Bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing and preparation method thereof
Through the compounding of bacterial cellulose and dialdehyde carboxy starch, a hydrogel wound dressing with higher mechanical properties and antibacterial properties is formed, which solves the problem of insufficient mechanical strength of bacterial cellulose dressings and the toxicity of composite materials, and achieves faster and faster wound dressings. Higher wound healing effect.
Patent Information
- Application Number
- CN202410852543.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The mechanical strength and mechanical properties of bacterial cellulose hydrogel wound dressings are insufficient, and the antibacterial components in the composite materials are toxic to human cells. It is difficult to improve their mechanical properties and reduce cytotoxicity while maintaining antibacterial properties and wound healing properties. .
Bacterial cellulose and dialdehyde carboxy starch are composited, and the dialdehyde carboxy starch is prepared through periodate oxidation, and soaked with bacterial cellulose in a specific proportion of polyvinyl alcohol solution to form a composite hydrogel wound dressing.
It improves the dressing's ability to promote wound healing, promote the growth of new granulation tissue and produce collagen. It has higher water content, softness, extensibility and antibacterial properties, while reducing cytotoxicity and forming a denser microstructure.
Smart Images

Figure CN118846201A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biomedical hydrogels, in particular to a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing and a preparation method thereof. Background Art
[0002] Wound dressing is a protective layer used to cover the wound. It plays a role in preventing wound infection, promoting cell proliferation, and protecting the wound from secondary trauma during the wound healing process. Hydrogel dressings have a unique three-dimensional network structure. Its soft elasticity and high hydrophilicity make the dressing easy to disassemble, prevent adhesion, prevent secondary trauma, and help provide a moist environment for the wound and promote the growth of epithelial granulation tissue. Bacterial cellulose (BC) is a natural polymer synthesized by microorganisms with a nanoscale fiber network structure. As a hydrogel material, it has good biocompatibility, high plasticity and high porosity, and has application potential in the field of wound dressings.
[0003] At present, the preparation method of bacterial cellulose hydrogel wound dressings mainly uses bacterial cellulose as the matrix material and enhances its performance by adding reinforcing materials. Bacterial cellulose is often compounded with other materials with antibacterial and anti-inflammatory functions to prepare bacterial cellulose composite hydrogel wound dressings to improve their mechanical properties, antibacterial properties and / or ability to promote wound healing.
[0004] Bacterial cellulose hydrogels are increasingly used in the medical field, but they still have certain limitations. Their mechanical strength and mechanical properties are still insufficient compared to natural plant or synthetic fiber dressings. At the same time, although ingredients such as nanosilver and phenytoin in composite materials have strong antibacterial, anti-inflammatory and high wound healing abilities, they have certain toxicity to human cells or tissues and organs. How to improve the mechanical properties of bacterial cellulose hydrogel wound dressings and reduce the cytotoxicity of composite materials while maintaining antibacterial and wound healing properties is the development direction of bacterial cellulose hydrogel wound dressings.
[0005] Our previous application number is 202310679359.5, a bacterial cellulose-xyloglucan-dextran composite hydrogel wound dressing and its preparation method, the activated bacterial cellulose production bacteria are inoculated into the seed liquid culture medium to obtain the seed liquid; the obtained seed liquid is inoculated into the fermentation medium containing xyloglucan with a mass concentration of 0.2-1% and dextran with a mass concentration of 0.2-1% to cultivate and harvest the bacterial cellulose-xyloglucan-dextran complex, which is repeatedly soaked and washed with pure water for many times until the color is close to white, and the complex is washed with pure water to a neutral pH to obtain the bacterial cellulose-xyloglucan-dextran composite hydrogel wound dressing. The bacterial cellulose-xyloglucan-dextran composite hydrogel wound dressing has good fit, softness and ductility, and the ability to accelerate wound healing; however, the manufacturing process is more complicated, and the ability to promote wound healing, the ability to promote the growth of new granulation tissue and the ability to promote collagen production need to be improved.
[0006] Dialdehyde-carboxyl-amylose (DACA) is an oxidized starch with high water solubility, antibacterial properties and good biocompatibility. It has the potential to be combined with bacterial cellulose to produce a new type of composite hydrogel wound dressing.
[0007] Therefore, it is urgent to try to prepare a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing. Summary of the invention
[0008] In order to solve the above technical problems, the present invention provides a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing and a preparation method thereof.
[0009] To achieve the above object, the present invention is implemented according to the following technical solutions:
[0010] One of the purposes of the present invention is to provide a method for preparing a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing, comprising the following steps:
[0011] S1: using carboxylated starch as raw material, dialdehyde carboxylated starch was prepared by periodate oxidation;
[0012] S2: inoculating the bacterial cellulose producing strain into a fermentation medium, culturing at 25-36°C for 3-5 days to obtain a strain concentrate; the fermentation medium is composed of the following components: 20-25 g / L glucose, 2.0-3.0 g / L anhydrous disodium hydrogen phosphate, 1.0-2.0 g / L citric acid monohydrate, 5-10 g / L yeast extract, 5-10 g / L peptone, and the balance is deionized water, and the pH is adjusted to 4.0-5.0 with 1 mol / L hydrochloric acid solution;
[0013] S3: inoculating the obtained bacterial concentrate into a fermentation medium at a ratio of 8-15 (v / v)%, placing it in a constant temperature box at 25-36°C for 5-9 days to obtain bacterial cellulose, soaking and washing it with pure water for multiple times until the color is close to white and the pH is neutral, to obtain a bacterial cellulose hydrogel; the fermentation medium is composed of the following components: 20-25 g / L glucose, 2.0-3.0 g / L anhydrous disodium hydrogen phosphate, 1.0-2.0 g / L monohydrate citric acid, 5-10 g / L yeast extract, 5-10 g / L peptone, and the balance deionized water, and adjusting the pH to 4.0-5.0 with 1 mol / L hydrochloric acid solution;
[0014] S4: Soaking the purified bacterial cellulose in a solution containing 0.5-2% polyvinyl alcohol and dialdehyde carboxyl starch at a mass concentration for 3-5 days to obtain a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing.
[0015] Furthermore, the preparation method of the carboxyl starch in step S1 is: oxidizing the starch with 2,2,6,6-tetramethylpiperidine-1-oxyl free radical, sodium bromide, and sodium hypochlorite in sequence, and dialyzing to obtain the carboxyl starch.
[0016] Furthermore, the molar concentration of sodium periodate in step S1 is 0.5M-1.1M, preferably 0.9M.
[0017] Furthermore, the bacterial cellulose producing bacteria used in step S1 is one of the genera Acetobacter, Acetobacter xylinum, and Xylella fastidiosa, preferably Acetobacter xylinum.
[0018] Furthermore, in step S2, the total number of bacterial cellulose producing bacteria in each milliliter of bacterial concentrate is 10 2 -10 4 CFU.
[0019] The second object of the present invention is to provide a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing prepared by the above method.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] Compared with commercially available sterile gauze, commercially available hydrocolloid dressings and bacterial cellulose hydrogel wound dressings, bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressings have stronger ability to promote wound healing, the growth of new granulation tissue and the production of collagen during long-term (2 weeks) use.
[0022] Compared with medical sterile gauze, commercially available hydrocolloid dressings, bacterial cellulose hydrogel wound dressings and bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressings, the bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing has the microstructural characteristics of fiber porous properties, as well as mechanical characteristics such as high water content, good softness and good ductility; in addition, it also has certain antibacterial properties and excellent biocompatibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Scanning electron microscopy (SEM) images of bacterial cellulose hydrogel (BC) and different bacterial cellulose-diacetic acid carboxyl starch composite hydrogels (BC-DACA(E)).
[0024] Figure 2 The infrared spectra (FTIR) of bacterial cellulose hydrogel (BC) and different bacterial cellulose-dialdehyde carboxyl starch composite hydrogels (BC-DACA(E)).
[0025] Figure 3 These are the results of tensile tests and creep-recovery experiments on bacterial cellulose hydrogel (BC) and different bacterial cellulose-diacetic acid carboxyl starch composite hydrogels (BC-DACA(E)).
[0026] Figure 4 These are the rheological amplitude scanning and frequency scanning results of bacterial cellulose hydrogel (BC) and different bacterial cellulose-diacetic carboxyl starch composite hydrogels (BC-DACA(E)).
[0027] Figure 5 These are the rheological amplitude scanning and frequency scanning results of bacterial cellulose hydrogel (BC) and different bacterial cellulose-diacetic carboxyl starch composite hydrogels (BC-DACA(E)).
[0028] Figure 6 These are the antibacterial rate test results of bacterial cellulose hydrogel (BC) and different bacterial cellulose-diadehydic carboxyl starch composite hydrogels (BC-DACA).
[0029] Figure 7 These are the cell compatibility test results of bacterial cellulose hydrogel (BC) and different bacterial cellulose-diacetic acid carboxylated starch composite hydrogels (BC-DACA(E)). DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the invention.
[0031] Unless otherwise specified, the reagents and materials used in the following examples were commercially available or homemade; Acetobacter xylinum was purchased from the China Microbiological Protection Center; the fermentation medium consisted of the following ingredients: 20 g / L glucose, 2.7 g / L anhydrous disodium hydrogen phosphate, 1.26 g / L citric acid monohydrate, 5 g / L yeast extract, 5 g / L peptone, and the balance deionized water, and the pH was adjusted to 5.0 with 1 mol / L hydrochloric acid solution.
[0032] Example 1
[0033] S1: The starch was oxidized by 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium bromide, and sodium hypochlorite in sequence, and then dialyzed to obtain carboxyl starch; secondly, the carboxyl starch was used as a raw material and oxidized by periodate at a concentration of 0.5 M to prepare dialdehyde carboxyl starch (DACA1);
[0034] S2: inoculating the activated Acetobacter xylinum into the fermentation medium, culturing at 30°C for 3 days to obtain a strain concentrate;
[0035] S3: inoculating the obtained bacterial concentrate into a fermentation medium, placing it in a constant temperature box at 30°C for 5 days, harvesting the bacterial cellulose hydrogel, and repeatedly soaking and washing it with pure water until the color is close to white and the pH is neutral, thereby obtaining the bacterial cellulose hydrogel;
[0036] S4: The bacterial cellulose was immersed in a solution containing 1% polyvinyl alcohol and dialdehyde carboxyl starch (DACA1) at a mass concentration of 1% for 3 days to obtain a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1(E)) wound dressing.
[0037] Example 2
[0038] S1: Starch was oxidized by 2,2,6,6-tetramethylpiperidin-1-oxyl radical, sodium bromide, and sodium hypochlorite in sequence, and then dialyzed to obtain carboxyl starch. Then, carboxyl starch was used as a raw material and oxidized by periodate at a concentration of 0.7 M to prepare dialdehyde carboxyl starch (DACA2);
[0039] S2: inoculating the activated Acetobacter xylinum into the fermentation medium, culturing at 30°C for 3 days to obtain a strain concentrate;
[0040] S3: inoculating the obtained bacterial concentrate into a fermentation medium, placing it in a constant temperature box at 30°C for 5 days, harvesting the bacterial cellulose hydrogel, and repeatedly soaking and washing it with pure water until the color is close to white and the pH is neutral, thereby obtaining the bacterial cellulose hydrogel;
[0041] S4: The bacterial cellulose was immersed in a solution containing 1% polyvinyl alcohol and dialdehyde carboxyl starch (DACA2) at a mass concentration of 1% for 3 days to obtain a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA2(E)) wound dressing.
[0042] Example 3
[0043] S1: The starch was oxidized by 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium bromide, and sodium hypochlorite in sequence, and then dialyzed to obtain carboxyl starch; secondly, the carboxyl starch was used as a raw material and oxidized by periodate at a concentration of 0.9 M to prepare dialdehyde carboxyl starch (DACA3);
[0044] S2: inoculating the activated Acetobacter xylinum into the fermentation medium, culturing at 30°C for 3 days to obtain a strain concentrate;
[0045] S3: inoculating the obtained bacterial concentrate into a fermentation medium, placing it in a constant temperature box at 30°C for 5 days, harvesting the bacterial cellulose hydrogel, and repeatedly soaking and washing it with pure water until the color is close to white and the pH is neutral, thereby obtaining the bacterial cellulose hydrogel;
[0046] S4: The bacterial cellulose was immersed in a solution containing 1% polyvinyl alcohol and dialdehyde carboxyl starch (DACA3) at a mass concentration of 1% for 3 days to obtain a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA3(E)) wound dressing.
[0047] Example 4
[0048] S1: The starch was oxidized by 2,2,6,6-tetramethylpiperidin-1-oxyl free radical, sodium bromide, and sodium hypochlorite in sequence, and then dialyzed to obtain carboxyl starch; secondly, the carboxyl starch was used as a raw material and oxidized by periodate at a concentration of 1.1 M to prepare dialdehyde carboxyl starch (DACA4);
[0049] S2: inoculating the activated Acetobacter xylinum into the fermentation medium, culturing at 30°C for 3 days to obtain a strain concentrate;
[0050] S3: inoculating the obtained bacterial concentrate into a fermentation medium, placing it in a constant temperature box at 30°C for 5 days, harvesting the bacterial cellulose hydrogel, and repeatedly soaking and washing it with pure water until the color is close to white and the pH is neutral, thereby obtaining the bacterial cellulose hydrogel;
[0051] S4: The bacterial cellulose was immersed in a solution containing 1% polyvinyl alcohol and dialdehyde carboxyl starch (DACA4) at a mass concentration of 1% for 3 days to obtain a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA4 (E)) wound dressing.
[0052] Comparative Example 1
[0053] S1: inoculating the activated Acetobacter xylinum into the fermentation medium, culturing at 30°C for 3 days to obtain a strain concentrate;
[0054] S2: The obtained bacterial concentrate was inoculated into the fermentation medium and placed in a constant temperature box at 30°C for 3 days;
[0055] S3: The bacterial cellulose is harvested, and it is repeatedly soaked and washed with purified water until the color is close to white, and the hydrogel is washed with purified water until the color is close to white and the pH is neutral, thereby obtaining a bacterial cellulose (BC) wound dressing.
[0056] The bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1(E), BC-DACA2(E), BC-DACA3(E), BC-DACA4(E)) wound dressings and bacterial cellulose (BC) wound dressings prepared in Examples 1-4 and Comparative Example 1 were respectively made into circular wound dressings of the same area. The physical comparison diagram is as follows: Figure 1 Some physical parameters of the wound dressings are shown in Table 1. The moisture content of the five kinds of dressings is all above 96%, which has an extremely high moisture content, and the thickness is also significantly reduced, making the dressings easier to fit human skin.
[0057] Table 1
[0058]
[0059]
[0060] Note: Different letters in the same column indicate significant differences (p<0.05)
[0061] Further, the bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1(E), BC-DACA2(E), BC-DACA3(E), BC-DACA4(E)) wound dressings and bacterial cellulose (BC) wound dressings prepared in Examples 1-4 and Comparative Example 1 were cut into small pieces of about 2×2 mm and freeze-dried for 48 h. After gold coating, the microscopic morphology was observed under a scanning electron microscope at an appropriate field of view and magnification, and photographed and recorded. The results are shown in FIG. Figure 1 As shown. Different from BC fibers, BC-DACA (E) fibers have more substances attached to them, especially the fiber joints present obvious sheet-like structures. Impregnation composite allows the polymer to pass through the BC network, fill the free gaps between fibers, reduce the distance between cellulose chains, promote the bonding of fiber bundles, reduce the porosity of the hydrogel, and make the composite hydrogel have a denser and filled structure than pure BC.
[0062] In this example, the functional group determination of bacterial cellulose (BC) wound dressing and bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA (E)) wound dressing was also carried out, as follows:
[0063] The transmittance of bacterial cellulose-bisaldehyde carboxyl starch composite hydrogel (BC-DACA1(E), BC-DACA2(E), BC-DACA3(E), BC-DACA4(E)) wound dressings and bacterial cellulose (BC) wound dressing dry film prepared in Examples 1-4 and Comparative Example 1 was tested using the attenuated total reflectance (ATR) module of a Fourier transform infrared spectrometer (FTIR). The number of scans was 32, the resolution was 4, and the transmittance was 4000-400 cm -1 Record spectra in between.
[0064] Figure 2 In the FTIR spectrum, BC is at 3345cm -1 The absorption peak at 1092cm is the vibration absorption peak of -OH. The absorption peak of BC-DACA(E) is blue-shifted, which is caused by the formation of hydrogen bonds. -1 is the stretching vibration of -CO-, which is similar to the 1040cm -1 The peaks merged into a broad peak with increased peak intensity, indicating that the hydrogen bonding effect was enhanced. -1 A new absorption peak clearly appeared at 1640 cm -1 The peaks at correspond to the symmetric vibration and antisymmetric vibration peaks of the carboxylic acid group after combination, indicating that DACA is incorporated into the structural system.
[0065] In order to verify the softness and ductility of the wound dressing prepared by the present invention, the mechanical properties of bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1(E), BC-DACA2(E), BC-DACA3(E), BC-DACA4(E)) wound dressings and bacterial cellulose (BC) wound dressings were tested. The mechanical properties test includes three parts: ① tensile test; ② creep-recovery test; ③ amplitude sweep and frequency sweep test:
[0066] 1) Tensile test: According to ISO37-4 standard, use a punch to cut the gel into dumbbell-shaped samples with 6×35mm at the end and 2×10mm in the middle. Use a texture analyzer or a universal testing machine to perform axial stretching at a speed of 10mm / min and a maximum load of 5N, and record the stretching distance and tensile stress (σ, MPa). The stretching distance is converted into tensile strain (ε, %), and Young's modulus (E, MPa) is defined as the slope of the linear part of the strain-stress curve.
[0067] 2) Creep-recovery test: A rotational rheometer was used to test. An initial shear stress (τ0) of 10 Pa was applied to the sample for 171 seconds, and then the stress was removed. The sample was allowed to recover for 171 seconds and the creep compliance (J, Pa -1 ) changes with time, and the creep parameter α is calculated by the following formula (α=1 represents a completely viscous body, α=0 represents a completely elastic body, and 0<α<1 represents a viscoelastic body).
[0068]
[0069] Where J(t) is the creep compliance, γ(t) is the strain during the test, τ0 is the instantaneous stress applied, λ1 and λ2 are the inverses of the sample gel elastic modulus in the creep and recovery stages, respectively, Γ(x) is the gamma function, t is the test time, and t m is the time when the recovery phase starts, and H(x) is the Heaviside step function.
[0070] 3) Amplitude sweep and frequency sweep test: The test was performed using a rotational rheometer. The amplitude sweep was performed at a constant frequency of 10 rad / s, and the shear strain amplitude was increased logarithmically from 0.01% to 100%. The storage modulus (G') and loss modulus (G") were recorded. The frequency sweep was performed at a fixed amplitude of 0.01%, and the frequency was increased from 0.4 rad / s to 400 rad / s, and the storage modulus (G') and loss modulus (G") at different frequencies were recorded.
[0071] The tensile test, creep-recovery test results, and rheological amplitude sweep and frequency sweep results of bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1(E), BC-DACA2(E), BC-DACA3(E), BC-DACA4(E)) wound dressings and bacterial cellulose (BC) wound dressings are shown in Figure 2 . Figure 3 , Figure 4 shown.
[0072] Figure 3The mechanical properties of BC and BC-DACA(E) hydrogel wound dressings are shown. Compared with BC hydrogel, BC-DACA(E) has a lower Young's modulus and a significantly higher fracture strain, indicating that the BC-DACA(E) composite hydrogel becomes softer than the BC hydrogel; the tensile stress of BC-DACA4(E) increases significantly, indicating that the addition of DACA4 improves the ductility of the composite hydrogel while maintaining a certain stiffness. The α value of the BC-DACA4(E) composite hydrogel is the largest (0.82), indicating that its viscosity is higher than that of other composite hydrogels. Compared with BC (44.71%), the recovery rates of the BC-DACA3(39.77%) and BC-DACA4(28.84%) composite hydrogels are reduced, indicating that the addition of DACA makes the composite hydrogel more deformable under the action of external stress.
[0073] Figure 4 The rheological properties of BC and BC-DACA(E) hydrogel wound dressings are shown. The critical shear strain of BC is 1.38%, and the critical shear strain of other BC-DACA(E)s generally shows a decreasing trend (0.83-1.55%), indicating that the BC-DACA(E) composite hydrogel is softer and easier to deform. The initial storage modulus and initial loss modulus of BC are 9.66 kPa and 1.34 kPa, respectively. The initial storage modulus and initial loss modulus of BC-DACA4(E) are both reduced, and the loss factor is increased, indicating that the addition of DACA makes the composite hydrogel more viscous, that is, BC-DACA4(E) is the softest of all composite hydrogels, which is consistent with the results of tensile and creep tests.
[0074] In order to determine the antibacterial rate of the wound dressing prepared by the present invention, bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1(E), BC-DACA2(E), BC-DACA3(E), BC-DACA4(E)) wound dressings and bacterial cellulose (BC) wound dressings were tested for their antibacterial rate. The specific experimental process is as follows:
[0075] The activated three bacterial suspensions: Staphylococcus aureus (S. aureus), Pseudomonas aeruginosa (P. aeruginosa), Escherichia coli (E. coli) were diluted to about 10 5 CFU / mL, 1 mL of bacterial suspension was added to a 24-well plate, and BC and BC-DACA(E) composite hydrogels were cut into circles with a diameter of 1 cm and immersed in the bacterial suspension. The bacterial suspension was used as a control, and the optical density (OD = 600 nm) of the bacteria after 24 h of culture was measured using an ultraviolet spectrophotometer to calculate the inhibition rate.
[0076] The antibacterial rate test results of bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1(E), BC-DACA2(E), BC-DACA3(E), BC-DACA4(E)) wound dressings are as follows Figure 5 shown.
[0077] Depend on Figure 5 It can be seen that BC-DACA3(E) composite hydrogel has the best antibacterial effect on Staphylococcus aureus, and BC-DACA4(E) has the best inhibitory effect on Escherichia coli and Pseudomonas aeruginosa. Other composite hydrogels have certain antibacterial properties, and have a more prominent inhibitory effect on Pseudomonas aeruginosa. BC-DACA(E) prepared by non-in situ synthesis has certain antibacterial properties, and DACA with a high degree of oxidation has a better inhibitory effect on bacteria, which is caused by the carboxyl and aldehyde groups of DACA.
[0078] In order to determine the biocompatibility of the wound dressing prepared by the present invention, the biocompatibility tests of bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1(E), BC-DACA2(E), BC-DACA3(E), BC-DACA4(E)) wound dressings, bacterial cellulose (BC) wound dressings and commercially available hydrocolloid dressings were conducted. The specific experimental process is as follows:
[0079] Before the experiment, the hydrogel samples need to be extracted. Under sterile operation, BC and BC-DACA (E) composite hydrogels are mixed with DMEM culture medium containing 10% serum by volume at a ratio of 0.2g / mL, and extracted at 37°C for 24h. The blank control uses DMEM culture medium containing 10% serum by volume without hydrogel extraction, and the extract is diluted 0, 2, 4, 6 and 8 times. HaCaT cells are inoculated in a 96-well plate at a concentration of 10,000 cells / well, and blank DMEM culture medium containing 10% serum by volume is added at 37°C and 5% CO2 by volume to make the cells completely adhere to the wall, and a circle of PBS is added at the edge of the 96-well plate to prevent edge effect. After the cells grow to nearly cover the bottom of the 96-well plate, the blank culture medium is aspirated, and the blank control, positive control and bacterial cellulose dressing extract are added. The culture medium is replaced with 200μL of culture medium containing different concentrations of extract (prepared and used), and all concentrations are paralleled 3 times. The treated plate was placed in 5% CO2 and cultured at 37°C for 72h. After the reaction, the original culture medium was replaced, and 100 μL of 10% CCK-8 was added to each well. The plate was placed in a cell culture incubator and incubated for 2h in the dark at 37°C. Finally, the OD value (OD = 450nm) was measured with a multifunctional microplate reader, and the cells of each group were placed under a microscope to observe the culture results.
[0080] The biocompatibility test results of bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1(E), BC-DACA2(E), BC-DACA3(E), BC-DACA4(E)) wound dressings, bacterial cellulose (BC) wound dressings and commercially available hydrocolloid dressings are shown in Figure 2. Figure 6 shown.
[0081] Depend on Figure 6 It can be seen that only the extract of commercially available hydrocolloids has a certain inhibitory effect on the proliferation of human immortalized epidermal cells (HaCaT) (81.38-89.60%), and any multiple dilution of the extract of BC and BC-DACA (E) can promote the proliferation of HaCaT cells. The results show that the BC-DACA (E) composite hydrogel has excellent biocompatibility.
[0082] On the basis of the above examples, in order to further verify the wound healing ability of the wound dressing prepared by the present invention, bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1 (E), BC-DACA2 (E), BC-DACA3 (E), BC-DACA4 (E)) wound dressings, bacterial cellulose (BC) wound dressings and commercially available hydrocolloid dressings were used for animal experiments. The specific experimental process is as follows:
[0083] 8-week-old SD (Sprague-Dawley) rats were used for wound healing experiments. The rats were anesthetized with sodium pentobarbital (80 mg / kg) and shaved, and three full-thickness wound incisions with a diameter of about 1 cm were cut along the outer edge of the circle with surgical scissors. The wounds were covered with bacterial cellulose and bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressings, respectively, and medical sterile gauze and commercially available hydrocolloid dressings were used as controls. The hydrogel wound dressing was fixed to the wound using Tegaderm material and a layer of bandage. The bandage was changed every 2 days from 0 to 6 days at the beginning of the experiment, and every 4 days from 6 to 14 days. The wound healing was observed under a microscope, and the proportion of wound healing area was calculated. On the 7th and 14th days, the wounds and surrounding skin tissues of the rats were fixed with 4% paraformaldehyde, and the fixed skin tissue samples were embedded in paraffin to prepare pathological sections. The tissue sections were stained with hematoxylin-eosin (H&E) and Masson's staining to evaluate the degree of wound healing at different time points.
[0084] The results of animal wound healing ability tests on bacterial cellulose-dialdehyde carboxyl starch composite hydrogel (BC-DACA1(E), BC-DACA2(E), BC-DACA3(E), BC-DACA4(E)) wound dressings, bacterial cellulose (BC) wound dressings and commercially available hydrocolloid dressings are shown in Figure 2. Figure 7 shown.
[0085] Depend on Figure 7 It can be seen that on the 4th day, except for the gauze group, all wounds had obvious growth of new granulation tissue, especially the BC-DACA (E) composite hydrogel, whose wound healing area was significantly higher than that of other groups. On the 14th day, all wounds were basically healed, and there was no large area of scab wound exposed to the outside. From the wound healing area chart, it can be found that the wound healing degree and healing rate of the gauze group were the slowest, and the wound healing degree and healing rate of the BC-DACA group were significantly higher than those of other groups. After the 14th day, all wounds were basically healed, and the wound healing area of the BC-DACA4 (E) group was significantly higher than that of other groups. There was no significant difference in the healing area between the commercially available hydrocolloid and other sample groups. Overall, the sample groups showed good performance in terms of healing degree and healing rate, especially BC-DACA3 (E) showed the fastest healing rate, and BC-DACA4 (E) showed the highest healing degree, indicating that the BC-DACA (E) composite hydrogel has the performance of promoting wound healing. Observation of H&E tissue staining results showed that 7 days after surgery, the wound skin tissue structure of the gauze group and the hydrocolloid group was still severely abnormal; the epidermis was lost in the field of vision, the dermis was exposed (as shown by the red arrow), and the dermis had a large area of collagen fiber loss (as shown by the blue arrow). A large number of inflammatory cells were infiltrated in the tissue (as shown by the yellow arrow), a large number of cells were necrotic, the nucleus was fragmented, and the shrinkage was darkly stained (as shown by the black arrow). The BC group was accompanied by local tissue bleeding (as shown by the brown arrow); the BC-DACA3 (E) and BC-DACA4 (E) groups also had epidermal loss, accompanied by varying degrees of tissue inflammation. 14 days after surgery, the epidermis structure in the BC-DACA4 (E) group was intact in the field of vision, the spinous layer was thin and uniform, no obvious inflammatory reaction was observed, it was closest to the normal skin around the incision, and the thickness of the new granulation tissue was significantly higher than that of the other groups. The results of Masson tissue staining showed that the collagen content in the BC-DACA3(E) and BC-DACA4(E) groups was the highest and the arrangement was more regular.
[0086] In summary, compared with medical sterile gauze, commercially available hydrocolloid dressings and bacterial cellulose hydrogel wound dressings, bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressings have faster and higher abilities to promote wound healing, growth of new granulation tissue and collagen production during long-term (2 weeks) use.
[0087] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.
Claims
1. A method for preparing a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing, characterized in that: The following steps are involved: S1: using carboxylated starch as raw material, dialdehyde carboxylated starch was prepared by periodate oxidation; S2: inoculating the bacterial cellulose producing strain into a fermentation medium, culturing at 25-36°C for 3-5 days to obtain a strain concentrate; the fermentation medium is composed of the following components: 20-25 g / L glucose, 2.0-3.0 g / L anhydrous disodium hydrogen phosphate, 1.0-2.0 g / L citric acid monohydrate, 5-10 g / L yeast extract, 5-10 g / L peptone, and the balance is deionized water, and the pH is adjusted to 4.0-5.0 with 1 mol / L hydrochloric acid solution; S3: inoculating the obtained bacterial concentrate into a fermentation medium at a ratio of 8-15 (v / v)%, placing it in a constant temperature box at 25-36°C for 5-9 days to obtain bacterial cellulose, soaking and washing it with pure water for multiple times until the color is close to white and the pH is neutral, to obtain a bacterial cellulose hydrogel; the fermentation medium is composed of the following components: 20-25 g / L glucose, 2.0-3.0 g / L anhydrous disodium hydrogen phosphate, 1.0-2.0 g / L monohydrate citric acid, 5-10 g / L yeast extract, 5-10 g / L peptone, and the balance deionized water, and adjusting the pH to 4.0-5.0 with 1 mol / L hydrochloric acid solution; S4: Soaking the purified bacterial cellulose in a solution containing 0.5-2% polyvinyl alcohol and dialdehyde carboxyl starch at a mass concentration for 3-5 days to obtain a bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing.
2. The method for preparing the bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing according to claim 1, characterized in that: The preparation method of the carboxyl starch in step S1 is: oxidizing starch in sequence with 2,2,6,6-tetramethylpiperidine-1-oxyl free radical, sodium bromide, and sodium hypochlorite, and dialyzing to obtain the carboxyl starch.
3. The method for preparing the bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing according to claim 1, characterized in that: The molar concentration of sodium periodate in step S1 is 0.5M-1.1M.
4. The method for preparing the bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing according to claim 1, characterized in that: The bacterial cellulose producing bacteria used in step S1 is one of the genus Acetobacter, Acetobacter xylinum, and Komagabatius xylosus.
5. The method for preparing the bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing according to claim 1, characterized in that: In step S2, the total number of bacterial cellulose producing bacteria in each milliliter of bacterial concentrate is 10 2 -10 4 CFU.
6. A bacterial cellulose-dialdehyde carboxyl starch composite hydrogel wound dressing prepared by the method according to any one of claims 1 to 5.
Citation Information
Patent Citations
Application of aldehyde-modified polysaccharide containing carboxyl to preparing medicine and medical material
CN101632685A
Novel medical antibacterial spray
CN106821979A
Bacterial cellulose / polyvinyl alcohol antibacterial hydrogel and preparation method and application thereof
CN109369948A
Functional drug-sustained-release medical dressing constructed by alginic acid aminated derivative / bacterial cellulose nanocrystal composite gel
CN110152055A
Preparation method of high bond strength moisture-permeable wound healing-promoting dressing
CN110302415A
Cited By
Efficient phosphate fertilizer for inhibiting cadmium absorption and preparation method thereof
CN118724652A
A high-efficiency phosphate fertilizer for inhibiting cadmium absorption and preparation method thereof
CN118724652B