UOX under magnetic field stimulation can more efficiently and controllably ablate MSU crystals and improve joint swelling and pain in acute gout rat models. The oxygen generated by magnetic heat enhancement can also improve joint cavity hypoxia and relieve joint inflammation. Therefore, the magnetic nanohybrid uricase proposed in the present invention has the potential to simultaneously improve the therapeutic effect and safety of gout.
[0027] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a flow chart of a method for preparing a magnetic nano-hybrid uricase with adjustable activity provided by an embodiment of the present invention;
[0029] Figure 2 It is a TEM, FTIR and DLS data diagram of an activity-regulatable magnetic nano-hybrid uricase provided by an embodiment of the present invention;
[0030] Figure 3 This is a relationship diagram between the oxygen production of an activity-regulatable magnetic nanohybrid uricase and the magnetic field enhancement provided by an embodiment of the present invention;
[0031] Figure 4 This is a uric acid decrease curve of an activity-regulatable magnetic nano-hybrid uricase under magnetic field control provided by an embodiment of the present invention;
[0032] Figure 5 This is a polarizing microscope image of a magnetic nanohybrid uricase with adjustable activity provided by an embodiment of the present invention ablating MSU crystals under magnetic field control;
[0033] Figure 6 This is a data graph showing that an activity-regulatable magnetic nanohybrid uricase provided in an embodiment of the present invention regulates uric acid homeostasis under magnetic field control;
[0034] Figure 7 This is a data graph of the treatment of gout by an activity-regulatable magnetic nanohybrid uricase under magnetic field control provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0035] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, the activity-regulatable magnetic nano-hybrid uricase and its preparation method and application proposed by the present invention are described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0036] The above and other technical contents, features and effects of the present invention are clearly presented in the following detailed description of the specific implementation modes in conjunction with the accompanying drawings. Through the description of the specific implementation modes, the technical means and effects adopted by the present invention to achieve the predetermined purpose can be more deeply and specifically understood. However, the attached drawings are only for reference and explanation purposes and are not used to limit the technical solutions of the present invention.
[0037] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants are intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also other elements that are not explicitly listed. In the absence of more restrictions, the elements defined by the statement "including one..." do not exclude the existence of other identical elements in the article or device including the elements.
[0038] Embodiment 1
[0039] See also Figure 1 , Figure 1 The present invention provides a flow chart of a method for preparing a magnetic nano-hybrid uricase with adjustable activity, the method comprising:
[0040] S1: Take a predetermined amount of carboxylated vortex magnetic ferroferric oxide nanorings, add morpholineethanesulfonic acid solution, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride solution and N-hydroxysuccinimide solution in sequence, and react fully to activate the carboxyl groups on the surface of the carboxylated vortex magnetic ferroferric oxide nanorings to obtain carboxyl-activated vortex magnetic ferroferric oxide nanorings.
[0041] Specifically, a predetermined amount of carboxylated vortex magnetic ferroferric oxide nanoring (Fe3O4 NR) liquid is weighed and placed in a centrifuge tube; a predetermined amount of morpholineethanesulfonic acid (MES) powder, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride (EDC) powder and N-hydroxysuccinimide (NHS) powder are selected and proportioned into solutions, that is, morpholineethanesulfonic acid solution, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride solution and N-hydroxysuccinimide solution are proportioned respectively, wherein the mass ratio of ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride powder to N-hydroxysuccinimide powder is 1:1.5, and the pH value of the proportioned morpholineethanesulfonic acid solution is 6, and the concentration is 25mmol / L.
[0042] Then, morpholineethanesulfonic acid solution, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride solution and N-hydroxysuccinimide solution are added to the above centrifuge tube in sequence, and the reaction is shaken at room temperature for 10 to 40 minutes to activate the carboxyl groups on the surface of the carboxylated vortex magnetic ferroferric oxide nanorings. During the reaction, EDC forms EDC-NHS buffer hydrochloride with NHS; EDC-NHS buffer hydrochloride reacts with the hydroxyl groups in the carboxylated vortex magnetic ferroferric oxide nanoring molecules to form an ester bond; after the ester bond is formed, NHS spontaneously dissociates into NHS alcohol and equivalent acid, and the ester bond is further strengthened; the EDC activated part is hydrolyzed into EDC alcohol, thereby realizing the activation of the carboxyl groups on the surface of the carboxylated vortex magnetic ferroferric oxide nanorings.
[0043] Subsequently, magnetic separation technology is used to separate the carboxyl-activated vortex magnetic ferroferric oxide nanorings, and the upper solution is discarded, that is, the used mixed solution of morpholineethanesulfonic acid, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride and N-hydroxysuccinimide is discarded to obtain the carboxylated vortex magnetic ferroferric oxide nanorings after carboxyl activation.
[0044] S2: Add a predetermined amount of phosphate buffered saline solution, urate oxidase and deionized water to the vortex magnetic ferroferric oxide nanoring after carboxyl group activation, and react sufficiently to connect the carboxyl group on the surface of the vortex magnetic ferroferric oxide nanoring with the amino group on the surface of the urate oxidase in the form of an amide bond.
[0045] Specifically, a predetermined amount of phosphate buffered saline solution, uricase oxidase and deionized water are added to the vortex magnetic ferroferric oxide nanorings after carboxyl group activation, and ultrasonic dispersion is performed to form a dispersed solution, wherein the concentration of the added phosphate buffered saline solution is 0.1 mol / L and the pH value is 7.5; the dispersed solution is placed on a shaker and reacted at a temperature of 4 to 25° C. for 1 to 5 hours, so that the carboxyl group on the surface of the vortex magnetic ferroferric oxide nanorings after carboxyl group activation is connected to the amino group on the surface of the uricase oxidase in the form of an amide bond.
[0046] During the preparation process, the mass ratio of the carboxylated vortex magnetic ferroferric oxide nanorings to the uricase oxidase is (1:0.1) to (1:10). In this embodiment, the mass of the carboxylated vortex magnetic ferroferric oxide nanorings is weighed to be 0.01 to 10 mg, and the mass of the uricase oxidase is weighed to be 0.01 to 2 mg.
[0047] S3: After the reaction is completed, the reaction solution is centrifuged, and the activity-regulatable magnetic nanohybrid uricase is obtained after washing and refrigerated storage.
[0048] Specifically, after the reaction, the reaction solution was centrifuged to obtain the activity-regulatable magnetic nanohybrid uricase Fe3O4 NR@UOX, which was then washed three times and dispersed in a phosphate buffered saline solution and stored in a refrigerator.
[0049] Furthermore, the preparation method further comprises: regulating the activity of CAT enzyme in the magnetic nano-hybrid uricase with adjustable activity by means of an alternating magnetic field. The alternating magnetic field has a frequency of 100 kHz to 1 MHz and a magnetic field strength of 0 to 500 Oe.
[0050] Embodiment 2
[0051] On the basis of Example 1, this embodiment provides an activity-regulatable magnetic nanohybrid uricase, which includes a composite material of carboxylated vortex magnetic ferroferric oxide nanorings and uricase oxidase. In the magnetic nanohybrid uricase, the mass ratio of the carboxylated vortex magnetic ferroferric oxide nanorings and uricase oxidase is 0.1:10, wherein the carboxylated vortex magnetic ferroferric oxide nanorings are connected to the uricase oxidase via an amide bond. The size of the carboxylated vortex magnetic ferroferric oxide nanorings is 40 to 300 nm.
[0052] See also Figure 2 , Figure 2 The TEM (transmission electron microscope), FTIR (Fourier transform infrared spectrometer) and DLS (dynamic light scattering) data diagram of an activity-regulatable magnetic nanohybrid uricase provided by an embodiment of the present invention, wherein: Figure 2 a is the TEM image of Fe3O4 NR@UOX after negative staining with phosphotungstic acid. It can be seen that there is a layer of protein on the surface of Fe3O4 NR, which is UOX. Figure 2 b It can be seen that UOX is successfully modified on Fe3O4 NR. Figure 2 c It can be seen that the particle size of Fe3O4 NR@UOX increases from 91nm to 113nm compared with Fe3O4 NR. The above results prove the successful construction of Fe3O4 NR@UOX.
[0053] Embodiment 3
[0054] On the basis of the above embodiments, this embodiment provides the application of the activity-regulatable magnetic nanohybrid uricase Fe3O4 NR@UOX in maintaining uric acid homeostasis, ablating MSU crystals, and alleviating gouty joint damage and inflammation.
[0055] (1) Application in regulating uric acid-lowering activity.
[0056] Test conditions:
[0057] First, the CAT enzyme activity of Fe3O4 NR was observed in the following two ways.
[0058] The first method: Use a dissolved oxygen meter to measure the oxygen content in the solution. Test conditions: Add 3500μL of PBS solution with pH 7.4, 1000μL of 500mM H2O2 solution, and 500μL of 100μL / mL Fe3O4 NR solution to four centrifuge tubes. The total volume of the solution in each centrifuge tube is 5mL. Place the four centrifuge tubes in a magnetic field of 0Oe, 200Oe, 300Oe, and 400Oe for 20 minutes.
[0059] The second method: add 300 μL of 5M H2O2, 100 μL of 300 μg / mL Fe3O4NR and 2600 μL of PBS with pH 7.4 to four centrifuge tubes, place them under magnetic fields of 0 Oe, 200 Oe, 300 Oe and 400 Oe for 30 min respectively, and photograph the bubbles in the centrifuge tubes.
[0060] The experimental results are as follows Figure 3 As shown, the increase of magnetic field intensity can accelerate the CAT enzyme activity in Fe3O4 NR and accelerate the generation of O2.
[0061] Subsequently, the uric acid-lowering activity of the magnetic field-controlled enzyme was observed in the following manner.
[0062] Fe3O4 NR@UOX, UA (uric acid) and PBS solutions were added to the cuvette, and the cuvette was placed in the in-situ magnetothermal ultraviolet spectroscopic system. The magnetic field (334kHz, 400Oe) was repeatedly switched on and off, and the absorbance at 292nm was monitored over time. Specifically, the absorbance was measured using the in-situ magnetothermal ultraviolet spectroscopic system, and the instrument parameters were set: the wavelength was set to 292nm. All solutions used in the experiment were introduced with N2 in advance to simulate an oxygen-deficient environment.
[0063] See also Figure 4 , Figure 4 This is a graph showing the decrease of uric acid in a magnetic nanohybrid uricase with adjustable activity under magnetic field control provided by an embodiment of the present invention. Figure 4It can be seen that in an oxygen-deficient environment, when the magnetic field is turned on, the uric acid decrease rate will increase instantaneously; after the magnetic field is turned off, the uric acid decrease rate will decrease, indicating that the magnetic field can real-time and reversibly regulate the uric acid decrease rate of Fe3O4 NR@UOX.
[0064] (2) Application in controlled ablation of MSU crystals.
[0065] Test conditions:
[0066] Weigh 0.15 mg of MSU crystals, add 10 mL of UA solution to make a 0.015 mg / mL MSU solution, take 1 mL of the solution in 3 centrifuge tubes (experimental groups: Water, Fe3O4 NR@UOX, Fe3O4 NR@UOX+AMF (alternating magnetic field)), and place them in an oxygen-deficient environment for reaction. The corresponding UOX in the solution is 0.1 mg / mL. Then place the centrifuge tube of the Fe3O4 NR@UOX+AMF experimental group in a magnetic field for 30 min (362 kHz, 400 Oe), and the other experimental groups are not added with a magnetic field. Finally, take the bottom crystal precipitate and observe and photograph it under a polarizing microscope.
[0067] See also Figure 5 , Figure 5 This is a data graph of a magnetic nanohybrid uricase with adjustable activity provided by an embodiment of the present invention, which ablate MSU crystals under magnetic field control. Figure 5 It can be seen that Fe3O4 NR@UOX driven by magnetic field has excellent MSU crystallization dissolution effect.
[0068] (3) Application in dynamically regulating uric acid levels and maintaining uric acid homeostasis.
[0069] Test conditions:
[0070] UA (uric acid), PBS and Fe3O4NR@UOX prepared in the embodiment of the present invention were added to the cuvette, and the total volume of the solution was 1 mL, so that the concentration of UA in the cuvette was greater than 420 μmol / L, and the concentration of UOX loaded on Fe3O4 NR@UOX was 0.05 mg / mL. An alternating magnetic field of 400 Oe was applied, and the absorbance at 292 nm was measured at regular intervals until the uric acid concentration dropped to between 180-360 μmol / L; then UA solution was added to the cuvette until the uric acid concentration was greater than 420 μmol / L, and the subsequent operations were the same as above. The effect of magnetic field regulation on the uric acid level of Fe3O4 NR@UOX enzyme activity was observed.
[0071] The experimental results are as follows Figure 6As shown, when the uric acid concentration is at a high uric acid level, the magnetic field is turned on to accelerate the decomposition of uric acid; when the uric acid level reaches the normal range, the magnetic field is turned off, and the uric acid concentration can be maintained at a normal level for a long time. Supplementing uric acid into the system again to simulate the fluctuation of uric acid levels caused by diet can still achieve steady-state regulation of uric acid levels through the ON-OFF conversion of the magnetic field.
[0072] (4) Application in the body to simultaneously relieve gout joint damage and inflammation.
[0073] Test conditions:
[0074] An acute gout model was established by injecting 8 mg of MSU crystals (MSU crystals were sieved through a 250 μm sieve in advance) into the ankle joint of rats. 24 hours after modeling, the same method was used to inject drugs (100 μg Fe / 0.19 mg UOX) into the gout joint cavity. The magnetic field treatment group was subjected to a magnetic field (420 kHz, 300 Oe) at 24, 36, 48, 60, and 66 hours after modeling. The rats were dissected at 72 hours after modeling (i.e., 48 hours after injection) and the following observations were made:
[0075] 1) Use a vernier caliper to measure the diameter of the left hind ankle joint of the rats at 0, 24, 36, 48, 60, 66, and 72 hours after modeling, measure three times and take the average value to calculate the degree of joint swelling. White light photography of the rat joints was performed at 0, 24, 36, 48, 60, 66, and 72 hours.
[0076] 2) The rats were anesthetized and killed, and the ankle joints were removed and fixed in a paraformaldehyde solution for more than 24 hours to harden the tissues, and then placed in a decalcification solution for decalcification. After decalcification, the joints were embedded and sliced, and stained with safranin-fast green, IL-6 and HIF-1α immunohistochemically. The experimental results are shown in Figure 7 As shown, Figure 7 a is the change of ankle joint swelling of rats over time (measured by vernier caliper); Figure 7 b is a picture of the rat ankle joint; Figure 7 c is a section staining image of the rat ankle joint: Safranin Fast Green (scale bar: 200 μm), IL-6 (scale bar: 100 μm) and HIF-1α (scale bar: 100 μm), respectively. Figure 7 a and Figure 7 b shows that the degree of joint swelling reduction in the Fe3O4 NR@UOX+AMF treatment group is the greatest, and the treatment effect is good; Figure 7 c It shows that the Fe3O4 NR@UOX+AMF treatment group has the greatest effect in alleviating joint injury, inflammation and hypoxia, and has a good therapeutic effect. It shows that the magnetic field combined with the Fe3O4 NR@UOX treatment group has the best effect in reducing joint swelling, and effectively relieves joint hypoxia and joint inflammation.
[0077] In summary, in the magnetic nanohybrid uricase with adjustable activity of the present invention, the magnetic induction heat mediated by Fe3O4 NR can drive the CAT nanozyme of Fe3O4 NR to produce oxygen to activate uricase, and realize the reversible regulation of the alternating magnetic field on the uric acid-lowering treatment process of Fe3O4 NR@UOX. As a gentle and non-invasive regulation method, magnetic heat can repeatedly activate and shut down the activity of Fe3O4 NR@UOX through an external magnetic field. When the uric acid level is high, the magnetic field is turned on to reduce the uric acid to a normal level, and then the magnetic field is turned off to silence the enzyme activity, which can effectively maintain the uric acid at a normal level and avoid the toxic side effects caused by excessive, low or drastic fluctuations in uric acid levels. In addition, Fe3O4 NR@UOX under magnetic field stimulation can more efficiently and controllably ablate MSU crystals and improve joint swelling and pain in acute gout rat models. The oxygen generated by magnetic heat enhancement can also improve joint cavity hypoxia and relieve joint inflammation. Therefore, the magnetic nanohybrid uricase proposed by the present invention has the potential to simultaneously improve the therapeutic effect and safety of gout.
[0078] In the several embodiments provided by the present invention, it should be understood that the apparatus and method disclosed by the present invention can be implemented in other ways. For example, the apparatus embodiments described above are only illustrative, for example, the division of the modules is only a logical function division, and there may be other division methods in actual implementation, such as multiple modules or components can be combined or integrated into another system, or some features can be ignored or not executed.
[0079] In addition, each functional module in each embodiment of the present invention may be integrated into one processing module, or each module may exist physically separately, or two or more modules may be integrated into one module. The above-mentioned integrated module may be implemented in the form of hardware or in the form of hardware plus software functional modules.
[0080] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing a magnetic nano-hybrid uricase with adjustable activity, characterized in that: include: S1: taking a predetermined amount of carboxylated vortex magnetic ferroferric oxide nanorings, adding morpholineethanesulfonic acid solution, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride solution and N-hydroxysuccinimide solution in sequence, reacting sufficiently to activate the carboxyl groups on the surface of the carboxylated vortex magnetic ferroferric oxide nanorings, and obtaining vortex magnetic ferroferric oxide nanorings after carboxyl group activation; S2: adding a predetermined amount of phosphate buffered saline solution, urate oxidase and deionized water to the vortex magnetic ferroferric oxide nanoring after the carboxyl group activation, and reacting them sufficiently so that the carboxyl group on the surface of the vortex magnetic ferroferric oxide nanoring is connected to the amino group on the surface of the urate oxidase in the form of an amide bond; S3: After the reaction is completed, the reaction solution is centrifuged and washed to obtain the activity-regulatable magnetic nano-hybrid uricase.
2. The method for preparing the activity-regulatable magnetic nano-hybrid uricase according to claim 1, characterized in that: The mass ratio of the carboxylated vortex magnetic ferroferric oxide nanoring to the uricase is (1:0.1) to (1:10).
3. The method for preparing the activity-regulatable magnetic nano-hybrid uricase according to claim 1, characterized in that: The S1 includes: A predetermined amount of carboxylated vortex magnetic ferroferric oxide nanorings is placed in a centrifuge tube; Selecting predetermined amounts of morpholineethanesulfonic acid powder, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride powder and N-hydroxysuccinimide powder and respectively proportioning them into solutions, wherein the mass ratio of the ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride powder to the N-hydroxysuccinimide powder is 1:1.5, and the pH value of the proportioned morpholineethanesulfonic acid solution is 6, and the concentration is 25 mmol / L; Adding morpholineethanesulfonic acid solution, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride solution and N-hydroxysuccinimide solution into the centrifuge tube in sequence, shaking and reacting at room temperature for 10 to 40 minutes to activate the carboxyl groups on the surface of the carboxylated vortex magnetic ferrosoferric oxide nanorings; Magnetic separation technology is used to separate the carboxyl-activated vortex magnetic ferroferric oxide nanorings, and the mixed solution of morpholineethanesulfonic acid, ethyl [3-(dimethylamino)propyl] carbodiimide hydrochloride and N-hydroxysuccinimide in the upper layer is discarded to obtain the carboxylated vortex magnetic ferroferric oxide nanorings after carboxyl activation.
4. The method for preparing the activity-regulatable magnetic nano-hybrid uricase according to claim 1, characterized in that: The S2 includes: Adding a predetermined amount of phosphate buffered saline solution, urate oxidase and deionized water to the vortex magnetic ferrosoferric oxide nanorings after carboxyl activation, and ultrasonically dispersing to form a dispersed solution, wherein the concentration of the added phosphate buffered saline solution is 0.1 mol / L; The dispersed solution is placed on a shaker and reacted at 4-25° C. for 1-5 hours, so that the carboxyl groups on the surface of the vortex magnetic ferroferric oxide nanorings after carboxyl group activation are connected to the amino groups on the surface of the urate oxidase in the form of amide bonds.
5. The method for preparing the activity-regulatable magnetic nano-hybrid uricase according to claim 1, characterized in that: Also includes: The CAT enzyme activity in the activity-regulatable magnetic nanohybrid uricase is regulated by an alternating magnetic field.
6. The method for preparing the activity-regulatable magnetic nano-hybrid uricase according to claim 5, characterized in that: The conditions of the alternating magnetic field are a frequency of 100 kHz to 1 MHz and a magnetic field strength of 0 to 500 Oe.
7. A magnetic nanohybrid uricase with adjustable activity, characterized in that: The magnetic nanohybrid uricase is prepared by the preparation method according to any one of claims 1 to 6, wherein the magnetic nanohybrid uricase comprises a composite material of carboxylated vortex magnetic ferroferric oxide nanorings and uricase oxidase.
8. The activity-regulatable magnetic nanohybrid uricase according to claim 7, characterized in that: The size of the carboxylated vortex magnetic ferroferric oxide nanoring is 40 to 300 nm.
9. The activity-regulatable magnetic nanohybrid uricase according to claim 7, characterized in that: In the magnetic nano-hybrid uricase, the mass ratio of the carboxylated vortex magnetic ferroferric oxide nanoring to the uricase oxidase is 0.1:10, and the carboxylated vortex magnetic ferroferric oxide nanoring and the uricase oxidase are connected via an amide bond.
10. Use of the activity-regulatable magnetic nanohybrid uricase according to claims 7 to 9 in maintaining uric acid homeostasis, ablating MSU crystals, and alleviating gouty joint damage and inflammation.