Composite aerogel aviation fabric
By designing composite structures in aerospace fabrics and subjecting airgel fibers to moisture resurgence and heat treatment, the problem of insufficient mechanical strength of airgel is solved, the fabric is lightweight and high mechanical strength is achieved, and the thermal insulation and wear resistance properties are improved. .
Patent Information
- Application Number
- CN202410752314.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Aerogels have insufficient mechanical strength in aerospace fabrics, making them easily crushed or damaged, limiting their application scope.
It adopts a structural design from the inside to the outside, including a skin-friendly layer, an airgel fiber layer, a flame retardant layer and a sealing layer. The thickness of the airgel fiber layer is not less than 1mm. It is ejected, fiber formed and pulled through the spinneret. The airgel fibers are prepared by stretching, orienting, shaping and winding, and the airgel powder is subjected to moisture resurgence treatment and heat treatment to improve its mechanical strength.
It significantly improves the mechanical strength of airgel fibers and avoids scratches, pressure damage or wear. At the same time, it maintains the thermal insulation and lightness properties of airgel and enhances the overall performance of the fabric.
Smart Images

Figure CN118744571A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fabric preparation, and in particular to a composite aerogel aviation fabric. Background Art
[0002] Aviation fabrics have a series of strict performance requirements in the application of aerospace, such as high temperature resistance, wear and damage resistance, flame retardancy, etc., to ensure that they can meet extreme operating environments and safety standards. Existing aviation fabrics are usually composed of a variety of materials, including cotton fiber, glass fiber, nylon and other chemical fibers, as well as polycarbonate, polyurethane, Teflon, chloroprene rubber, etc., which can be compounded according to different needs. However, in general, in order to achieve multi-faceted performance standards, these material combinations often have an obvious defect, that is, they are heavy and slightly bulky, which is not conducive to the movement and operation of astronauts.
[0003] Aerogel is a nano-scale porous solid material with extremely low density. The lightest silicon aerogel currently has only 0.16 mg / cm3, and it will not melt until the temperature reaches 1200 degrees Celsius. Due to these characteristics, aerogel can be used in the field of aerospace fabrics.
[0004] However, as a special material, aerogel has many unique advantages, but it also has some obvious disadvantages. The most important disadvantage is that aerogel has low density and loose structure, which leads to weak mechanical strength and is easily crushed or damaged. Especially in situations where high mechanical strength is required, the use of aerogel will have obvious limitations. Therefore, when preparing aerogel aviation fabrics, we need to overcome the defects of aerogel in mechanical strength. Summary of the invention
[0005] The purpose of the present invention is to provide a composite aerogel aviation fabric, which solves the mechanical strength defects of aerogel in aerospace fabrics.
[0006] The present invention achieves the above-mentioned purpose through the following technical solutions:
[0007] A composite aerogel aviation fabric comprises a skin-friendly layer, an aerogel fiber layer, a flame-retardant layer and a sealing layer arranged in sequence from the inside to the outside, wherein the thickness of the aerogel fiber layer is not less than 1 mm, and the preparation method comprises: taking a spinning solution and adding aerogel powder, spraying it through a spinneret after mixing evenly, and then performing fiber forming, drawing orientation, shaping and winding to obtain aerogel fibers, and finally weaving the aerogel fibers to obtain the aerogel fiber layer;
[0008] The aerogel powder is obtained by sequentially subjecting silicon dioxide aerogel powder to moisture reconditioning treatment and heat treatment.
[0009] A further improvement is that the skin-friendly layer is selected from one of a pure cotton fiber layer, a linen fiber layer, a silk fiber layer or a wool fiber layer.
[0010] A further improvement is that the spinning solution is a polyurethane resin spinning solution or a polyacrylonitrile spinning solution.
[0011] A further improvement is that the aerogel powder accounts for 60-80% of the mass of the spinning solution.
[0012] A further improvement is that the moisture regain treatment refers to placing the silica aerogel powder in a constant temperature and humidity chamber at a temperature of 40-50°C and a humidity of 80-90% for 2-5 hours, so that the moisture regain of the silica aerogel powder reaches 8-12%.
[0013] A further improvement is that during the rehumidification process, isoamyl alcohol vapor is introduced into the box and the air pressure in the box is controlled to be 300-320 kPa.
[0014] A further improvement is that the heat treatment refers to: placing the silica aerogel powder in a crucible, heating it from room temperature to 800-850°C at a heating rate of 10-12°C / min in a nitrogen atmosphere, and then keeping it warm for 0.2-0.5h.
[0015] A further improvement is that the flame retardant layer is made of aramid fiber layer, and the warp and weft density ranges from 15 to 20 strands / cm, and the fabric tightness is 40 to 60%.
[0016] A further improvement is that the sealing layer uses a PBAT high temperature resistant water vapor sealing film.
[0017] The beneficial effects of the present invention are as follows: the present invention is compounded with an aerogel fiber layer in the fabric, which is helpful to achieve the lightweight of aerospace fabrics, and the aerogel powder used in the present invention has been subjected to moisture recovery treatment and heat treatment, wherein the heat treatment can transform the aerogel powder from amorphous to crystalline, significantly improving its mechanical strength, thereby effectively avoiding scratches, pressure loss or wear, and the moisture recovery treatment can effectively reduce the pore collapse and powder aggregation during the crystal transformation process, maintain the porous skeleton structure of the aerogel, thereby maintaining the advantages of the aerogel in heat insulation and lightness, and after the moisture recovery treatment, a heat treatment of more than 800°C can be used, which helps to deepen the degree of crystal transformation. In addition, the auxiliary conditions of isoamyl alcohol vapor and high pressure are used in the moisture recovery process, which can reduce the surface tension of the powder and improve the compatibility, thereby improving the moisture recovery effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is an electron microscope SEM image of the silica aerogel powder of Example 4;
[0019] Figure 2This is an electron microscope SEM image of the silica aerogel powder of Comparative Example 1;
[0020] Figure 3 This is an electron microscope SEM image of the silica aerogel powder of Comparative Example 2; DETAILED DESCRIPTION
[0021] The present application is further described in detail below in conjunction with the accompanying drawings. It is necessary to point out here that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technical personnel in this field can make some non-essential improvements and adjustments to the present application based on the above application content.
[0022] 1. Main instruments and materials
[0023] Silica aerogel powder: Common commercially available hydrophilic silica aerogel powder is used, which is white and slightly transparent, with a particle size between 0.02-0.05mm and a density of 92.4kg / m 3 The porosity is calculated by Brunau-EmmettTeller (BET) model to be 96.5%.
[0024] Electron microscope: A scanning electron microscope (SEM) model S4800 from Hitachi, Japan was used.
[0025] 2. Implementation of the experiment
[0026] Example 1
[0027] A composite aerogel aviation fabric comprises a skin-friendly layer, an aerogel fiber layer, a flame-retardant layer and a sealing layer arranged in sequence from the inside to the outside (the layers are connected by bonding, the same below), wherein the thickness of the aerogel fiber layer is 1 mm, and the preparation method is as follows: adding aerogel powder to a polyurethane resin spinning solution, wherein the aerogel powder accounts for 60% of the mass of the spinning solution, mixing evenly and spraying through a spinneret, then undergoing fiber forming, drawing orientation, shaping and winding to obtain aerogel fibers, and finally weaving the aerogel fibers to obtain an aerogel fiber layer;
[0028] The aerogel powder is obtained by sequentially subjecting the silica aerogel powder to moisture regain treatment and heat treatment. The moisture regain treatment refers to placing the silica aerogel powder in a constant temperature and humidity chamber at a temperature of 40°C and a humidity of 80% for 5 hours (normal pressure) to make the moisture regain of the silica aerogel powder reach 8%. The heat treatment refers to placing the silica aerogel powder in a crucible, heating it from room temperature to 800°C at a heating rate of 10°C / min in a nitrogen atmosphere, and then keeping it warm for 0.5 hours.
[0029] In addition, the skin-friendly layer is made of pure cotton fiber layer. The flame-retardant layer is made of aramid fiber layer, and the warp and weft density range is 15 strands / cm, and the fabric tightness is 40%. The sealing layer is made of PBAT high temperature resistant water vapor sealing film.
[0030] Example 2
[0031] A composite aerogel aviation fabric comprises a skin-friendly layer, an aerogel fiber layer, a flame-retardant layer and a sealing layer arranged in sequence from the inside to the outside, wherein the thickness of the aerogel fiber layer is 1.2 mm, and the preparation method is as follows: adding aerogel powder to polyacrylonitrile spinning solution, wherein the aerogel powder accounts for 70% of the mass of the spinning solution, mixing evenly and then spraying out through a spinneret, and then undergoing fiber forming, drawing orientation, shaping and winding to obtain aerogel fibers, and finally weaving the aerogel fibers to obtain the aerogel fiber layer;
[0032] The aerogel powder is obtained by sequentially subjecting the silica aerogel powder to moisture regain treatment and heat treatment. The moisture regain treatment refers to placing the silica aerogel powder in a constant temperature and humidity chamber at a temperature of 45°C and a humidity of 85% for 3 hours (normal pressure) to make the moisture regain of the silica aerogel powder reach 10%. The heat treatment refers to placing the silica aerogel powder in a crucible, heating it from room temperature to 820°C at a heating rate of 11°C / min in a nitrogen atmosphere, and then keeping it warm for 0.4 hours.
[0033] In addition, the skin-friendly layer is made of silk fiber layer. The flame-retardant layer is made of aramid fiber layer, and the warp and weft density range is 18 strands / cm, and the fabric tightness is 50%. The sealing layer is made of PBAT high temperature resistant water vapor sealing film.
[0034] Example 3
[0035] A composite aerogel aviation fabric comprises a skin-friendly layer, an aerogel fiber layer, a flame-retardant layer and a sealing layer arranged in sequence from the inside to the outside, wherein the thickness of the aerogel fiber layer is 1.2 mm, and the preparation method is as follows: adding aerogel powder to a polyurethane resin spinning solution, wherein the aerogel powder accounts for 80% of the mass of the spinning solution, mixing evenly and then spraying out through a spinneret, and then undergoing fiber forming, drawing orientation, shaping and winding to obtain aerogel fibers, and finally weaving the aerogel fibers to obtain an aerogel fiber layer;
[0036] The aerogel powder is obtained by sequentially subjecting the silica aerogel powder to moisture regain treatment and heat treatment. The moisture regain treatment refers to placing the silica aerogel powder in a constant temperature and humidity chamber at a temperature of 50°C and a humidity of 90% for 2 hours (normal pressure) to make the moisture regain of the silica aerogel powder reach 12%. The heat treatment refers to placing the silica aerogel powder in a crucible, heating it from room temperature to 850°C at a heating rate of 12°C / min in a nitrogen atmosphere, and then keeping it warm for 0.2 hours.
[0037] In addition, the skin-friendly layer is made of wool fiber layer. The flame-retardant layer is made of aramid fiber layer, and the warp and weft density range is 20 strands / cm, and the fabric tightness is 60%. The sealing layer is made of PBAT high temperature resistant water vapor sealing film.
[0038] Example 4
[0039] A composite aerogel aviation fabric comprises a skin-friendly layer, an aerogel fiber layer, a flame-retardant layer and a sealing layer arranged in sequence from the inside to the outside, wherein the thickness of the aerogel fiber layer is 1.2 mm, and the preparation method is as follows: adding aerogel powder to polyacrylonitrile spinning solution, wherein the aerogel powder accounts for 70% of the mass of the spinning solution, mixing evenly and then spraying out through a spinneret, and then undergoing fiber forming, drawing orientation, shaping and winding to obtain aerogel fibers, and finally weaving the aerogel fibers to obtain the aerogel fiber layer;
[0040] The aerogel powder is obtained by sequentially subjecting the silica aerogel powder to a rehydration treatment and a heat treatment. The rehydration treatment refers to placing the silica aerogel powder in a constant temperature and humidity chamber at a temperature of 45°C and a humidity of 85% for 3 hours, so that the moisture regain of the silica aerogel powder reaches 10%; and during the rehydration treatment, isoamyl alcohol vapor is introduced into the chamber and the air pressure in the chamber is controlled to be 300 kPa. The heat treatment refers to placing the silica aerogel powder in a crucible, heating it from room temperature to 820°C at a heating rate of 11°C / min in a nitrogen atmosphere, and then keeping it warm for 0.4 hours.
[0041] The electron microscope SEM image of the obtained silica aerogel powder is as follows: Figure 1 As shown, it can be seen that crystallization has occurred, but the microscopic pore structure is rarely destroyed, and the pore collapse and powder aggregation phenomena are not obvious.
[0042] In addition, the skin-friendly layer is made of silk fiber layer. The flame-retardant layer is made of aramid fiber layer, and the warp and weft density range is 18 strands / cm, and the fabric tightness is 50%. The sealing layer is made of PBAT high temperature resistant water vapor sealing film.
[0043] Comparative Example 1
[0044] A composite aerogel aviation fabric comprises a skin-friendly layer, an aerogel fiber layer, a flame-retardant layer and a sealing layer arranged in sequence from the inside to the outside, wherein the thickness of the aerogel fiber layer is 1.2 mm, and the preparation method is as follows: adding aerogel powder to polyacrylonitrile spinning solution, wherein the aerogel powder accounts for 70% of the mass of the spinning solution, mixing evenly and then spraying out through a spinneret, and then undergoing fiber forming, drawing orientation, shaping and winding to obtain aerogel fibers, and finally weaving the aerogel fibers to obtain the aerogel fiber layer;
[0045] The aerogel powder is obtained by heat treating the silica aerogel powder. The heat treatment refers to placing the silica aerogel powder in a crucible, heating it from room temperature to 820° C. at a heating rate of 11° C. / min in a nitrogen atmosphere, and then keeping the temperature for 0.4 h.
[0046] The electron microscope SEM image of the obtained silica aerogel powder is as follows: Figure 2 As shown, it can be seen that it is completely crystallized, the microscopic pore structure is completely destroyed, and the particles become larger and aggregated together.
[0047] In addition, the skin-friendly layer is made of silk fiber layer. The flame-retardant layer is made of aramid fiber layer, and the warp and weft density range is 18 strands / cm, and the fabric tightness is 50%. The sealing layer is made of PBAT high temperature resistant water vapor sealing film.
[0048] Comparative Example 2
[0049] A composite aerogel aviation fabric comprises a skin-friendly layer, an aerogel fiber layer, a flame-retardant layer and a sealing layer arranged in sequence from the inside to the outside, wherein the thickness of the aerogel fiber layer is 1.2 mm, and the preparation method is as follows: adding aerogel powder to polyacrylonitrile spinning solution, wherein the aerogel powder accounts for 70% of the mass of the spinning solution, mixing evenly and then spraying out through a spinneret, and then undergoing fiber forming, drawing orientation, shaping and winding to obtain aerogel fibers, and finally weaving the aerogel fibers to obtain the aerogel fiber layer;
[0050] The aerogel powder is ordinary silica aerogel powder, and its electron microscope SEM image is as follows Figure 3 As shown, it can be seen that its porous structure is obvious and the particles are dispersed.
[0051] In addition, the skin-friendly layer is made of silk fiber layer. The flame-retardant layer is made of aramid fiber layer, and the warp and weft density range is 18 strands / cm, and the fabric tightness is 50%. The sealing layer is made of PBAT high temperature resistant water vapor sealing film.
[0052] 3. Performance Test
[0053] The aerogel fiber layers and the final composite aerogel aviation fabric samples prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to the following performance tests:
[0054] (1) Thermal insulation performance: Six groups of sealable glass bottles filled with 90°C water (5 bottles in each group) were taken, and each group was wrapped with the composite aerogel aviation fabric samples prepared in the above Examples 1-4 and Comparative Examples 1-2. After wrapping, they were placed at room temperature, and the water temperature in the glass bottles was recorded after 2 hours. The average temperature loss rate of each group was calculated using the calculation formula: temperature loss rate = (initial temperature - temperature after 2 hours) / initial temperature * 100%. The calculation results are statistically obtained in Table 1 below.
[0055] (2) Wear resistance: Referring to GB / T21196.2-2007 "Determination of the wear resistance of textile fabrics by the Martindale method", the aerogel fiber layer samples prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to wear resistance tests in the initial state and after being folded 10,000 times, and their wear resistance index Ai (average mass loss per friction) was detected. The statistical results are shown in Table 2 below.
[0056] 4. Results Analysis
[0057] (1) Thermal insulation performance.
[0058] Table 1: Temperature loss rate results of various embodiments and comparative examples
[0059] Group Initial temperature Temperature after 2h Average temperature loss rate / % Example 1 90.0℃ 62.1℃ 31.0% Example 2 90.0℃ 61.4℃ 31.8% Example 3 90.0℃ 63.0℃ 30.0% Example 4 90.0℃ 73.7℃ 18.1% Comparative Example 1 90.0℃ 52.9℃ 41.2% Comparative Example 2 90.0℃ 74.2℃ 17.6%
[0060] (2) Wear resistance.
[0061] Table 2: Wear resistance index Ai results of various embodiments and comparative examples
[0062]
[0063] Analysis: It can be seen from Table 1 and Table 2 above that Examples 1-3 of the present invention use silica aerogel powders that have been subjected to moisture recovery treatment and heat treatment, and their overall thermal insulation performance is good, which is significantly improved compared to Comparative Example 1 (without moisture recovery treatment). The wear resistance of Examples 1-3 is also good, close to the level of Comparative Example 1, and significantly better than Comparative Example 2 (ordinary silica aerogel powder); Based on Example 2, Example 4 of the present invention adds auxiliary conditions of isoamyl alcohol vapor and high pressure during the moisture recovery treatment, so that the thermal insulation performance is further improved, which is equivalent to Comparative Example 2; In addition, the silica aerogel powder of Comparative Example 1 has only been heat-treated, and although its wear resistance is the best, its thermal insulation performance is the worst; Comparative Example 2 uses ordinary silica aerogel powder, and its thermal insulation performance is the best, but its wear resistance is the worst.
[0064] In summary, the present invention uses silica aerogel powder that has been subjected to moisture recovery and heat treatment, effectively reducing pore collapse and powder aggregation during the crystal transformation process, maintaining the porous skeleton structure of the aerogel, and thus maintaining the advantages of the aerogel in thermal insulation performance, so that the fabric fiber layer has both thermal insulation and mechanical strength. And after moisture recovery treatment, heat treatment above 800°C can be used (generally, heat treatment above 700°C will basically completely destroy the aerogel structure and make it lose its function), which helps to deepen the degree of crystal transformation. In addition, the auxiliary conditions of isoamyl alcohol vapor and high pressure are used in the moisture recovery process, which can reduce the surface tension of the powder and improve the compatibility, thereby improving the moisture recovery effect, and ultimately reflected in the further improvement of thermal insulation performance.
[0065] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A composite aerogel aviation fabric, characterized in that: The invention comprises a skin-friendly layer, an aerogel fiber layer, a flame-retardant layer and a sealing layer which are sequentially arranged from the inside to the outside, wherein the thickness of the aerogel fiber layer is not less than 1 mm, and the preparation method comprises: taking a spinning solution and adding aerogel powder, spraying the mixture through a spinneret after uniform mixing, and then performing fiber forming, drawing orientation, shaping and winding to obtain aerogel fibers, and finally weaving the aerogel fibers to obtain the aerogel fiber layer; The aerogel powder is obtained by sequentially subjecting silicon dioxide aerogel powder to moisture reconditioning treatment and heat treatment.
2. The composite aerogel aviation fabric according to claim 1, characterized in that: The skin-friendly layer is selected from one of a pure cotton fiber layer, a hemp fiber layer, a silk fiber layer or a wool fiber layer.
3. The composite aerogel aviation fabric according to claim 1, characterized in that: The spinning solution is selected from polyurethane resin spinning solution or polyacrylonitrile spinning solution.
4. The composite aerogel aviation fabric according to claim 1, characterized in that: The aerogel powder accounts for 60-80% of the mass of the spinning solution.
5. The composite aerogel aviation fabric according to claim 1, characterized in that: The moisture regain treatment refers to placing the silica aerogel powder in a constant temperature and humidity chamber at a temperature of 40-50° C. and a humidity of 80-90% for 2-5 hours, so that the moisture regain of the silica aerogel powder reaches 8-12%.
6. The composite aerogel aviation fabric according to claim 5, characterized in that: During the rehumidification process, isoamyl alcohol vapor is introduced into the box and the air pressure in the box is controlled at 300-320 kPa.
7. The composite aerogel aviation fabric according to claim 1, characterized in that: The heat treatment refers to: placing the silica aerogel powder in a crucible, heating it from room temperature to 800-850° C. at a heating rate of 10-12° C. / min in a nitrogen atmosphere, and then keeping the temperature for 0.2-0.5 h.
8. The composite aerogel aviation fabric according to claim 1, characterized in that: The flame retardant layer is made of aramid fiber layer, and the warp and weft density ranges from 15 to 20 strands / cm, and the fabric tightness is 40 to 60%.
9. The composite aerogel aviation fabric according to claim 1, characterized in that: The sealing layer adopts PBAT high temperature resistant water vapor sealing film.
Citation Information
Patent Citations
Silicon dioxide aerogel coating and preparation method thereof
CN108084746A
Preparation method of water-resisting aerogel material
CN108249943A
Preparation method of nano cellulose aerogel composite fabric
CN112411187A
Preparation method of polylactic acid aerogel composite functional fiber
CN114214756A
Multifunctional thermal protection suit fabric for high-temperature operation and preparation method thereof
CN114889256A
Cited By
Para-aramid aerogel fiber and preparation method thereof
CN119162689A