Amorphous / crystal core-shell catalyst and preparation method thereof

By adopting an amorphous/crystalline core-shell structure in the oxidative desulfurization catalyst, using tungsten-doped molybdenum phosphide crystals and amorphous tungsten oxide coatings, combined with layered carrier materials, the stability and preparation complexity of the existing catalysts are solved solve the problem and achieve high-efficiency, low-cost catalytic activity and selectivity, which is suitable for ultra-deep oxidation desulfurization in petroleum products.

CN118744003APending Publication Date: 2024-10-08GUANGDONG UNIV OF PETROCHEMICAL TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410435859.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-11
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

When improving the catalytic activity of existing oxidative desulfurization catalysts, the active sites are easily destroyed by harmful chemicals, resulting in poor stability. The preparation process is complex and the cost is high, making it difficult to be widely used.

Method used

An amorphous/crystalline core-shell catalyst is used, including a tungsten-doped molybdenum phosphide crystal surface covered with an amorphous tungsten oxide coating and grown on a layered carrier material. The catalyst is formed through polymerization and calcination to simplify the process and improve stability.

Benefits of technology

The catalytic activity and stability of the catalyst are significantly improved, and highly selective ultra-deep oxidative desulfurization is achieved. The process is simple and low-cost, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744003A_ABST
    Figure CN118744003A_ABST
Patent Text Reader

Abstract

The invention discloses an amorphous / crystal core-shell catalyst and a preparation method thereof. The catalyst comprises a tungsten-doped molybdenum phosphide crystal and an amorphous tungsten oxide coating coated on the surface of the tungsten-doped molybdenum phosphide crystal. The preparation method comprises the following steps: preparing ammonium tungstate and ammonium molybdate into a molybdenum / tungsten precursor solution, mixing the molybdenum / tungsten precursor solution with melamine and a phosphorus source, carrying out polymerization reaction, and calcining to obtain the amorphous / crystal core-shell catalyst. According to the amorphous / crystal core-shell catalyst disclosed by the invention, the catalytic activity and stability of the catalyst can be remarkably improved by utilizing the synergistic effect between crystals and non-crystals, the amorphous / crystal core-shell catalyst has the advantages of high catalytic activity, excellent selectivity, good stability and the like, thiophene sulfur-containing compounds in an oil product can be quickly and effectively removed, and the application prospect is wide. And high-selectivity ultra-deep oxidation desulfurization can be achieved, the use value is high, and the application prospect is good. The preparation method has the advantages of being simple in process, easy to operate, low in cost, green, free of pollution and the like, large-scale production can be achieved, and industrial application is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the fields of multiphase catalysis technology and petrochemical technology, and relates to an amorphous / crystalline core-shell catalyst and a preparation method thereof. Background Art

[0002] Oxidative desulfurization (ODS) can easily oxidize sulfur-containing compounds into corresponding sulfones, which can then be removed by simple extraction or adsorption; at the same time, ODS has the advantages of low energy consumption and high cost-effectiveness, so ODS is considered to be a very promising technology for achieving ultra-deep desulfurization. So far, various types of catalysts have been developed, such as polyoxymetallic salts, ionic liquids, inorganic-organic hybrid nanocomposites, porous compounds, and metal-organic frameworks, which are used as ODS catalysts to produce ultra-low sulfur fuel oil. However, most catalysts still require cumbersome catalyst preparation processes, long reaction times, or large amounts of oxidants to achieve fairly high desulfurization performance. In addition, in existing oxidative desulfurization catalysts, in order to promote the improvement of catalytic activity, more active sites are usually exposed to the outside, and the defects are: these active sites are easily in contact with external harmful chemicals, thereby destroying the electronic structure of the catalyst surface, and then causing the catalyst to deteriorate in stability; at the same time, if a protective layer is coated on the outside of the active site, it is not only easy to cause the number of reactive active sites to decrease, but also increase the complexity of the preparation process, which is not easy to be widely used. Therefore, synthesizing high-performance ODS catalysts through a green, economical and rapid method will enable better desulfurization efficiency to be achieved at a lower cost and in a more convenient way, which is of great significance for achieving the effective conversion of sulfur-containing organic pollutants in petroleum products and improving the availability of petroleum products. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art, provide an amorphous / crystalline core-shell catalyst with high catalytic activity, excellent selectivity and good stability, and also provide a method for preparing the amorphous / crystalline core-shell catalyst with simple process, low cost, convenient operation and green and pollution-free.

[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0005] An amorphous / crystalline core-shell catalyst comprises tungsten-doped molybdenum phosphide crystals, the surface of which is coated with an amorphous tungsten oxide coating.

[0006] The above-mentioned amorphous / crystalline core-shell catalyst is further improved in that the molar ratio of molybdenum to tungsten in the amorphous / crystalline core-shell catalyst is 0.4 to 4:1.

[0007] The above-mentioned amorphous / crystalline core-shell catalyst is further improved in that the particle size of the amorphous / crystalline core-shell catalyst is 10nm to 40nm.

[0008] The above-mentioned amorphous / crystalline core-shell catalyst is further improved, and further comprises a layered support material; the amorphous / crystalline core-shell catalyst is grown on the layered support material; the layered support material is at least one of carbon nanosheets, graphene, graphene oxide, reduced graphene oxide, and graphyne; the specific surface area of ​​the layered support material is 100 m 2 / g~500 m 2 / g; the thickness of the layered carrier material is 2 nm to 10 nm.

[0009] As a general technical concept, a method for preparing an amorphous / crystalline core-shell catalyst comprises the following steps:

[0010] S1, preparing a molybdenum / tungsten precursor solution by ammonium tungstate and ammonium molybdate;

[0011] S2, mixing the molybdenum / tungsten precursor solution obtained in step S1, melamine and a phosphorus source to carry out a polymerization reaction to obtain an amorphous / crystalline core-shell catalyst precursor powder;

[0012] S3, calcining the amorphous / crystalline core-shell catalyst precursor powder obtained in step S2 to obtain an amorphous / crystalline core-shell catalyst.

[0013] The above-mentioned method for preparing the amorphous / crystalline core-shell catalyst is further improved, and in step S2, it also includes adding a layered carrier material; the method for preparing the amorphous / crystalline core-shell catalyst precursor powder includes the following steps:

[0014] (1) adding melamine to a molybdenum / tungsten precursor solution and stirring to obtain a suspension A;

[0015] (2) adding the layered support material to the suspension A, stirring, and ultrasonicating to obtain a suspension B;

[0016] (3) adding the phosphorus source to the suspension B, stirring, and ultrasonicating to obtain a suspension C;

[0017] (4) The suspension C is heated to 60° C. to 80° C. for polymerization reaction, filtered, and dried to obtain an amorphous / crystalline core-shell catalyst precursor powder.

[0018] The above-mentioned method for preparing amorphous / crystalline core-shell catalyst is further improved, in which in step (1), the mass of melamine is 2.5% to 3% of the mass of the molybdenum / tungsten precursor solution; and the stirring time is 10 min to 30 min.

[0019] The above-mentioned method for preparing amorphous / crystalline core-shell catalyst is further improved, in which, in step (2), the mass of the layered support material is 0.5% to 1% of the mass of the suspension A; the layered support material is at least one of carbon nanosheets, graphene, graphene oxide, reduced graphene oxide, and graphyne; the specific surface area of ​​the layered support material is 100 m 2 / g~500 m 2 / g; the thickness of the layered carrier material is 2 nm to 10 nm; the stirring time is 10 min to 30 min; and the ultrasonic time is 30 min to 60 min.

[0020] The above-mentioned method for preparing amorphous / crystalline core-shell catalyst is further improved. In step (3), the phosphorus source is a phosphoric acid solution and / or a phytic acid solution; the mass concentration of the phosphoric acid solution or the phytic acid solution is 85%; the mass of the phosphorus source is 5% to 10% of the mass of the suspension B; the stirring time is 30 min to 60 min; and the ultrasonic time is 30 min to 60 min.

[0021] The above-mentioned method for preparing amorphous / crystalline core-shell catalyst is further improved, in which in step (4), the polymerization reaction time is 12 h to 16 h; the drying temperature is 60° C. to 80° C.; and the drying time is 12 h to 16 h.

[0022] The above-mentioned method for preparing amorphous / crystalline core-shell catalyst is further improved. In step S1, the method for preparing the molybdenum / tungsten precursor solution comprises the following steps: mixing ammonium molybdate and ammonium tungstate with water, and stirring for 10 min to 30 min to obtain a molybdenum / tungsten precursor solution.

[0023] The above-mentioned method for preparing amorphous / crystalline core-shell catalyst is further improved, in which, in step S3, the calcination is carried out under an inert atmosphere; the inert atmosphere is a nitrogen or argon atmosphere; the calcination temperature is 800°C to 900°C; and the calcination time is 2 to 3 hours.

[0024] The above-mentioned method for preparing amorphous / crystalline core-shell catalyst is further improved in that in step S3, during the calcination process, hydrogen is introduced into the calcination system; and the volume fraction of hydrogen in the calcination system is ≤4%.

[0025] The preparation method of the above-mentioned amorphous / crystalline core-shell catalyst is further improved. In step S3, the amorphous / crystalline core-shell catalyst includes tungsten-doped molybdenum phosphide crystals; the surface of the tungsten-doped molybdenum phosphide crystals is coated with an amorphous tungsten oxide coating; the molar ratio of molybdenum to tungsten in the amorphous / crystalline core-shell catalyst is 0.4 to 4:1; the particle size of the amorphous / crystalline core-shell catalyst is 10nm to 40nm; the amorphous / crystalline core-shell catalyst grows on a layered carrier material.

[0026] Compared with the prior art, the advantages of the present invention are:

[0027] (1) The present invention provides an amorphous / crystalline core-shell catalyst, comprising a tungsten-doped molybdenum phosphide crystal, the surface of which is coated with an amorphous tungsten oxide coating. On the one hand, the amorphous tungsten oxide coating coated on the surface of the tungsten-doped molybdenum phosphide crystal can effectively prevent harmful chemicals such as oxidants from directly contacting the surface of the tungsten-doped molybdenum phosphide, thereby effectively protecting the electronic structure of the surface of the tungsten-doped molybdenum phosphide crystal, thereby improving the stability of the catalyst. On the other hand, the amorphous structure on the surface of the amorphous / crystalline core-shell catalyst contains a large number of dangling bonds and defects, which can provide more reactive sites for the catalytic reaction, which is conducive to improving the activity of the catalyst. Therefore, the amorphous / crystalline core-shell catalyst of the present invention can significantly improve the catalytic activity and stability of the catalyst by utilizing the synergistic effect between the crystal and the amorphous phase, and has the advantages of high catalytic activity, excellent selectivity, good stability, etc. It is a novel oxidative desulfurization catalyst with excellent performance and can be widely used, which can realize the rapid and effective removal of thiophene sulfur-containing compounds in oil products, and can achieve highly selective ultra-deep oxidative desulfurization, with high use value and good application prospects.

[0028] (2) In the present invention, the particle size of the amorphous / crystalline core-shell catalyst is 10nm to 40nm. This nano-scale catalyst can expose more active sites and effectively improve the catalytic efficiency of the catalyst. In addition, the layered support material used as the growth substrate of the amorphous / crystalline core-shell catalyst is an ultra-thin nanosheet with a specific surface area of ​​up to 100m 2 / g~500m 2 / g, and the thickness is only 2nm to 10nm, which is beneficial to the mass transfer of amorphous / crystalline core-shell catalysts in the reaction and further improves the catalytic activity.

[0029] (3) The present invention also provides a method for preparing an amorphous / crystalline core-shell catalyst, comprising preparing a molybdenum / tungsten precursor solution with ammonium tungstate and ammonium molybdate, and using melamine as a reducing agent and a cross-linking agent. An amorphous / crystalline core-shell catalyst precursor is first formed by a polymerization reaction, and then tungsten-doped molybdenum phosphide crystals are formed by calcination. An amorphous tungsten oxide coating is coated on the surface of the tungsten-doped molybdenum phosphide crystals, thereby preparing an amorphous / crystalline core-shell catalyst with high catalytic activity, excellent selectivity and good stability. The preparation method of the present invention has the advantages of simple process, simple operation method, low cost, and green and pollution-free. In addition, flammable phosphorus and highly toxic phosphine are not used as phosphating agents, the equipment requirements are not high, the repeatability is strong, and large-scale production can be achieved, which is conducive to industrial application.

[0030] (4) The present invention provides an application of an amorphous / crystalline core-shell catalyst. The amorphous / crystalline core-shell catalyst has the advantages of strong catalytic activity, high selectivity, good stability, etc. Therefore, when the amorphous / crystalline core-shell catalyst is used for catalytic oxidation treatment of sulfur-containing organic compounds in oil products, it can quickly and efficiently achieve effective conversion of sulfur-containing organic compounds in fuel products, and can achieve ultra-high efficiency and ultra-deep oxidation desulfurization. It has the advantages of simple process, convenient operation, low cost, high removal efficiency, etc., and has excellent economic benefits and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0032] Figure 1 This is a flow chart of the preparation process of the amorphous / crystalline core-shell catalyst in Example 1 of the present invention.

[0033] Figure 2 High-resolution transmission electron microscopy image of the amorphous / crystalline core-shell catalyst prepared in Example 1 of the present invention.

[0034] Figure 3 This is the X-ray diffraction pattern of the amorphous / crystalline core-shell catalyst prepared in Example 1 of the present invention.

[0035] Figure 4 This is the XPS graph of the amorphous / crystalline core-shell catalyst prepared in Example 1 of the present invention.

[0036] Figure 5 This is a diagram showing the removal effect of dibenzothiophene sulfur in fuel by the amorphous / crystalline core-shell catalyst in Example 2 of the present invention.

[0037] Figure 6 This is a diagram showing the effect of repeated cyclic removal of dibenzothiophene sulfur in fuel by the amorphous / crystalline core-shell catalyst in Example 3 of the present invention. DETAILED DESCRIPTION

[0038] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby.

[0039] The materials and instruments used in the following examples are all commercially available.

[0040] Example 1

[0041] An amorphous / crystalline core-shell catalyst comprises tungsten-doped molybdenum phosphide crystals and an amorphous tungsten oxide coating, wherein the surface of the tungsten-doped molybdenum phosphide crystals is coated with the amorphous tungsten oxide coating.

[0042] In this embodiment, the molar ratio of molybdenum to tungsten in the amorphous / crystalline core-shell catalyst is 1:2.3.

[0043] In this embodiment, the particle size of the amorphous / crystalline core-shell catalyst is 10 nm to 40 nm, and the average particle size is 30 nm.

[0044] In this embodiment, the amorphous / crystalline core-shell catalyst is grown on a layered support material, wherein the layered support material is a carbon nanosheet with a specific surface area of ​​465 m 2 / g, thickness is 4nm.

[0045] A method for preparing the amorphous / crystalline core-shell catalyst in the above embodiment of the present invention, the preparation process flow chart is as follows Figure 1 As shown, the following steps are included:

[0046] (1) Weigh 19.9 mg of ammonium tungstate and 5.9 mg of ammonium molybdate, dissolve them in 19 mL of ultrapure water, and stir for 30 min to prepare a molybdenum / tungsten precursor solution.

[0047] (2) Add 0.5 g of melamine to the molybdenum / tungsten precursor solution obtained in step (1), and continue stirring for 10 min to obtain a suspension A.

[0048] (3) Add 0.1 g of carbon nanosheets to the suspension A obtained in step (2), continue stirring for 20 min, and ultrasonicate for 30 min to obtain a suspension B.

[0049] (4) Slowly add 1 mL of 85% phosphoric acid solution to the suspension B obtained in step (3), stir for 30 min, and perform ultrasound for 30 min to obtain a suspension C.

[0050] (5) The suspension C obtained in step (4) was transferred to a water bath at 80° C. for reaction for 12 h, filtered without washing, and dried at 80° C. for 12 h to obtain an amorphous / crystalline core-shell catalyst precursor powder.

[0051] (6) The amorphous / crystalline core-shell catalyst precursor powder obtained in step (5) is transferred to a tubular furnace, heated to 900° C. at a heating rate of 5° C. / min in an argon atmosphere, calcined for 2 h, and naturally cooled to room temperature to obtain an amorphous / crystalline core-shell catalyst.

[0052] In this embodiment, during the calcination process, when hydrogen is introduced into the calcination system, that is, calcination is performed under a reducing atmosphere of H2 / Ar, an amorphous / crystalline core-shell catalyst can also be synthesized, and the prepared core (tungsten-doped molybdenum phosphide crystal) has a higher degree of crystallinity, which is more conducive to improving the catalytic performance of the catalyst. For example, during the calcination process, hydrogen and argon are introduced together to construct a calcination system composed of H2 and argon, and the volume fraction of hydrogen in the calcination system is 4%. At this time, the prepared amorphous / crystalline core-shell catalyst has a more excellent catalytic performance.

[0053] In this embodiment, the specific surface area of ​​the carbon nanosheets used is 465 m 2 / g, thickness is 4nm.

[0054] In this embodiment, the method for preparing the carbon nanosheets comprises the following steps:

[0055] S1. Weigh 5.0 g of sodium dihydrogen citrate and place it in a quartz boat, put it in a tube furnace, heat it to 780° C. at a heating rate of 5° C. / min in an argon environment and maintain it for 2 h, then cool it naturally to room temperature to obtain a porous carbon nanosheet precursor.

[0056] S2. Grind the porous carbon nanosheet precursor obtained in step S1 into powder, add it into 30 mL of hydrochloric acid solution (2M), react at room temperature for 24 h, collect the black product by filtration, wash it with deionized water and ethanol three times each, and dry it at 70° C. for 2 h to obtain carbon nanosheets.

[0057] In this embodiment, when the layered carrier material is graphene, graphene oxide, reduced graphene oxide, or graphyne, it can also be used to grow tungsten-doped molybdenum phosphide crystals and form an amorphous tungsten oxide coating on the surface of the tungsten-doped molybdenum phosphide crystals to obtain an amorphous / crystalline core-shell catalyst.

[0058] In this embodiment, amorphous / crystalline core-shell catalyst precursor powder is prepared in a step-by-step manner, which can completely dissolve the precursor and disperse it evenly, thereby making the reaction more uniform, and ultimately facilitating the acquisition of amorphous / crystalline core-shell nanoparticles with more uniform sizes.

[0059] Figure 2 High-resolution transmission electron microscopy image of the amorphous / crystalline core-shell catalyst prepared in Example 1 of the present invention. Figure 2 In the figure, a and b are transmission electron microscope images at different magnifications. Figure 2It can be seen that the average particle size of the amorphous / crystalline core-shell catalyst prepared by the present invention is 30nm, and the lattice fringes of the crystal core can be observed on a high-resolution transmission electron microscope, and the lattice spacing is 0.21nm, which is respectively attributed to the (101) crystal plane of molybdenum phosphide. In addition, the surface of the crystal core is covered with an amorphous shell with a thickness of 9nm, which indicates that the amorphous / crystalline core-shell catalyst has been successfully synthesized.

[0060] Figure 3 is the X-ray diffraction pattern of the amorphous / crystalline core-shell catalyst prepared in Example 1 of the present invention. Figure 3 It can be seen that the diffraction peaks of the amorphous / crystalline core-shell catalysts can be perfectly summarized as typical characteristic peaks of molybdenum phosphide, and no obvious characteristic peaks of tungsten phosphide were found. The results show that tungsten has been successfully doped into the lattice of molybdenum phosphide and has formed an amorphous shell on the outer surface of molybdenum phosphide.

[0061] Figure 4 The XPS graph of the amorphous / crystalline core-shell catalyst prepared in Example 1 of the present invention is shown in FIG. Figure 4 It can be seen that excluding the C element introduced by the carbon substrate, this shows that the amorphous / crystalline core-shell catalyst is mainly composed of Mo, W, P, and O elements.

[0062] Example 2

[0063] The catalytic oxidation desulfurization activity of the amorphous / crystalline core-shell catalyst of the present invention was investigated. Specifically, the amorphous / crystalline core-shell catalyst prepared in Example 1 was used to remove dibenzothiophene from oil products, comprising the following steps:

[0064] 2.0 mg of the amorphous / crystalline core-shell catalyst prepared in Example 1 was accurately weighed and added to 10 mL of a dibenzothiophene (DBT)-dodecane solution (i.e., a simulated petroleum containing dibenzothiophene) with a sulfur concentration of 500 ppm, and then 2 mL of an acetonitrile solution with a mass fraction of 99% was added and stirred for 10 min to reach extraction equilibrium. Then, 48 μL of a hydrogen peroxide solution with a mass fraction of 30% (oxidant, O / S molar ratio of 4) was added, and a catalytic oxidation reaction was carried out at a temperature of 60° C. and magnetic stirring (speed of 800 r / min) for 60 min. Among them, the catalytic oxidation reaction was carried out in acetonitrile, and dibenzothiophene was converted into dibenzothiophene sulfone and retained in acetonitrile, completing the removal of dibenzothiophene in the oil product. After the reaction was completed, the acetonitrile phase (lower layer) was separated from the oil phase (upper layer) to obtain clean fuel oil.

[0065] In this embodiment, after the reaction is completed, the content of sulfur in dibenzothiophene in the product solution obtained by the reaction is measured by gas chromatography, and the conversion rate of sulfur in dibenzothiophene is obtained by calculation. The results are as follows: Figure 5 shown.

[0066] Figure 5 This is a diagram showing the effect of the amorphous / crystalline core-shell catalyst in Example 2 of the present invention on the removal of dibenzothiophene sulfur in fuel. Figure 5 It can be seen that the amorphous / crystalline core-shell catalyst can remove 100% of dibenzothiophene in simulated petroleum within 60 minutes. The results show that the amorphous / crystalline core-shell catalyst prepared by the present invention has good catalytic oxidation performance. The total sulfur content in the oil treated with the amorphous / crystalline core-shell catalyst prepared by the present invention is <10ppm, which meets the Euro VI fuel standard, and the total desulfurization rate is as high as 100%. In particular, the amorphous / crystalline core-shell catalyst shows excellent dibenzothiophene catalytic oxidation effect under the condition of extremely small amounts of catalyst (0.2g / L) and oxidant (O:S=4), and has good economic benefits and industrial application prospects.

[0067] Example 3

[0068] The reusability of the amorphous / crystalline core-shell catalyst of the present invention was investigated. The amorphous / crystalline core-shell catalyst prepared in Example 1 was used to catalytically oxidize and remove dibenzothiophene from oil products, comprising the following steps:

[0069] Weigh 2 mg of amorphous / crystalline core-shell catalyst, add it to 10 mL of dibenzothiophene (DBT)-dodecane solution (i.e., simulated petroleum containing dibenzothiophene) with a sulfur concentration of 500 ppm, then add 2 mL of 99% acetonitrile solution, and stir for 10 minutes to reach extraction equilibrium. Then, add 48 μL of 30% hydrogen peroxide solution (oxidant, O / S molar ratio of 4), and carry out catalytic oxidation reaction for 60 minutes at a temperature of 60°C and magnetic stirring (speed of 800 r / min). Among them, the catalytic oxidation reaction is carried out in acetonitrile, and dibenzothiophene is converted into dibenzothiophene sulfone and retained in acetonitrile, completing the removal of dibenzothiophene in the oil product. After the reaction is completed, the upper oil phase is extracted. Then the catalytic device with catalyst, acetonitrile, oxidant, sulfone product and water is placed in an 80°C environment for drying for 3 hours to completely remove acetonitrile, oxidant and water. After the reactor was cooled to room temperature, 10 mL of dibenzothiophene (DBT)-dodecane solution with a sulfur concentration of 500 ppm, 2 mL of 99% acetonitrile solution, and 48 μL of 30% hydrogen peroxide solution were added to the reactor to carry out a new round of catalytic reaction without changing the reaction conditions. The cycle was repeated 8 times. The results are as follows: Figure 6 shown.

[0070] Figure 6 This is a diagram showing the effect of repeated cyclic removal of dibenzothiophene sulfur in fuel by the amorphous / crystalline core-shell catalyst in Example 3 of the present invention. Figure 6It can be seen that the amorphous / crystalline core-shell catalyst of the present invention can still achieve a 100% dibenzothiophene removal rate after being reused 5 times. Even after the 8th use, the removal rate of dibenzothiophene still reaches 94.2%. After multiple cycles, it can still maintain excellent catalytic performance, which shows that the porous carbon nanosheet-loaded bimetallic phosphide catalyst of the present invention has very good reusability and stability.

[0071] From the above results, it can be seen that the amorphous / crystalline core-shell catalyst of the present invention can significantly improve the catalytic activity and stability of the catalyst by utilizing the synergistic effect between crystals and amorphous substances, and has the advantages of high catalytic activity, excellent selectivity, good stability, etc. It is a new type of oxidative desulfurization catalyst with excellent performance and can be widely used. It can achieve rapid and effective removal of thiophene sulfur-containing compounds in oil products, and can achieve highly selective ultra-deep oxidative desulfurization, with high use value and good application prospects.

[0072] The above embodiments are only preferred implementations of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. An amorphous / crystalline core-shell catalyst, characterized in that: The invention comprises a tungsten-doped molybdenum phosphide crystal, the surface of which is coated with an amorphous tungsten oxide coating.

2. The amorphous / crystalline core-shell catalyst according to claim 1, characterized in that: The molar ratio of molybdenum to tungsten in the amorphous / crystalline core-shell catalyst is 0.4 to 4:

1.

3. The amorphous / crystalline core-shell catalyst according to claim 2, characterized in that: The particle size of the amorphous / crystalline core-shell catalyst is 10 nm to 40 nm.

4. The amorphous / crystalline core-shell catalyst according to any one of claims 1 to 3, characterized in that The present invention also includes a layered support material; the amorphous / crystalline core-shell catalyst is grown on the layered support material; the layered support material is at least one of carbon nanosheets, graphene, graphene oxide, reduced graphene oxide, and graphyne; the specific surface area of ​​the layered support material is 100 m 2 / g~500m 2 / g; the thickness of the layered carrier material is 2nm to 10nm.

5. A method for preparing an amorphous / crystalline core-shell catalyst, characterized in that: The following steps are involved: S1, preparing a molybdenum / tungsten precursor solution by ammonium tungstate and ammonium molybdate; S2, mixing the molybdenum / tungsten precursor solution obtained in step S1, melamine and a phosphorus source to carry out a polymerization reaction to obtain an amorphous / crystalline core-shell catalyst precursor powder; S3, calcining the amorphous / crystalline core-shell catalyst precursor powder obtained in step S2 to obtain an amorphous / crystalline core-shell catalyst.

6. The method for preparing an amorphous / crystalline core-shell catalyst according to claim 5, characterized in that: Step S2 also includes adding a layered carrier material; the method for preparing the amorphous / crystalline core-shell catalyst precursor powder includes the following steps: (1) adding melamine to a molybdenum / tungsten precursor solution and stirring to obtain a suspension A; (2) adding the layered support material to the suspension A, stirring, and ultrasonicating to obtain a suspension B; (3) adding the phosphorus source to the suspension B, stirring, and ultrasonicating to obtain a suspension C; (4) The suspension C is heated to 60° C. to 80° C. for polymerization reaction, filtered, and dried to obtain an amorphous / crystalline core-shell catalyst precursor powder.

7. The method for preparing an amorphous / crystalline core-shell catalyst according to claim 6, characterized in that: In step (1), the mass of the melamine is 2.5% to 3% of the mass of the molybdenum / tungsten precursor solution; the stirring time is 10 min to 30 min; In step (2), the mass of the layered carrier material is 0.5% to 1% of the mass of the suspension A; the layered carrier material is at least one of carbon nanosheets, graphene, graphene oxide, reduced graphene oxide, and graphyne; the specific surface area of ​​the layered carrier material is 100m 2 / g~500m 2 / g; the thickness of the layered carrier material is 2nm to 10nm; the stirring time is 10min to 30min; the ultrasonic time is 30min to 60min; In step (3), the phosphorus source is a phosphoric acid solution and / or a phytic acid solution; the mass concentration of the phosphoric acid solution or the phytic acid solution is 85%; the mass of the phosphorus source is 5% to 10% of the mass of the suspension B; the stirring time is 30 min to 60 min; the ultrasonic time is 30 min to 60 min; In step (4), the polymerization reaction time is 12 hours to 16 hours; the drying temperature is 60° C. to 80° C.; and the drying time is 12 hours to 16 hours.

8. The method for preparing an amorphous / crystalline core-shell catalyst according to any one of claims 5 to 7, characterized in that: In step S1, the method for preparing the molybdenum / tungsten precursor solution comprises the following steps: mixing ammonium molybdate, ammonium tungstate and water, and stirring for 10 min to 30 min to obtain a molybdenum / tungsten precursor solution.

9. The method for preparing an amorphous / crystalline core-shell catalyst according to any one of claims 5 to 7, characterized in that: In step S3, the calcination is carried out under an inert atmosphere; the inert atmosphere is a nitrogen or argon atmosphere; the calcination temperature is 800°C to 900°C; the calcination time is 2 to 3 hours; during the calcination process, hydrogen is also introduced into the calcination system; the volume fraction of hydrogen in the calcination system is ≤4%.

10. The method for preparing an amorphous / crystalline core-shell catalyst according to claim 6, characterized in that: In step S3, the amorphous / crystalline core-shell catalyst includes tungsten-doped molybdenum phosphide crystals; the surface of the tungsten-doped molybdenum phosphide crystals is coated with an amorphous tungsten oxide coating; the molar ratio of molybdenum to tungsten in the amorphous / crystalline core-shell catalyst is 0.4 to 4:1; the particle size of the amorphous / crystalline core-shell catalyst is 10 nm to 40 nm; the amorphous / crystalline core-shell catalyst grows on a layered carrier material.

Citation Information

Patent Citations

  • Preparation method of thermometal phosphide hydrofining catalyst

    CN103157497A

  • Preparation method of molybdenum phosphide catalysts

    CN108620108A

  • Preparation method and application of carbon nanotube-modified molybdenum-doped tungsten oxide catalyst

    CN112588286A

  • Molybdenum phosphide composite catalyst and preparation method thereof

    CN116713015A

  • Tungsten catalysts

    US20060091045A1