Modified polyvinylidene fluoride membrane for adsorbing heavy metals and preparation method thereof
The modified polyvinylidene fluoride membrane is prepared by electrospinning technology, combined with the dopamine self-polymerization effect, which solves the problems of low efficiency and complicated preparation of existing adsorption materials, achieves efficient removal of mercury ions in water, and simplifies the process flow.
Patent Information
- Application Number
- CN202411013180.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Existing adsorption materials have low efficiency in removing mercury ions from water and are difficult to recycle, and their preparation methods are complex, resulting in insufficient adsorption capacity and unstable performance.
Electrospinning technology is used to blend thiol polypyrrole and polyvinylidene fluoride, and a polydopamine layer is deposited on the membrane surface through the dopamine self-polymerization effect to form a modified polyvinylidene fluoride membrane to improve its hydrophilicity and adsorption performance.
It achieves the ability to efficiently remove mercury ions in water, with an adsorption rate of 77.74% to 99.26%, and simplifies the preparation process, making it suitable for industrial application.
Smart Images

Figure CN118743983A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional nanomaterials, in particular to a modified polyvinylidene fluoride membrane for adsorbing heavy metals and a preparation method thereof. Background Art
[0002] With the continuous development of industry, the discharge of heavy metal wastewater is increasing day by day. Its toxicity and enrichment have a significant environmental impact on the natural world and cause serious physiological health problems to organisms. Among them, mercury is an extremely toxic heavy metal substance. Among many environmental pollutant indicators, it is listed as the first category of pollutants. Mercury has inherent solubility and stability, and can accumulate in organisms even at very low concentrations. Mercury pollution in water bodies is mainly caused by human activities, the most important of which is the arbitrary discharge of industrial wastewater from factories that produce mercury or use mercury compounds. Mercury (Hg(II)) ions in water are highly active and easily methylated. Methylmercury is quickly absorbed into the animal body and accumulates in the brain, liver and kidneys, which is extremely toxic. Therefore, reducing the content of mercury ions in wastewater before discharge is the focus of research in the field of mercury pollution control in the water environment.
[0003] Traditional adsorption materials have the problem of low adsorption capacity and non-recyclability. How to design and synthesize an adsorption material with large adsorption capacity, high efficiency and recyclability is an urgent problem to be solved. Membrane adsorption is a new adsorption technology that combines membrane technology with chemical adsorption technology. It connects functional groups to the surface and pore walls of polymer membranes to make a membrane adsorbent; the target pollutants can be selectively adsorbed by the functional groups on the membrane adsorbent, effectively separating them from the contaminated water. Membrane adsorption has the advantages of low cost, good removal effect, and strong operability. Moreover, while membrane adsorption is in progress, membrane filtration can also be achieved, which greatly simplifies the sewage treatment process.
[0004] There are many methods for preparing thin films, such as phase separation, self-assembly and electrospinning. Among them, electrospun films have high porosity, large surface area, excellent mechanical properties, thickness, controllable biological properties, and a wide range of raw material sources. By changing the relevant process parameters of electrospinning, the surface morphology, orientation, mechanical properties, etc. of the electrospun film can be regulated. The main methods for modifying membrane materials include surface coating, physical blending and surface grafting. These modification methods can significantly improve the hydrophilicity, anti-pollution properties and other properties of the membrane, but there are problems in the prior art such as complex preparation methods and easy loss of added functional monomers.
[0005] In summary, an adsorption membrane and preparation method with simple preparation, excellent mechanical properties, high stability and good adsorption performance are urgently needed to be developed. Summary of the invention
[0006] The purpose of the present invention is to provide a modified polyvinylidene fluoride membrane for adsorbing heavy metals and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art and achieve efficient removal of mercury ions in mercury ion-contaminated water.
[0007] To achieve the above object, the present invention provides the following solutions:
[0008] The present invention provides a method for preparing a modified polyvinylidene fluoride film, comprising the following steps:
[0009] The mercapto polypyrrole and polyvinylidene fluoride are mixed in a solvent to obtain an electrospinning solution;
[0010] The electrospinning solution is subjected to electrospinning treatment to obtain a PVDF-PPySH membrane;
[0011] Soaking the PVDF-PPySH membrane in anhydrous ethanol to obtain an activated PVDF-PPySH membrane;
[0012] The activated PVDF-PPySH membrane is immersed in a dopamine solution to obtain the modified polyvinylidene fluoride membrane.
[0013] As a further preferred embodiment of the present invention, the mercapto polypyrrole is obtained by oxidative polymerization of mercaptoacetic acid and pyrrole. More specifically, mercaptoacetic acid is added to a pyrrole aqueous solution, and oxidative polymerization is performed, and then washed and dried to obtain polypyrrole grafted with mercapto groups, i.e., mercapto polypyrrole;
[0014] As further preferred embodiment of the present invention, the solvent includes dimethyl sulfoxide, N,N-dimethylformamide or acetone.
[0015] More preferably, mercaptopolypyrrole and polyvinylidene fluoride are first heated and dissolved in solvent A (dimethyl sulfoxide or N,N-dimethylformamide), and then solvent B (acetone) is added to obtain a spinning solution. The temperature for heating and dissolving is preferably 70°C.
[0016] More preferably, the volume ratio of solvent A to solvent B is 8 mL:4-6 mL.
[0017] As a further preferred embodiment of the present invention, the ambient temperature of the electrospinning treatment is 25-30° C., and the voltage is 10-12 kV, more preferably 11 kV.
[0018] The more preferred electrospinning processing parameters are: ambient temperature of 25-30°C, receiving distance of 10-12cm, propulsion flow rate of 0.70mL / h, spinning time of 5 hours, voltage of 11kV, drum speed of 400r / min, and slide scanning speed of 30mm / s.
[0019] As a further preferred embodiment of the present invention, the mercapto polypyrrole and polyvinylidene fluoride (CH2CF2) n The mass ratio of is 0.05g-0.55g:1g. Wherein, the molecular weight of polyvinylidene fluoride is 500,000-1,000,000, more preferably 700,000.
[0020] As a further preferred embodiment of the present invention, the PVDF-PPySH membrane is immersed in anhydrous ethanol for 1 hour.
[0021] As a further preferred embodiment of the present invention, the concentration of the dopamine solution is 4 mg / mL.
[0022] As a further preference of the present invention, the soaking time is 7 hours.
[0023] The present invention also provides a modified polyvinylidene fluoride film prepared by the above preparation method.
[0024] The present invention further provides the use of the modified polyvinylidene fluoride membrane in removing Hg(II) ions in water.
[0025] Polyvinylidene fluoride (PVDF) has good film-forming properties, is thermally stable and resistant to chemical corrosion, and is one of the main film-forming materials. However, its inherent hydrophobicity and the lack of active functional groups on its surface limit its application in the adsorption field.
[0026] The present invention bulk blends mercapto polypyrrole in polyvinylidene fluoride spinning solution, spins it into a film through electrostatic spinning technology, and then utilizes the self-polymerization effect of dopamine (DA) to deposit a polydopamine (PDA) layer on the surface of the base film to make the material hydrophilic.
[0027] In the present invention, the thiol functional group containing thioglycolic acid plays an important role in the mercury removal process due to its strong ability to combine soft acidic mercury with soft alkaline mercaptan.
[0028] The present invention discloses the following technical effects:
[0029] The present invention makes technical improvements on the performance defects of polyvinylidene fluoride (PVDF), blends mercapto polypyrrole with polyvinylidene fluoride, obtains a membrane material by electrostatic spinning, and then deposits a polydopamine layer on the surface of the membrane material by the dopamine self-polymerization effect. The modified polyvinylidene fluoride membrane prepared by the present invention has excellent Hg (II) ion adsorption effect and good hydrophilicity, and has important application prospects in the removal of mercury ions in sewage.
[0030] The preparation method of the invention is simple and suitable for industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 This is a physical picture of the modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane) prepared in Example 3 of the present invention.
[0033] Figure 2 This is a physical picture of the PVDF membrane prepared in Comparative Example 3 of the present invention.
[0034] Figure 3 This is an infrared spectrum of the modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane) prepared in Example 3 of the present invention before and after the adsorption of Hg (II) ions.
[0035] Figure 4 This is a SEM image of the modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane) prepared in Example 3 of the present invention.
[0036] Figure 5 The contact angles of the modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane) prepared in Example 3 of the present invention, the PVDF-PDA membrane prepared in Comparative Example 1, the PVDF-PPySH membrane prepared in Comparative Example 2, and the PVDF membrane prepared in Comparative Example 3. DETAILED DESCRIPTION
[0037] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0038] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0039] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0040] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0041] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0042] Example 1
[0043] The preparation steps of modified polyvinylidene fluoride membrane are as follows:
[0044] (1) Preparation of mercapto polypyrrole (adsorption functional polymer):
[0045] Take 0.5 mL of pyrrole (Py) monomer and stir it in 30 mL of deionized water for 3 hours to obtain a pyrrole aqueous solution; add 1 mL of thioglycolic acid and continue stirring for 3 hours to obtain a pyrrole-thiol aqueous solution, take 4 g of ammonium persulfate and dissolve it in 10 mL of deionized water to obtain an ammonium persulfate solution as an initiator; then slowly add the ammonium persulfate solution dropwise to the pyrrole-thiol aqueous solution, slowly stir for 6 hours, collect the precipitate after standing overnight, repeatedly wash it with distilled water and ethanol, and then dry it to obtain thiol polypyrrole powder PPySH.
[0046] (2) Preparation of bulk blended modified polyvinylidene fluoride membrane:
[0047] a. Add 0.05 g of mercaptopolypyrrole powder into 8 mL of dimethyl sulfoxide (DMSO), disperse evenly by ultrasonication, then add 1 g of polyvinylidene fluoride (molecular weight 700,000), heat and stir (70°C) for 3 h to make it evenly dissolved, then stop heating, add 4 mL of acetone and continue stirring for 4 h to obtain a spinning solution;
[0048] b. Place the prepared spinning solution in an electrospinning device for spinning, with aluminum foil as the receiving device. Ambient temperature: 25°C, receiving distance: 12 cm, propulsion flow rate: 0.70 mL / h, spinning time: 5 hours, voltage: 11 kV, drum speed: 400 r / min, slide scanning speed: 30 mm / s.
[0049] c. Place the spun film evenly in deionized water, perform solid-liquid phase transformation by phase inversion method to obtain PVDF-PPySH adsorption film, and finally soak the adsorption film in deionized water.
[0050] d. Cut the membrane into 3*3cm pieces and soak it in 15mL of anhydrous ethanol for 1h. Then take it out and clean it.
[0051] (3) Hydrophilic modification of membrane:
[0052] Dopamine was dissolved in a 1.5M Tris-HCl buffer solution to prepare a dopamine solution with a concentration of 4 mg / mL. The adsorption membrane prepared in step (2) was then immersed in the dopamine solution and placed in a shaker. The membrane was shaken at a constant temperature for 7 hours under an aerobic environment to self-polymerize a dopamine hydrophilic layer on the surface of the membrane. The membrane was then washed with deionized water and dried to obtain a modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane).
[0053] The adsorption experiment was carried out in a constant temperature shaker at 30°C and 100 rpm. 20 mL of mercury ion solution with an initial concentration of 50 mg / L was taken and placed in 20 mg of modified polyvinylidene fluoride membrane. The results showed that the removal rate of Hg(II) ions reached 77.74% in 1 hour and 78.6% in 4 hours.
[0054] Example 2
[0055] The preparation steps of modified polyvinylidene fluoride membrane are as follows:
[0056] (1) Preparation of mercapto polypyrrole (adsorption functional polymer):
[0057] Take 0.5 mL of pyrrole (Py) monomer and stir it in 30 mL of deionized water for 3 hours to obtain a pyrrole aqueous solution; add 1 mL of thioglycolic acid and continue stirring for 3 hours to obtain a pyrrole-thiol aqueous solution, take 4 g of ammonium persulfate and dissolve it in 10 mL of deionized water to obtain an ammonium persulfate solution as an initiator; then slowly add the ammonium persulfate solution dropwise to the pyrrole-thiol aqueous solution, slowly stir for 6 hours, collect the precipitate after standing overnight, repeatedly wash it with distilled water and ethanol, and then dry it to obtain thiol polypyrrole powder PPySH.
[0058] (2) Preparation of bulk blended modified polyvinylidene fluoride membrane:
[0059] a. Add 0.15 g of mercaptopolypyrrole powder into 8 mL of dimethyl sulfoxide (DMSO), disperse evenly by ultrasonication, then add 1 g of polyvinylidene fluoride (molecular weight 700,000), heat and stir (70°C) for 3 h to make it evenly dissolved, then stop heating, add 4 mL of acetone and continue stirring for 4 h to obtain a spinning solution;
[0060] b. Place the prepared spinning solution in an electrospinning device for spinning, with aluminum foil as the receiving device. Ambient temperature: 27°C, receiving distance: 12 cm, propulsion flow rate: 0.70 mL / h, spinning time: 5 hours, voltage: 11 kV, drum speed: 400 r / min, slide scanning speed: 30 mm / s.
[0061] c. Place the spun film evenly in deionized water, perform solid-liquid phase transformation by phase inversion method to obtain PVDF-PPySH adsorption film, and finally soak the adsorption film in deionized water.
[0062] d. Cut the membrane into 3*3cm pieces and soak it in 15mL of anhydrous ethanol for 1h. Then take it out and clean it.
[0063] (3) Hydrophilic modification of membrane:
[0064] Dopamine was dissolved in a 1.5M Tris-HCl buffer solution to prepare a dopamine solution with a concentration of 4 mg / mL. The adsorption membrane prepared in step (2) was then immersed in the dopamine solution and placed in a shaker. The membrane was shaken at a constant temperature for 7 hours under an aerobic environment to self-polymerize a dopamine hydrophilic layer on the surface of the membrane. The membrane was then washed with deionized water and dried to obtain a modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane).
[0065] The adsorption experiment was carried out in a constant temperature shaker at 30°C and 100 rpm. 20 mL of mercury ion solution with an initial concentration of 50 mg / L was taken and placed in 20 mg of modified polyvinylidene fluoride membrane. The results showed that the removal rate of Hg(II) ions reached 90.6% in 1 hour and 97.08% in 4 hours.
[0066] Example 3
[0067] The preparation steps of modified polyvinylidene fluoride membrane are as follows:
[0068] (1) Preparation of mercapto polypyrrole (adsorption functional polymer):
[0069] Take 0.5 mL of pyrrole (Py) monomer and stir it in 30 mL of deionized water for 3 hours to obtain a pyrrole aqueous solution; add 1 mL of thioglycolic acid and continue stirring for 3 hours to obtain a pyrrole-thiol aqueous solution, take 4 g of ammonium persulfate and dissolve it in 10 mL of deionized water to obtain an ammonium persulfate solution as an initiator; then slowly add the ammonium persulfate solution dropwise to the pyrrole-thiol aqueous solution, slowly stir for 6 hours, collect the precipitate after standing overnight, repeatedly wash it with distilled water and ethanol, and then dry it to obtain thiol polypyrrole powder PPySH.
[0070] (2) Preparation of bulk blended modified polyvinylidene fluoride membrane:
[0071] a. Add 0.25 g of mercaptopolypyrrole powder to 8 mL of dimethyl sulfoxide (DMSO), disperse evenly by ultrasonication, then add 1 g of polyvinylidene fluoride (molecular weight 700,000) and heat and stir (70°C) for 3 h to dissolve it evenly, then stop heating, add 4 mL of acetone and continue stirring for 4 h to obtain a spinning solution;
[0072] b. Place the prepared spinning solution in an electrospinning device for spinning, with aluminum foil as the receiving device. Ambient temperature: 30°C, receiving distance: 12 cm, propulsion flow rate: 0.70 mL / h, spinning time: 5 hours, voltage: 11 kV, drum speed: 400 r / min, slide scanning speed: 30 mm / s.
[0073] c. Place the spun film evenly in deionized water, perform solid-liquid phase transformation by phase inversion method to obtain PVDF-PPySH adsorption film, and finally soak the adsorption film in deionized water.
[0074] d. Cut the membrane into 3*3cm pieces and soak it in 15mL of anhydrous ethanol for 1h. Then take it out and clean it.
[0075] (3) Hydrophilic modification of membrane:
[0076] Dopamine was dissolved in a 1.5M Tris-HCl buffer solution to prepare a dopamine solution with a concentration of 4 mg / mL. The adsorption membrane prepared in step (2) was then immersed in the dopamine solution and placed in a shaker. The membrane was shaken at a constant temperature for 7 hours under an aerobic environment to self-polymerize a dopamine hydrophilic layer on the surface of the membrane. The membrane was then washed with deionized water and dried to obtain a modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane).
[0077] The modified polyvinylidene fluoride membrane prepared in Example 3 of the present invention exhibits excellent Hg(II) ion removal capability:
[0078] The adsorption experiment was carried out in a constant temperature shaker at 30°C and 100 rpm. 20 mL of mercury ion solution with an initial concentration of 50 mg / L was taken and placed in 20 mg of modified polyvinylidene fluoride membrane. The results showed that the removal rate of Hg(II) ions reached 93.28% in 1 hour and 99.26% in 4 hours.
[0079] The modified polyvinylidene fluoride membrane prepared in Example 3 of the present invention also exhibits good hydrophilicity, and the water contact angle of ionized water after contacting the membrane surface for 1 second is 15.76°.
[0080] Figure 1 This is a physical picture of the modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane) prepared in Example 3 of the present invention.
[0081] Figure 3This is an infrared spectrum of the modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane) prepared in Example 3 of the present invention before and after the adsorption of Hg (II) ions.
[0082] Figure 4 This is a SEM image of the modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane) prepared in Example 3 of the present invention.
[0083] Example 4
[0084] The preparation steps of modified polyvinylidene fluoride membrane are as follows:
[0085] (1) Preparation of mercapto polypyrrole (adsorption functional polymer):
[0086] Take 0.5 mL of pyrrole (Py) monomer and stir it in 30 mL of deionized water for 3 hours to obtain a pyrrole aqueous solution; add 1 mL of thioglycolic acid and continue stirring for 3 hours to obtain a pyrrole-thiol aqueous solution, take 4 g of ammonium persulfate and dissolve it in 10 mL of deionized water to obtain an ammonium persulfate solution as an initiator; then slowly add the ammonium persulfate solution dropwise to the pyrrole-thiol aqueous solution, slowly stir for 6 hours, collect the precipitate after standing overnight, repeatedly wash it with distilled water and ethanol, and then dry it to obtain thiol polypyrrole powder PPySH.
[0087] (2) Preparation of bulk blended modified polyvinylidene fluoride membrane:
[0088] a. Add 0.35 g of mercapto polypyrrole powder into 8 mL of dimethyl sulfoxide (DMSO), disperse evenly by ultrasonication, then add 1 g of polyvinylidene fluoride (molecular weight 700,000), heat and stir (70°C) for 3 h to make it evenly dissolved, then stop heating, add 4 mL of acetone and continue stirring for 4 h to obtain a spinning solution;
[0089] b. Place the prepared spinning solution in an electrospinning device for spinning, with aluminum foil as the receiving device. Ambient temperature: 28°C, receiving distance: 11 cm, propulsion flow rate: 0.70 mL / h, spinning time: 5 hours, voltage: 11 kV, drum speed: 400 r / min, slide scanning speed: 30 mm / s.
[0090] c. Place the spun film evenly in deionized water, perform solid-liquid phase transformation by phase inversion method to obtain PVDF-PPySH adsorption film, and finally soak the adsorption film in deionized water.
[0091] d. Cut the membrane into 3*3cm pieces and soak it in 15mL of anhydrous ethanol for 1h. Then take it out and clean it.
[0092] (3) Hydrophilic modification of membrane:
[0093] Dopamine was dissolved in a 1.5M Tris-HCl buffer solution to prepare a dopamine solution with a concentration of 4 mg / mL. The adsorption membrane prepared in step (2) was then immersed in the dopamine solution and placed in a shaker. The membrane was shaken at a constant temperature for 7 hours under an aerobic environment to self-polymerize a dopamine hydrophilic layer on the surface of the membrane. The membrane was then washed with deionized water and dried to obtain a modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane).
[0094] The adsorption experiment was carried out in a constant temperature shaker at 30°C and 100 rpm. 20 mL of mercury ion solution with an initial concentration of 50 mg / L was taken and placed in 20 mg of modified polyvinylidene fluoride membrane. The results showed that the removal rate of Hg(II) ions reached 96.68% in 1 hour and 99.54% in 4 hours.
[0095] Example 5
[0096] The preparation steps of modified polyvinylidene fluoride membrane are as follows:
[0097] (1) Preparation of mercapto polypyrrole (adsorption functional polymer):
[0098] Take 0.5 mL of pyrrole (Py) monomer and stir it in 30 mL of deionized water for 3 hours to obtain a pyrrole aqueous solution; add 1 mL of thioglycolic acid and continue stirring for 3 hours to obtain a pyrrole-thiol aqueous solution, take 4 g of ammonium persulfate and dissolve it in 10 mL of deionized water to obtain an ammonium persulfate solution as an initiator; then slowly add the ammonium persulfate solution dropwise to the pyrrole-thiol aqueous solution, slowly stir for 6 hours, collect the precipitate after standing overnight, repeatedly wash it with distilled water and ethanol, and then dry it to obtain thiol polypyrrole powder PPySH.
[0099] (2) Preparation of bulk blended modified polyvinylidene fluoride membrane:
[0100] a. Add 0.45 g of mercaptopolypyrrole powder to 8 mL of dimethyl sulfoxide (DMSO), disperse evenly by ultrasonication, then add 1 g of polyvinylidene fluoride (molecular weight 700,000) and heat and stir (70°C) for 3 h to dissolve it evenly, then stop heating, add 4 mL of acetone and continue stirring for 4 h to obtain a spinning solution;
[0101] b. Place the prepared spinning solution in an electrospinning device for spinning, with aluminum foil as the receiving device. Ambient temperature: 25°C, receiving distance: 10 cm, propulsion flow rate: 0.70 mL / h, spinning time: 5 hours, voltage: 11 kV, drum speed: 400 r / min, slide scanning speed: 30 mm / s.
[0102] c. Place the spun film evenly in deionized water, perform solid-liquid phase transformation by phase inversion method to obtain PVDF-PPySH adsorption film, and finally soak the adsorption film in deionized water.
[0103] d. Cut the membrane into 3*3cm pieces and soak it in 15mL of anhydrous ethanol for 1h. Then take it out and clean it.
[0104] (3) Hydrophilic modification of membrane:
[0105] Dopamine was dissolved in a 1.5M Tris-HCl buffer solution to prepare a dopamine solution with a concentration of 4 mg / mL. The adsorption membrane prepared in step (2) was then immersed in the dopamine solution and placed in a shaker. The membrane was shaken at a constant temperature for 7 hours under an aerobic environment to self-polymerize a dopamine hydrophilic layer on the surface of the membrane. The membrane was then washed with deionized water and dried to obtain a modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane).
[0106] The adsorption experiment was carried out in a constant temperature shaker at 30°C and 100 rpm. 20 mL of mercury ion solution with an initial concentration of 50 mg / L was taken and placed in 20 mg of modified polyvinylidene fluoride membrane. The results showed that the removal rate of Hg(II) ions reached 95.87% in 1 hour and 98.68% in 4 hours.
[0107] Example 6
[0108] The preparation steps of modified polyvinylidene fluoride membrane are as follows:
[0109] (1) Preparation of mercapto polypyrrole (adsorption functional polymer):
[0110] Take 0.5 mL of pyrrole (Py) monomer and stir it in 30 mL of deionized water for 3 hours to obtain a pyrrole aqueous solution; add 1 mL of thioglycolic acid and continue stirring for 3 hours to obtain a pyrrole-thiol aqueous solution, take 4 g of ammonium persulfate and dissolve it in 10 mL of deionized water to obtain an ammonium persulfate solution as an initiator; then slowly add the ammonium persulfate solution dropwise to the pyrrole-thiol aqueous solution, slowly stir for 6 hours, collect the precipitate after standing overnight, repeatedly wash it with distilled water and ethanol, and then dry it to obtain thiol polypyrrole powder PPySH.
[0111] (2) Preparation of bulk blended modified polyvinylidene fluoride membrane:
[0112] a. Add 0.55 g of mercaptopolypyrrole powder into 8 mL of dimethyl sulfoxide (DMSO), disperse uniformly by ultrasonication, then add 1 g of polyvinylidene fluoride (molecular weight 700,000), heat and stir (70°C) for 3 h to make it uniformly dissolved, then stop heating, add 4 mL of acetone and continue stirring for 4 h to obtain a spinning solution;
[0113] b. Place the prepared spinning solution in an electrospinning device for spinning, with aluminum foil as the receiving device. Ambient temperature: 30°C, receiving distance: 12 cm, propulsion flow rate: 0.70 mL / h, spinning time: 5 hours, voltage: 11 kV, drum speed: 400 r / min, slide scanning speed: 30 mm / s.
[0114] c. Place the spun film evenly in deionized water, perform solid-liquid phase transformation by phase inversion method to obtain PVDF-PPySH adsorption film, and finally soak the adsorption film in deionized water.
[0115] d. Cut the membrane into 3*3cm pieces and soak it in 15mL of anhydrous ethanol for 1h. Then take it out and clean it.
[0116] (3) Hydrophilic modification of membrane:
[0117] Dopamine was dissolved in a 1.5M Tris-HCl buffer solution to prepare a dopamine solution with a concentration of 4 mg / mL. The adsorption membrane prepared in step (2) was then immersed in the dopamine solution and placed in a shaker. The membrane was shaken at a constant temperature for 7 hours under an aerobic environment to self-polymerize a dopamine hydrophilic layer on the surface of the membrane. The membrane was then washed with deionized water and dried to obtain a modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane).
[0118] The adsorption experiment was carried out in a constant temperature shaker at 30°C and 100 rpm. 20 mL of mercury ion solution with an initial concentration of 50 mg / L was taken and placed in 20 mg of modified polyvinylidene fluoride membrane. The results showed that the removal rate of Hg(II) ions reached 95.73% in 1 hour and 98.82% in 4 hours.
[0119] Comparative Example 1
[0120] The preparation steps of PVDF-PDA membrane are as follows:
[0121] (1) Preparation of membrane:
[0122] a. Add 1g of polyvinylidene fluoride (molecular weight 700,000) to 8mL of dimethyl sulfoxide (DMSO), heat and stir (70°C) for 3h to make it evenly dissolved, then stop heating, add 4mL of acetone and continue stirring for 4h to obtain the spinning solution;
[0123] b. Place the prepared spinning solution in an electrospinning device for spinning, with aluminum foil as the receiving device. Ambient temperature: 30°C, receiving distance: 12 cm, propulsion flow rate: 0.70 mL / h, spinning time: 5 hours, voltage: 11 kV, drum speed: 400 r / min, slide scanning speed: 30 mm / s.
[0124] c. Place the spun film evenly in deionized water, perform solid-liquid phase conversion by phase inversion method to obtain a PVDF membrane, and soak it in deionized water.
[0125] d. Cut the membrane into 3*3cm pieces and soak it in 15mL of anhydrous ethanol for 1h. Then take it out and clean it.
[0126] (2) Hydrophilic modification of membrane:
[0127] Dopamine was dissolved in a 1.5M Tris-HCl buffer solution to prepare a dopamine solution with a concentration of 4 mg / mL. The adsorption membrane prepared in step (1) was then immersed in the dopamine solution and placed in a shaker. The membrane was shaken at a constant temperature for 7 hours under an aerobic environment to self-polymerize a dopamine hydrophilic layer on the surface of the membrane. The membrane was then washed with deionized water and dried to obtain a PVDF-PDA membrane.
[0128] Comparative Example 2
[0129] The preparation steps of PVDF-PPySH are as follows:
[0130] (1) Preparation of mercapto polypyrrole (adsorption functional polymer):
[0131] Take 0.5 mL of pyrrole (Py) monomer and stir it in 30 mL of deionized water for 3 hours to obtain a pyrrole aqueous solution; add 1 mL of thioglycolic acid and continue stirring for 3 hours to obtain a pyrrole-thiol aqueous solution, take 4 g of ammonium persulfate and dissolve it in 10 mL of deionized water to obtain an ammonium persulfate solution as an initiator; then slowly add the ammonium persulfate solution dropwise to the pyrrole-thiol aqueous solution, slowly stir for 6 hours, collect the precipitate after standing overnight, repeatedly wash it with distilled water and ethanol, and then dry it to obtain thiol polypyrrole powder PPySH.
[0132] (2) Preparation of bulk blended modified polyvinylidene fluoride membrane:
[0133] a. Add 0.25 g of mercaptopolypyrrole powder to 8 mL of dimethyl sulfoxide (DMSO), disperse evenly by ultrasonication, then add 1 g of polyvinylidene fluoride (molecular weight 700,000) and heat and stir (70°C) for 3 h to dissolve it evenly, then stop heating, add 4 mL of acetone and continue stirring for 4 h to obtain a spinning solution;
[0134] b. Place the prepared spinning solution in an electrospinning device for spinning, with aluminum foil as the receiving device. Ambient temperature: 30°C, receiving distance: 12 cm, propulsion flow rate: 0.70 mL / h, spinning time: 5 hours, voltage: 11 kV, drum speed: 400 r / min, slide scanning speed: 30 mm / s.
[0135] c. Place the spun film evenly in deionized water, perform solid-liquid phase transformation by phase inversion method to obtain PVDF-PPySH membrane, and finally soak the adsorption membrane in deionized water.
[0136] Comparative Example 3
[0137] The preparation steps of PVDF electrospinning membrane are as follows:
[0138] (1) Preparation of membrane:
[0139] a. Add 1g of polyvinylidene fluoride (molecular weight 700,000) to 8mL of dimethyl sulfoxide (DMSO), heat and stir (70°C) for 3h to make it evenly dissolved, then stop heating, add 4mL of acetone and continue stirring for 4h to obtain the spinning solution;
[0140] b. Place the prepared spinning solution in an electrospinning device for spinning, with aluminum foil as the receiving device. Ambient temperature: 30°C, receiving distance: 12 cm, propulsion flow rate: 0.70 mL / h, spinning time: 5 hours, voltage: 11 kV, drum speed: 400 r / min, slide scanning speed: 30 mm / s.
[0141] c. Place the spun film evenly in deionized water, perform solid-liquid phase conversion by phase inversion method to obtain a PVDF membrane, and soak it in deionized water.
[0142] Figure 2 This is a physical picture of the PVDF membrane prepared in Comparative Example 3 of the present invention.
[0143] Figure 5 The contact angles of the modified polyvinylidene fluoride membrane (PVDF-PPySH-PDA membrane) prepared in Example 3 of the present invention, the PVDF-PDA membrane prepared in Comparative Example 1, the PVDF-PPySH membrane prepared in Comparative Example 2, and the PVDF membrane prepared in Comparative Example 3.
[0144] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a modified polyvinylidene fluoride film, It is characterized in that The following steps are involved: The mercapto polypyrrole and polyvinylidene fluoride are mixed in a solvent to obtain an electrospinning solution; The electrospinning solution is subjected to electrospinning treatment to obtain a PVDF-PPySH membrane; Soaking the PVDF-PPySH membrane in anhydrous ethanol to obtain an activated PVDF-PPySH membrane; The activated PVDF-PPySH membrane is immersed in a dopamine solution to obtain the modified polyvinylidene fluoride membrane.
2. The preparation method according to claim 1, It is characterized in that The mercaptopolypyrrole is obtained by oxidative polymerization of mercaptoacetic acid and pyrrole.
3. The preparation method according to claim 1, It is characterized in that The solvent includes dimethyl sulfoxide, N,N-dimethylformamide or acetone.
4. The preparation method according to claim 1, It is characterized in that The ambient temperature of the electrospinning process is 25-30° C., and the voltage is 10-12 kV.
5. The preparation method according to claim 1, It is characterized in that The mass ratio of the mercaptopolypyrrole to polyvinylidene fluoride is 0.05g-0.55g:1g.
6. The preparation method according to claim 1, It is characterized in that The concentration of the dopamine solution is 4 mg / mL.
7. The preparation method according to claim 1, It is characterized in that The immersion time in the dopamine solution is 7 hours; the immersion time in the anhydrous ethanol is 1 hour.
8. The modified polyvinylidene fluoride film prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the modified polyvinylidene fluoride membrane as claimed in claim 8 in removing Hg(II) ions from water.
Citation Information
Patent Citations
Electroactive double-layer periosteal-like material and preparation method thereof
CN108434526A
Catalyst capable of efficiently treating ammonia nitrogen wastewater at a relatively low temperature, and preparation method thereof
CN110898835A
Wastewater mercury removal agent, and preparation method and application thereof
CN112808246A
Preparation method of PPy coated rGO directly loaded electric control lithium ion imprinted membrane
CN117358217A
Composite graphene energy storage methods, devices, and systems
US10938032B1
Cited By
Ultrafiltration membrane for purifying and separating electroplating effluent and preparation method thereof
CN120189825A
Pretreatment method and preparation method of electrode foil for aluminum electrolytic capacitor, electrode foil and capacitor
CN122658899A