Antibacterial film and preparation method thereof
Through the reaction of aldehyde poly(caprolactone-co-lactide) and ε-polylysine, a bacteriostatic film with excellent mechanical properties and antibacterial properties is formed, which solves the mechanical problem of existing wound dressings in frequently moving parts. Issues of insufficient performance and risk of drug resistance, achieving efficient applicability for systemic wound repair.
Patent Information
- Application Number
- CN202410720430.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-08
AI Technical Summary
Existing wound dressings have insufficient mechanical properties when used on frequently moved body parts, leading to shedding problems. In addition, traditional antibacterial materials have high risks of general usability and drug resistance, making it difficult to meet the needs of systemic wound repair.
A porous film is formed from aldehyde poly(caprolactone-co-lactide) fiber, and reacts with the natural polypeptide ε-polylysine to form an antibacterial film with excellent mechanical properties and antibacterial properties, which is suitable for the human body Wound repair in various parts.
The wound dressing used on all parts of the body has good mechanical properties and antibacterial properties, reduces the risk of bacterial resistance, and is suitable for all types of wound repair.
Smart Images

Figure CN118743775A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of antibacterial films, and in particular to an antibacterial film and a preparation method thereof. Background Art
[0002] Wound healing is a natural process, but when the wound is exposed to the outside, it will be threatened by pathogens and may cause serious infection. At present, most traditional dressings choose to make skin accessories into hydrogels, which can make the dressings have better adhesion and moisture retention, but the nature of the hydrogel itself determines its brittle mechanical properties, and it is not suitable for use in active parts of the body. For example, the antibacterial hydrogel dressing for eliminating active oxygen provided by the publication number CN113577377A has uniform and efficient antibacterial properties, but its mechanical properties are poor and easy to break, resulting in falling off from the wound. The electrospun fiber has excellent flexibility and high porosity, can effectively isolate external moisture and maintain air permeability, and its high specific surface area can also promote cell adhesion and cell proliferation and differentiation, which is beneficial to wound tissue repair. According to the literature Synthesis of Poly(l-lactide-co-ε-caprolactone)Copolymer:Structure,Toughness,and Elasticity, PLCL material has excellent mechanical properties, the maximum elastic modulus can reach 46.2±5.9MPa, the maximum elongation at breaking point can reach 2860.0±135.8%, and the mechanical properties of the material can be adjusted by changing the ratio of caprolactone and lactide, so that the material can achieve the expected mechanical performance, which is very suitable for the preparation of electrospinning membranes.
[0003] Functional films have suitable physical and mechanical strength, are waterproof and breathable, and carry antibacterial active ingredients that can kill bacteria and facilitate wound healing. Poly(caprolactone-co-lactide) is a biocompatible polymer approved by the US Food and Drug Administration. It has good elasticity and biocompatibility and is an ideal drug-carrying material. According to the ACS Applied Bio Materials (DOI: 10.1021 / acsabm.9b00353) document published by the research group of Professor Li Peng of the team of Academician Huang Wei of Northwestern Polytechnical University and the research group of Professor Han Chunmao of the Burns Department of the Second Affiliated Hospital of Zhejiang University School of Medicine, the natural polypeptide ε-polylysine is antibacterial, biodegradable, and water-soluble. And the natural polypeptide ε-polylysine inhibits bacterial proliferation by destroying the cell membrane of microorganisms, which can effectively reduce the risk of bacterial resistance. At present, ε-polylysine has been approved for use as a food additive in the United States, South Korea, and Japan. It also has great prospects in the fields of skin tissue repair and bioadhesives, and has been used in the field of drugs / gene carriers. A wound repair dressing provided by publication number CN117752590A adds protocatechuic aldehyde-modified ε-polylysine to give it good antibacterial properties. However, it is a wound dressing for specific body parts, is not universally applicable, and has significantly poor mechanical properties.
[0004] Therefore, developing a material with good antibacterial and mechanical properties that can be used throughout the body is of great significance for human wound repair. Summary of the invention
[0005] The purpose of this application is to provide a new antibacterial film and a preparation method thereof.
[0006] In order to achieve the above objectives, this application adopts the following technical solutions:
[0007] One aspect of the present application discloses an antibacterial film, wherein a porous film formed by fibers of aldehyde-modified poly(caprolactone-co-lactide) reacts with polylysine to form the antibacterial film of the present application.
[0008] It should be noted that the antibacterial film of the present application creatively uses aldehyde-terminated multi-arm poly (caprolactone-co-lactide) as a raw material to prepare the base film, which not only has good safety and biocompatibility, but also has excellent mechanical properties. When used as a medical dressing, it can be better suitable for repairing various wounds; and polylysine is used to further modify the surface of the porous film to give it good antibacterial properties. Therefore, the antibacterial film of the present application has excellent mechanical properties, antibacterial properties and biocompatibility, and can be used as an antibacterial dressing for various parts of the human body according to the use requirements.
[0009] In one implementation of the present application, the porous film is made of aldehyde-modified poly(caprolactone-co-lactide) by electrospinning.
[0010] It should be noted that electrospinning is a specific method for preparing the porous film in one implementation of the present application. It is not excluded that other methods can be used to form the porous film, such as first forming aldehyde-modified poly (caprolactone-co-lactide) fibers, and then forming the porous film through other textile technologies or non-woven fabric technologies. No specific limitation is made here.
[0011] In one implementation of the present application, polylysine is connected to the aldehyde group on the surface of the porous film through its amino group through a Schiff base reaction, thereby forming the antibacterial film of the present application.
[0012] Another aspect of the present application discloses a method for preparing the antibacterial film of the present application, comprising immersing a porous film formed by fibers of aldehyde-modified poly(caprolactone-co-lactide) in an aqueous solution of polylysine. After the immersion is completed, the porous film is taken out, cleaned with ethanol, and dried to obtain the antibacterial film of the present application.
[0013] In one implementation of the present application, the soaking condition is 20-30° C. for 12-48 hours.
[0014] In one implementation of the present application, after soaking, cold ethanol at 2-8° C. is used for cleaning.
[0015] In one implementation of the present application, cold ethanol is used for washing at least 3 times.
[0016] It should be noted that in the preparation method of the present application, the purpose of ethanol washing is mainly to remove excess polylysine; in principle, as long as the polylysine can be effectively removed by washing, it is not limited to washing with cold ethanol. As for the number of washings, generally 3 times is sufficient; of course, the number of washings can also be adjusted according to actual conditions.
[0017] In one implementation of the present application, the porous film is immersed, cleaned and then dried by vacuum drying.
[0018] In one implementation of the present application, the time for vacuum drying the porous film is 12-48 hours.
[0019] It should be noted that in the preparation method of the present application, the purpose of drying the porous film is to remove excess solvent, such as ethanol used in washing and solvent in electrospinning; therefore, vacuum drying is preferably used. As for the drying time, vacuum drying for 12-48 hours is generally sufficient, such as vacuum drying for 12 hours, 20 hours, 24 hours, 30 hours, 36 hours or 48 hours.
[0020] In one implementation of the present application, the porous film is made by electrospinning, specifically including dissolving aldehyde-modified poly(caprolactone-co-lactide) in a solvent to prepare an electrospinning solution, and electrospinning the electrospinning solution to obtain the porous film of the present application.
[0021] In one implementation of the present application, the solvent for preparing the electrospinning solution is at least one of hexafluoroisopropanol, chloroform, dichloromethane and N,N-dimethylformamide.
[0022] Preferably, the solvent for preparing the electrospinning solution is a mixed solvent of dichloromethane and N,N-dimethylformamide.
[0023] Preferably, the volume ratio of dichloromethane to N,N-dimethylformamide in the mixed solvent is 7:3.
[0024] In one implementation of the present application, 1 g of formaldehyded poly(caprolactone-co-lactide) is dissolved in 5-10 mL of a mixed solvent of dichloromethane and N,N-dimethylformamide to form the electrospinning solution of the present application.
[0025] It should be noted that the ratio of formaldehyde-modified poly (caprolactone-co-lactide) and dichloromethane is mainly determined according to the use requirements of electrospinning. Different electrospinning equipment may have different requirements for parameters. It is only necessary to appropriately adjust the ratio of formaldehyde-modified poly (caprolactone-co-lactide) and dichloromethane, and no specific limitation is made here.
[0026] In one implementation of the present application, the aldehyde-modified poly(caprolactone-co-lactide) is prepared by the following method:
[0027] (1) drying the mixture of lactide and caprolactone under vacuum;
[0028] (2) adding an initiator to the product of step (1), heating to 100-140° C. and stirring for 1-5 h, adding a catalyst, and reacting at 110-130° C. under inert atmosphere with stirring for 10-24 h;
[0029] (3) adding a solvent to the product of step (2) to obtain a solution; pouring the solution into ice methanol or cold petroleum ether at 2-8° C., stirring while pouring, and drying to obtain a hydroxyl-terminated multi-arm poly(caprolactone-co-lactide);
[0030] (4) dissolving the hydroxyl-terminated multi-arm poly(caprolactone-co-lactide) obtained in step (3) in a solvent to prepare a reaction solution, adding p-formylbenzoic acid, dicyclohexylcarbodiimide, and 4-dimethylaminopyridine to the reaction solution under ice-water bath conditions, stirring and reacting for 24-48 hours under inert atmosphere protection at room temperature, centrifuging to remove insoluble impurities, using 2-8°C ice methanol or cold petroleum ether to precipitate a solid product, using 2-8°C ice methyl tert-butyl ether to wash the solid product, and drying to obtain the formaldehyde-modified poly(caprolactone-co-lactide).
[0031] In one implementation of the present application, the molar ratio of lactide to caprolactone in step (1) is 1:(1-4).
[0032] In one implementation of the present application, the initiator in step (2) is at least one of propylene glycol, pentaerythritol and dipentaerythritol.
[0033] In one implementation of the present application, the molar ratio of the initiator to the lactide is 1:(10-30).
[0034] In one implementation of the present application, the catalyst of step (2) is at least one of stannous octoate, tin isooctanoate and stannous isooctanoate.
[0035] In one implementation of the present application, the molar amount of the catalyst is marked as m1, the sum of the molar amounts of the initiator, lactide and caprolactone is marked as m2, and m1:m2=1:(2000-3000).
[0036] In one implementation of the present application, the inert atmosphere used in step (2) is argon or nitrogen.
[0037] In one implementation of the present application, the solvent in step (3) is dichloromethane.
[0038] In one implementation of the present application, after drying, the mixture is washed at least once with ice methanol or cold petroleum ether at 2-8°C.
[0039] In one implementation of the present application, the amount of ice methanol or cold petroleum ether used is at least 10 times the volume of the solution.
[0040] In one implementation of the present application, the drying method in step (3) is drying in a vacuum drying oven for 24-48 hours.
[0041] In one implementation of the present application, the solvent in step (4) is dichloromethane.
[0042] In one implementation of the present application, the molar ratio of the p-formylbenzoic acid in step (4) to the initiator in step (2) is (5-10):1.
[0043] In one implementation of the present application, the molar ratio of p-formylbenzoic acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 1:1:(0.2-0.3).
[0044] In one implementation of the present application, the inert atmosphere used in step (4) is argon or nitrogen.
[0045] Due to the adoption of the above technical solution, the beneficial effects of this application are:
[0046] The antibacterial film of the present application uses aldehyde-terminated multi-arm poly (caprolactone-co-lactide) as a raw material to prepare a porous film with good safety, good biocompatibility and excellent mechanical properties; the surface of the porous film is further modified with polylysine to give it good antibacterial properties. Therefore, the antibacterial film of the present application has excellent mechanical properties, antibacterial properties and biocompatibility, and when used as a medical antibacterial dressing, it can be applied to wound repair in various parts of the body. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 It is a synthetic route of the antibacterial film poly(caprolactone-co-lactide)-polylysine porous film in the embodiment of the present application;
[0048] Figure 2 is the NMR spectrum of the antibacterial film poly(caprolactone-co-lactide)-polylysine porous film in the embodiment of the present application;
[0049] Figure 3 This is a physical picture of the antibacterial film poly(caprolactone-co-lactide)-polylysine porous film in the embodiment of the present application;
[0050] Figure 4 is a microscopic structure diagram of the antibacterial film poly(caprolactone-co-lactide)-polylysine porous film in the embodiment of the present application;
[0051] Figure 5 1 is a graph showing the elastic modulus test results of the antibacterial film poly(caprolactone-co-lactide)-polylysine porous film in the embodiment of the present application;
[0052] Figure 6 This is a graph showing the elongation at break test result of the antibacterial film poly(caprolactone-co-lactide)-polylysine porous film in the examples of the present application. DETAILED DESCRIPTION
[0053] The present application creatively develops an antibacterial film formed by the reaction of a porous film formed by aldehyde-modified poly(caprolactone-co-lactide) fibers and polylysine. The synthetic route of the antibacterial film of the present application is as follows: Figure 1As shown, it includes reacting lactide and caprolactone under the action of an initiator and a catalyst to generate poly(caprolactone-co-lactide), adding p-formylbenzoic acid, DCC and DMAP to prepare aldehyde-terminated poly(caprolactone-co-lactide), electrospinning it to make a porous film formed of aldehyded poly(caprolactone-co-lactide) fibers, and soaking it in polylysine to obtain the poly(caprolactone-co-lactide) polylysine electrospun membrane of the present application, that is, the antibacterial film of the present application.
[0054] The present application is further described in detail below through specific examples. The following examples are only used to further illustrate the present application and should not be construed as limiting the present application.
[0055] Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art.
[0056] Example 1
[0057] The preparation method of the antibacterial film of this example includes:
[0058] (1) 2.2184 g of lactide and 1.7562 g of caprolactone were placed in a glass reactor and dried overnight under vacuum, wherein the molar ratio of lactide to caprolactone was 1:1;
[0059] (2) Add 0.0254 g of initiator glycerol to a dried glass reactor, heat it to 140° C., and stir until the solution in the reactor becomes clear and transparent; then add 0.005 g of catalyst stannous octoate and cool it to 110° C., stir and react for 24 h; the whole process is protected by argon;
[0060] (3) using 20 mL of dichloromethane to dissolve the product of step (2) to obtain a solution, pouring the solution into 10 times the volume of 4° C. ice methanol, stirring while pouring, and after completion, placing the solution in a vacuum drying oven to dry, and then washing the dried product with 10 times the volume of 4° C. ice methanol, repeating the washing with ice methanol for 3 times, and finally placing the solution in a vacuum drying oven to dry, thereby obtaining a hydroxyl-terminated multi-arm poly(caprolactone-co-lactide);
[0061] (4) using dichloromethane to dissolve the hydroxyl-terminated multi-arm poly (caprolactone-co-lactide), adding 0.225 g of p-formylbenzoic acid, 0.04575 g of DCC, and 0.309 g of DMAP in an ice water bath; stirring at room temperature for 24 hours, separating insoluble impurities using a centrifuge, and collecting the liquid; slowly pouring the liquid into 10 times the volume of 4°C ice petroleum ether, while rapidly stirring to precipitate the product, filtering out the solid product using vacuum filtration, and then washing the solid three times with 4°C ice methyl tert-butyl ether, and drying it in a vacuum drying oven for 24 hours to obtain the aldehyde-terminated multi-arm poly (caprolactone-co-lactide);
[0062] (5) dissolving the product of step (4) in a dichloromethane / N,N-dimethylformamide mixed solution at a ratio of 1 g:10 mL to prepare an electrospinning solution, and electrospinning the electrospinning solution to obtain an aldehyde-terminated multi-arm poly(caprolactone-co-lactide) fiber porous membrane, i.e., a porous film formed by aldehyde-terminated poly(caprolactone-co-lactide) fibers; the volume ratio of dichloromethane to N,N-dimethylformamide in the mixed solvent is 7:3;
[0063] (6) Prepare an ε-polylysine / ultrapure water solution with a concentration of 12 g / L, cut the porous film formed by the aldehyde-modified poly(caprolactone-co-lactide) fibers into 10 cm*10 cm pieces and soak them in the stirred ε-polylysine / ultrapure water solution for 24 h; take out and wash it three times with 4°C cold ethanol, and dry it in a vacuum drying oven for 24 h to obtain the poly(caprolactone-co-lactide)-polylysine electrospun membrane, i.e., the antibacterial film in this example.
[0064] Example 2
[0065] The preparation method of the antibacterial film of this example includes:
[0066] (1) 2.313 g of lactide and 3.662 g of caprolactone were placed in a glass reactor and dried overnight under vacuum, wherein the molar ratio of lactide to caprolactone was 1:2;
[0067] (2) Add 0.0254 g of propylene glycol to a dried glass reactor, heat it to 140° C., and stir until the solution in the reactor becomes clear and transparent; then add 0.00782 g of stannous octoate and cool it to 110° C., stir and react for 18 h; nitrogen protection is used throughout the process;
[0068] (3) using 20 mL of dichloromethane to dissolve the product of step (2) to obtain a solution, pouring the solution into 10 times the volume of 4° C. ice methanol, stirring while pouring, and after completion, placing the solution in a vacuum drying oven to dry, and then washing the dried product with 10 times the volume of 4° C. ice methanol, repeating the washing with ice methanol for 3 times, and finally placing the solution in a vacuum drying oven to dry, thereby obtaining a hydroxyl-terminated multi-arm poly(caprolactone-co-lactide);
[0069] (4) using dichloromethane to dissolve the hydroxyl-terminated multi-arm poly (caprolactone-co-lactide), adding 0.225 g of p-formylbenzoic acid, 0.04575 g of DCC, and 0.309 g of DMAP in an ice water bath; stirring at room temperature for 24 hours, separating insoluble impurities using a centrifuge, and collecting the liquid; slowly pouring the liquid into 10 times the volume of ice petroleum ether, while rapidly stirring to precipitate the product, filtering out the solid product using vacuum filtration, and then washing the solid three times with ice methyl tert-butyl ether, and drying it in a vacuum drying oven for 24 hours to obtain the aldehyde-terminated multi-arm poly (caprolactone-co-lactide);
[0070] (5) dissolving the product of step (4) in a dichloromethane / N,N-dimethylformamide mixed solution at a ratio of 1 g:5 mL to prepare an electrospinning solution, electrospinning the electrospinning solution to obtain an aldehyde-terminated multi-arm poly(caprolactone-co-lactide) fiber porous membrane, i.e., a porous film formed by aldehyde-terminated poly(caprolactone-co-lactide) fibers; the volume ratio of dichloromethane to N,N-dimethylformamide in the mixed solvent is 7:3;
[0071] (6) Prepare an ε-polylysine / ultrapure water solution with a concentration of 12 g / L, cut the aldehyde-terminated multi-arm poly(caprolactone-co-lactide) electrospun membrane into 10 cm*10 cm pieces and soak it in the stirred ε-polylysine / ultrapure water solution for 24 h; take it out and wash it with cold ethanol for 3 times, and dry it in a vacuum drying oven for 24 h to obtain an antibacterial poly(caprolactone-co-lactide)-polylysine electrospun membrane, i.e., the antibacterial film in this example.
[0072] Example 3
[0073] The preparation method of the antibacterial film of this example includes:
[0074] (1) 2.363 g of lactide and 5.612 g of caprolactone were placed in a glass reactor and dried overnight under vacuum, wherein the molar ratio of lactide to caprolactone was 1:3;
[0075] (2) Add 0.0254 g of propylene glycol to a dried glass reactor, heat it to 140° C., and stir until the solution in the reactor becomes clear and transparent; then add 0.0106 g of stannous octoate and cool it to 110° C., stir and react for 16 h; the whole process is protected by argon;
[0076] (3) using 20 mL of dichloromethane to dissolve the product of step (2) to obtain a solution, pouring the solution into 10 times the volume of 4° C. ice methanol, stirring while pouring, and after completion, placing the solution in a vacuum drying oven to dry, and then washing the dried product with 10 times the volume of 4° C. ice methanol, repeating the washing with ice methanol for 3 times, and finally placing the solution in a vacuum drying oven to dry, thereby obtaining a hydroxyl-terminated multi-arm poly(caprolactone-co-lactide);
[0077] (4) using dichloromethane to dissolve the hydroxyl-terminated multi-arm poly (caprolactone-co-lactide), adding 0.225 g of p-formylbenzoic acid, 0.04575 g of DCC, and 0.309 g of DMAP in an ice water bath; stirring at room temperature for 24 hours, separating insoluble impurities using a centrifuge, and collecting the liquid; slowly pouring the liquid into 10 times the volume of ice petroleum ether while rapidly stirring to precipitate the product, filtering out the solid product using vacuum filtration, and then washing the solid three times with ice methyl tert-butyl ether, and drying it in a vacuum drying oven for 24 hours to obtain the aldehyde-terminated multi-arm poly (caprolactone-co-lactide);
[0078] (5) dissolving the product of step (4) in a dichloromethane / N,N-dimethylformamide mixed solution at a ratio of 1 g:10 mL to prepare an electrospinning solution, and electrospinning the electrospinning solution to obtain an aldehyde-terminated multi-arm poly(caprolactone-co-lactide) fiber porous membrane, i.e., a porous film formed by aldehyde-terminated poly(caprolactone-co-lactide) fibers; the volume ratio of dichloromethane to N,N-dimethylformamide in the mixed solvent is 7:3;
[0079] (6) Prepare an ε-polylysine / ultrapure water solution with a concentration of 12 g / L, cut the aldehyde-terminated multi-arm poly(caprolactone-co-lactide) electrospun membrane into 10 cm*10 cm pieces and soak it in the stirred ε-polylysine / ultrapure water solution for 24 h; take it out and wash it with cold ethanol for 3 times, and dry it in a vacuum drying oven for 24 h to obtain an antibacterial poly(caprolactone-co-lactide)-polylysine electrospun membrane, i.e., the antibacterial film in this example.
[0080] Example 4
[0081] The preparation method of the antibacterial film of this example includes:
[0082] (1) 2.313 g of lactide and 7.324 g of caprolactone were placed in a glass reactor and dried overnight under vacuum, wherein the molar ratio of lactide to caprolactone was 1:4;
[0083] (2) Add 0.0254 g of propylene glycol to a dried glass reactor, heat to 140° C., and stir until the solution in the reactor becomes clear and transparent; then add 0.0130 g of stannous octoate and cool to 110° C., stir and react for 15 h; argon protection throughout the process;
[0084] (3) using 20 mL of dichloromethane to dissolve the product of step (2) to obtain a solution, pouring the solution into 10 times the volume of 4° C. ice methanol, stirring while pouring, and after completion, placing the solution in a vacuum drying oven to dry, and then washing the dried product with 10 times the volume of 4° C. ice methanol, repeating the washing with ice methanol for 3 times, and finally placing the solution in a vacuum drying oven to dry, thereby obtaining a hydroxyl-terminated multi-arm poly(caprolactone-co-lactide);
[0085] (4) using dichloromethane to dissolve the hydroxyl-terminated multi-arm poly (caprolactone-co-lactide), adding 0.225 g of p-formylbenzoic acid, 0.04575 g of DCC, and 0.309 g of DMAP in an ice water bath; stirring at room temperature for 24 hours, separating insoluble impurities using a centrifuge, and collecting the liquid; slowly pouring the liquid into 10 times the volume of ice petroleum ether while rapidly stirring to precipitate the product, filtering out the solid product using vacuum filtration, and then washing the solid three times with ice methyl tert-butyl ether, and drying it in a vacuum drying oven for 24 hours to obtain the aldehyde-terminated multi-arm poly (caprolactone-co-lactide);
[0086] (5) dissolving the product of step (4) in a dichloromethane / N,N-dimethylformamide mixed solution at a ratio of 1 g:10 mL to prepare an electrospinning solution, and electrospinning the electrospinning solution to obtain an aldehyde-terminated multi-arm poly(caprolactone-co-lactide) fiber porous membrane, i.e., a porous film formed by aldehyde-terminated poly(caprolactone-co-lactide) fibers; the volume ratio of dichloromethane to N,N-dimethylformamide in the mixed solvent is 7:3;
[0087] (6) Prepare an ε-polylysine / ultrapure water solution with a concentration of 12 g / L, cut the aldehyde-terminated multi-arm poly(caprolactone-co-lactide) electrospun membrane into 10 cm*10 cm pieces and soak it in the stirred ε-polylysine / ultrapure water solution for 24 h; take it out and wash it with cold ethanol for 3 times, and dry it in a vacuum drying oven for 24 h to obtain an antibacterial poly(caprolactone-co-lactide)-polylysine electrospun membrane, i.e., the antibacterial film in this example.
[0088] Comparative Example
[0089] The method for preparing the film of this example includes:
[0090] (1) 4.465 g of lactide and 3.535 g of caprolactone were placed in a glass reactor and dried overnight under vacuum, wherein the molar ratio of lactide to caprolactone was 1:1;
[0091] (2) Raise the temperature to 140°C, stir until the solution in the reactor is clear and transparent, then add 0.01 g of stannous octoate and cool to 110°C, stir and react for 17 hours; argon protection throughout the process; this example compares the effect of not adding an initiator on the film;
[0092] (3) using 20 mL of dichloromethane to dissolve the product of step (2) to obtain a solution, pouring the solution into 10 times the volume of 4° C. ice methanol, stirring while pouring, and after completion, placing the solution in a vacuum drying oven to dry, and then washing the dried product with 10 times the volume of 4° C. ice methanol, repeating the washing with ice methanol for 3 times, and finally placing the solution in a vacuum drying oven to dry, thereby obtaining a hydroxyl-terminated multi-arm poly(caprolactone-co-lactide);
[0093] (4) using dichloromethane to dissolve the hydroxyl-terminated multi-arm poly (caprolactone-co-lactide), adding 0.45 g of p-formylbenzoic acid, 0.0915 g of DCC, and 0.618 g of DMAP in an ice water bath; stirring at room temperature for 24 hours, separating insoluble impurities using a centrifuge, and collecting the liquid; slowly pouring the liquid into 10 times the volume of ice petroleum ether while rapidly stirring to precipitate the product, filtering out the solid product using vacuum filtration, and then washing the solid with ice methyl tert-butyl ether for 2-3 times, and drying it in a vacuum drying oven for 24 hours to obtain the aldehyde-terminated multi-arm poly (caprolactone-co-lactide);
[0094] (5) The product of step (4) is dissolved in a dichloromethane / N,N-dimethylformamide mixed solution at a ratio of 1 g:10 mL to prepare an electrospinning solution, and the electrospinning solution is electrospun to obtain an aldehyde-terminated multi-arm poly(caprolactone-co-lactide) fiber porous membrane as the film of this example; wherein the volume ratio of dichloromethane to N,N-dimethylformamide in the mixed solvent is 7:3.
[0095] The antibacterial film prepared in Example 1 was subjected to NMR analysis, and its NMR spectrum is shown as follows: Figure 2 As shown, Figure 2 The results show that polylysine is connected to the aldehyde group on the surface of the porous film through its amino group through Schiff base reaction. The structural formula of poly(caprolactone-co-lactide)-polylysine prepared in Example 1 is as follows:
[0096]
[0097] The antibacterial film prepared in Example 1 is as follows Figure 3 Its microstructure is shown in Figure 4 shown. Figure 4 It can be clearly seen that the antibacterial film is a porous film structure formed by the fibers of aldehyde-modified poly(caprolactone-co-lactide).
[0098] The antibacterial films prepared in Examples 1 to 4 and the films prepared in the comparative examples were subjected to antibacterial performance tests, mechanical property tests and cell compatibility tests, as follows:
[0099] Antibacterial rate test
[0100] The antibacterial films of Examples 1-4 and the films of the comparative example were subjected to antibacterial tests, the bacterial species being Gram-positive Staphylococcus aureus and Gram-positive Escherichia coli, and the antibacterial activity was evaluated, and the reference standard was WS / T650-2019.
[0101] Follow the following experimental method: Take the test bacteria and prepare PB into about 10 5 CFU / mL~10 6 CFU / mL concentration of bacterial suspension. Use sterile scissors to cut the test sample and control sample into 20mm×30mm pieces under sterile conditions for standby use. All standby pieces are sterilized by high-pressure steam. Use sterile tweezers to clamp the test sample and control sample and place them on a sterile plate. Each sample does not overlap. Place the culture plate in a water bath at 20℃±1℃ for 5min. Add 0.1mL of the test bacterial suspension to each sample. Immediately start the live bacteria culture counting method to determine the number of surviving bacteria. Take 1mL of solution from each test tube and inoculate 2 plates with each tube of solution. If the number of colonies growing on the plate is large, it can be diluted 10 times in series and then the live bacteria culture count can be performed. All samples were cultured in an atmosphere of 36℃±1℃. The test was repeated 3 times and the inhibition rate was calculated. The experimental results are shown in Table 1.
[0102] Table 1 Antibacterial rate test results
[0103]
[0104]
[0105] The results in Table 1 show that the antibacterial poly(caprolactone-co-lactide)-polylysine electrospinning membranes prepared in Examples 1 to 4 have obvious antibacterial properties, and the antibacterial properties come from polylysine.
[0106] Material mechanical properties test
[0107] A tensile test machine was used to perform tensile tests on each sample at room temperature. The sample size was 5 cm × 3 cm × 0.2 mm (length × width × thickness). The tensile rate was set to 5 mm / min. At least 5 tests were performed on each sample, and the average value was calculated. The test results are shown in Figure 2. Figure 5 and Figure 6As shown, Figure 5 is the elastic modulus test result, Figure 6 This is the elongation at breaking point test result.
[0108] result Figure 5 and Figure 6 The results show that the addition of glycerol has some effect on the mechanical properties of the material, but it is small; the ratio of lactide to caprolactone has a greater impact on the mechanical properties of the material. The results show that when the ratio of lactide in the material increases, the elastic modulus of the material also increases, and the corresponding elongation at break of the material also decreases.
[0109] The above contents are further detailed descriptions of the present application in combination with specific implementation methods, and it cannot be determined that the specific implementation of the present application is limited to these descriptions. For ordinary technicians in the technical field to which the present application belongs, several simple deductions or substitutions can be made without departing from the concept of the present application.
Claims
1. An antibacterial film, characterized in that: A porous film formed from fibers of aldehyded poly(caprolactone-co-lactide) is reacted with polylysine.
2. The antibacterial film according to claim 1, characterized in that: The porous film is made of aldehyde-modified poly(caprolactone-co-lactide) through electrostatic spinning.
3. The antibacterial film according to claim 1 or 2, characterized in that: The polylysine is connected to the aldehyde group on the surface of the porous film through the amino group thereof by Schiff base reaction.
4. The method for preparing the antibacterial film according to any one of claims 1 to 3, characterized in that: The method comprises soaking a porous film formed by aldehyded poly(caprolactone-co-lactide) fibers in a polylysine aqueous solution, taking out the porous film after soaking, washing it with ethanol, and drying it to obtain the antibacterial film.
5. The preparation method according to claim 4, characterized in that: The soaking condition is 20-30° C. for 12-48 hours; Preferably, after soaking, cold ethanol at 2-8°C is used for washing; Preferably, washing with cold ethanol is performed at least 3 times; Preferably, the drying method is vacuum drying; Preferably, the vacuum drying time is 12-48 hours.
6. The preparation method according to claim 4 or 5, characterized in that: The porous film is made by electrospinning, specifically comprising dissolving aldehyde-modified poly(caprolactone-co-lactide) in a solvent to prepare an electrospinning solution, and electrospinning the electrospinning solution to obtain the porous film; Preferably, the solvent is at least one of hexafluoroisopropanol, chloroform, dichloromethane and N,N-dimethylformamide; Preferably, the solvent is a mixed solvent of dichloromethane and N,N-dimethylformamide; Preferably, the volume ratio of dichloromethane to N,N-dimethylformamide in the mixed solvent is 7:3; Preferably, 1 g of aldehyded poly(caprolactone-co-lactide) is dissolved in 5-10 mL of the mixed solvent to form the electrospinning solution.
7. The preparation method according to claim 4 or 5, characterized in that: The aldehyde-modified poly(caprolactone-co-lactide) is prepared by the following method; (1) drying the mixture of lactide and caprolactone under vacuum; (2) adding an initiator to the product of step (1), heating to 100-140° C. and stirring for 1-5 h, adding a catalyst, and reacting at 110-130° C. under inert atmosphere with stirring for 10-24 h; (3) adding a solvent to the product of step (2) to obtain a solution; pouring the solution into ice methanol or cold petroleum ether at 2-8° C., stirring while pouring, and drying to obtain a hydroxyl-terminated multi-arm poly(caprolactone-co-lactide); (4) dissolving the hydroxyl-terminated multi-arm poly(caprolactone-co-lactide) obtained in step (3) in a solvent to prepare a reaction solution, adding p-formylbenzoic acid, dicyclohexylcarbodiimide, and 4-dimethylaminopyridine to the reaction solution under ice-water bath conditions, stirring and reacting for 24-48 hours under inert atmosphere protection at room temperature, centrifuging to remove insoluble impurities, using 2-8°C ice methanol or cold petroleum ether to precipitate a solid product, using 2-8°C ice methyl tert-butyl ether to wash the solid product, and drying to obtain the formaldehyde-modified poly(caprolactone-co-lactide).
8. The preparation method according to claim 7, characterized in that: In step (1), the molar ratio of lactide to caprolactone is 1:(1-4).
9. The preparation method according to claim 7, characterized in that: In step (2), the initiator is at least one of propylene glycol, pentaerythritol and dipentaerythritol; Preferably, the molar ratio of initiator to lactide is 1:(10-30); Preferably, the catalyst is at least one of stannous octoate, stannous isooctanoate and stannous isooctanoate; Preferably, the molar amount of the catalyst is marked as m1, and the sum of the molar amounts of the initiator, lactide and caprolactone is marked as m2, m1:m2=1:(2000-3000); Preferably, the inert atmosphere in step (2) is argon or nitrogen.
10. The preparation method according to claim 7, characterized in that: In step (3), the solvent is dichloromethane; Preferably, in step (3), after drying, the mixture is washed at least once with ice methanol or cold petroleum ether at 2-8°C; Preferably, in step (3), the amount of icy methanol or cold petroleum ether used is at least 10 times the volume of the solution; Preferably, in step (3), the drying method is drying in a vacuum drying oven for 24-48 hours; Preferably, in step (4), the solvent is dichloromethane; Preferably, in step (4), the molar ratio of p-formylbenzoic acid to the initiator in step (2) is (5-10):1; Preferably, in step (4), the molar ratio of p-formylbenzoic acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 1:1:(0.2-0.3); Preferably, the inert atmosphere in step (4) is argon or nitrogen.
Citation Information
Patent Citations
Active oxygen-eliminating antibacterial and anti-inflammatory hydrogel skin dressing and preparation method thereof
CN113577377A
Gynecological pelvic floor repair external dressing and preparation method thereof
CN117752590A