Method for preparing carbon nano tube by using waste olefin plastic and waste carbon fiber as raw materials and application of carbon nano tube in supercapacitor
By using waste olefin plastics and waste carbon fibers to grow carbon nanotubes in a tube furnace, the problems of high carbon nanotube growth costs and complex carbon fiber production are solved, and the preparation of high-performance carbon nanotubes and the reuse of waste are achieved. Suitable for supercapacitors.
Patent Information
- Application Number
- CN202410744550.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing technology, the growth of carbon nanotubes on carbon fibers requires expensive catalysts and gases, which limits its large-scale application. The high cost and complex production process of carbon fibers and the difficulty in waste disposal are also common.
Waste olefin plastics and waste carbon fibers are used as raw materials, and carbon nanotubes are grown in a tube furnace through steps such as pyrolysis, activation, electroplating and thermal decomposition. HZSM-5 catalyst and Fe2+/Fe3+ solution are used to promote the reaction to form high-performance Carbon nanotubes.
It achieves cost-effective growth of carbon nanotubes, improves the conductivity of carbon fiber, solves the environmental and management problems of waste materials, and provides supercapacitor materials with high specific capacity and specific capacity retention rate.
Smart Images

Figure BDA0004885996530000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon nanotube preparation, and in particular to a method for preparing carbon nanotubes using waste olefin plastics and waste carbon fibers as raw materials, and application of the method in supercapacitors. Background Art
[0002] Double layer capacitors are a special type of capacitor, also called supercapacitors, which have higher capacitance and energy density than traditional electrolytic capacitors. Double layer capacitors usually consist of two electrodes and an electrolyte between them. The electrolyte allows ions to move between the two electrodes, thus forming an electric charge. An important feature is the large specific surface area of the electrode surface, which can accommodate more charge. This problem can be solved by using carbon materials with high surface area and conductive properties to achieve the advantages of high power density, fast charging and discharging, long life and low internal resistance of double layer capacitors.
[0003] Carbon fiber is widely used in our lives because of its excellent strength. However, carbon fiber also has problems such as high cost, complex production process, and long preparation cycle, and how to dispose of waste has also become an environmental problem. Therefore, the recycling and reuse of waste plastic carbon fiber can not only solve the cost and environmental damage problems, but also prepare higher performance carbon fiber through modification. A common modification method is to enhance the performance of carbon fiber by adding carbon nanotubes. Because carbon nanotubes have excellent electrical conductivity, growing them on the surface of carbon fiber can significantly improve the electrical conductivity of carbon fiber, making it more widely used in some electronic devices and composite materials. A common preparation method is through CVD vapor deposition. In this way, carbon fiber grows carbon nanotubes. However, such methods usually involve the need for expensive catalysts and gases. This may limit the feasibility of large-scale application of carbon nanotubes grown on carbon fiber.
[0004] Therefore, it is of great application value to develop a carbon fiber grown carbon nanotube that is economical, improves the functionality of carbon fiber, and can be mass-produced. Summary of the invention
[0005] In order to overcome at least one of the technical problems existing in the prior art, the present invention provides a method for preparing carbon nanotubes using waste olefin plastics and waste carbon fibers as raw materials and an application thereof in supercapacitors.
[0006] The technical solution of the present invention is as follows:
[0007] The present invention first provides a method for preparing carbon nanotubes using waste olefin plastics and waste carbon fibers as raw materials, which comprises the following steps:
[0008] (1) introducing a mixed gas into a tubular furnace to pyrolyze the waste carbon fiber material to obtain desized carbon fiber; then placing the desized carbon fiber into a H2O2 solution for activation to obtain a pretreated carbon fiber;
[0009] (2) preparing a metal ion solution, and then electroplating the pretreated carbon fiber to obtain a carbon fiber coated with metal nanoparticles;
[0010] (3) Mixing the waste polyolefin material with the catalyst and placing it in the first temperature zone of the tubular furnace, followed by heating and decomposition to form small molecule compounds; under the impetus of protective gas, the small molecule compounds are input into the second temperature zone of the tubular furnace where carbon fibers coated with iron nanoparticles are placed to react and obtain carbon nanotubes.
[0011] Preferably, the mixed gas in step (1) comprises oxygen and nitrogen.
[0012] Preferably, the volume ratio of oxygen to nitrogen is 1:3-1:6.
[0013] Preferably, the metal ion solution in step (2) specifically refers to a solution containing Fe 2+ with Fe 3+ of solution.
[0014] Preferably, the Fe-containing 2+ with Fe 3+ Fe in solution 2+ with Fe 3+ The concentrations are 1 to 3 mol / L respectively.
[0015] Preferably, Fe 2+ with Fe 3+ The solution is specifically prepared with ferric chloride and ferrous chloride.
[0016] Preferably, the carbon fiber coated with metal nanoparticles is specifically carbon fiber coated with iron nanoparticles.
[0017] Preferably, the catalyst in step (3) is HZSM-5; wherein the weight ratio of the catalyst to the waste polyolefin material is 1:18-1:31.
[0018] Preferably, the waste polyolefin materials include waste petroleum wax, waste packaging films, waste lunch boxes and waste masks.
[0019] The invention also provides an application of the carbon nanotubes prepared by the method in a supercapacitor.
[0020] Beneficial effects: The present invention provides a new method for preparing carbon nanotubes; studies have shown that the negative electrode sheet made of carbon nanotubes prepared by the method of the present invention is used in supercapacitors, and has a high specific capacity and specific capacity retention rate after multiple cycles.
[0021] In addition, the present invention not only solves the environmental and management impacts brought about by the treatment of waste materials, but also enhances the economic value of the waste; it provides a new development direction for the recycling of waste carbon fiber materials and polyolefin materials. DETAILED DESCRIPTION
[0022] The present invention is further explained below in conjunction with specific examples, but the examples do not limit the protection scope of the present invention.
[0023] The waste polyolefin material used in the following embodiments is waste lunch boxes.
[0024] Example 1
[0025] (1) introducing a mixed gas into a tubular furnace, pyrolyzing the waste carbon fiber material at 470° C. for 60 minutes to obtain desizing carbon fiber; then placing the desizing carbon fiber in a H2O2 solution for activation for 3 hours, taking it out, washing and drying it to obtain pretreated carbon fiber; wherein the mixed gas is composed of oxygen and nitrogen in a volume ratio of 1:4;
[0026] (2) Preparation of Fe 2+ with Fe 3+ The solution is adjusted to pH 3.0 with HCl and NaOH; the pretreated carbon fiber is then electroplated to obtain carbon fiber coated with iron nanoparticles; the Fe-containing 2+ with Fe 3+ The solution is made of ferric chloride and ferrous chloride; Fe 2+ The concentrations were 2 mol / L, Fe 3+ The concentrations are 1 mol / L respectively; the specific method of electroplating is: immersing the two stages in the configured solution, using the pretreated carbon fiber as the cathode and the pure iron sheet as the anode; the electroplating process is carried out at room temperature of 25°C and at a speed of 1A / dm 2 The current density was used for electroplating for 20 minutes;
[0027] (3) Mixing the waste polyolefin material with the catalyst and placing it in the first temperature zone of a tubular furnace, followed by heating and decomposing it to form small molecule compounds; under the impetus of a protective gas, the small molecule compounds are input into the second temperature zone of the tubular furnace where carbon fibers coated with iron nanoparticles are placed for reaction to obtain carbon nanotubes; the catalyst is HZSM-5; wherein the weight ratio of the waste polyolefin material to the catalyst is 20:1; the heating and decomposition temperature of the first temperature zone of the tubular furnace is 450°C; the reaction temperature of the second temperature zone of the tubular furnace is 500°C, and the reaction time is hours.
[0028] Example 2
[0029] Only the ratio of oxygen to nitrogen introduced in step (1) of Example 1 was changed; the remaining parameters and steps were the same as those of Example 1;
[0030] The mixed gas is composed of oxygen and nitrogen in a volume ratio of 1:5.
[0031] Example 3
[0032] Only the ratio of oxygen to nitrogen introduced in step (1) of Example 1 was changed; the remaining parameters and steps were the same as those of Example 1;
[0033] The mixed gas is composed of oxygen and nitrogen in a volume ratio of 1:6.
[0034] Example 4
[0035] Only the weight ratio of the waste polyolefin material to the catalyst in step (3) of Example 1 was changed; the other parameters and steps were the same as those in Example 1;
[0036] The weight ratio of the waste polyolefin material to the catalyst is 19:1.
[0037] Example 5
[0038] Only the weight ratio of the waste polyolefin material to the catalyst in step (3) of Example 1 was changed; the other parameters and steps were the same as those in Example 1;
[0039] The weight ratio of the waste polyolefin material to the catalyst is 18:1.
[0040] Example 6
[0041] Only the weight ratio of the waste polyolefin material to the catalyst in step (3) of Example 1 was changed; the other parameters and steps were the same as those in Example 1;
[0042] The weight ratio of the waste polyolefin material to the catalyst is 17:1.
[0043] Comparative Example 1
[0044] (1) introducing a mixed gas into a tubular furnace, pyrolyzing the waste carbon fiber material at 470° C. for 60 minutes to obtain desizing carbon fiber; then placing the desizing carbon fiber in a H2O2 solution for activation for 3 hours, taking it out, washing and drying it to obtain pretreated carbon fiber; wherein the mixed gas is composed of oxygen and nitrogen in a volume ratio of 1:4;
[0045] (2) Mixing the waste polyolefin material with the catalyst and placing it in the first temperature zone of a tubular furnace, followed by heating and decomposing it to form small molecule compounds; under the impetus of a protective gas, the small molecule compounds are input into the second temperature zone of the tubular furnace where pretreated carbon fibers are placed for reaction to obtain carbon nanotubes; the catalyst is HZSM-5; wherein the weight ratio of the waste polyolefin material to the catalyst is 20:1; the heating and decomposition temperature of the first temperature zone of the tubular furnace is 450°C; the reaction temperature of the second temperature zone of the tubular furnace is 500°C, and the reaction time is hours.
[0046] The difference between Comparative Example 1 and Example 1 is that the step of preparing the carbon fiber coated with iron nanoparticles is not performed by electroplating.
[0047] Comparative Example 2
[0048] The only difference in Example 1 is that the catalyst is not added in step (3); the remaining parameters and steps are the same as those in Example 1.
[0049] The carbon nanotubes prepared in Examples 1 to 6 of the present invention and Comparative Example 1 were mixed with carbon black and binder PVDF in a mass ratio of 8:1:1 as negative electrode materials to form negative electrode sheets. Activated carbon, carbon black and binder PVDF were mixed in a mass ratio of 8:1:1 as positive electrode materials to form positive electrode sheets. The positive electrode sheets and negative electrode sheets were used to form supercapacitors, and their specific capacity and specific capacity retention rate after 50,000 cycles were tested; the test results are shown in Table 1.
[0050] Table 1. Specific capacity and specific capacity retention rate test results after 50,000 cycles
[0051] Specific volume ratio Specific capacity retention rate Carbon nanotubes prepared in Example 1 115F / g 76% Carbon nanotubes prepared in Example 2 131F / g 84% Carbon nanotubes prepared in Example 3 120F / g 79% Carbon nanotubes prepared in Example 4 132F / g 81% Example 5 Carbon nanotubes prepared 136F / g 84% Carbon nanotubes prepared in Example 6 135F / g 84% Carbon nanotubes prepared in Comparative Example 1 92F / g 58%
[0052] From the data in Table 1, we can see the effect of different carbon fiber thermal pretreatment temperatures on the electrochemical properties of the material. From Table 1 Examples 1 to 3, we can see that the ratio of mixed gas oxygen to nitrogen of 1:5 is the most suitable precursor for preparing carbon materials. Excessively high oxygen concentration and low oxygen concentration have an effect on the electrochemical properties of the material. This indicates that a certain proportion of mixed gas concentration plays an important role in the pretreatment of waste carbon fibers. In the process of providing small molecule olefins through waste polyolefin carbon materials. The ratio of waste plastics to molecular sieve HZSM-5 affects the subsequent growth of carbon nanotubes. HZSM-5 can promote the pyrolysis of waste polyolefin plastics to produce more light hydrocarbons (C1-C5), which is conducive to the generation of carbon nanotubes. From the data in Table 1, it can be seen that the performance of dry plastics and HZSM-5 placed at 18:1 is excellent.
[0053] From the data in Table 1, we can see that the specific capacity rate and specific capacity retention rate of the carbon nanotubes prepared in Example 1 after 50,000 cycles are significantly higher than those of the carbon nanotubes prepared in Comparative Example 1; this indicates that: in the preparation method of the present invention, the pretreated carbon fiber is placed in a Fe-containing 2+ with Fe 3+ The carbon nanotubes prepared by electroplating the carbon fibers coated with metal nanoparticles in a solution can greatly improve the specific capacity rate of the carbon nanotubes and the specific capacity retention rate after 50,000 cycles compared with the carbon nanotubes prepared without this step.
[0054] The carbon yield of the waste polyolefin material can be calculated by the following equation, where yc represents the carbon yield, mp represents the mass of the plastic bag, the mass of the pretreated carbon fiber, and mt represents the total weight of the product after the reaction.
[0055]
[0056] Table 2. Carbon yield of the method of the present invention
[0057] Carbon fiber mass / g Carbon yield Carbon nanotubes prepared in Example 4 1.5 37% Carbon nanotubes prepared in Example 5 1.5 41.5% Carbon nanotubes prepared in Example 6 1.5 41.1% Carbon nanotubes prepared in Comparative Example 2 1.5 32%
[0058] The carbon nanotubes prepared in Table 2 Examples 4 to 6 and Comparative Example 2 were combined to test the carbon material yield of their carbon yield. It was found that when HZSM-5 was present, the carbon yield was much higher than the carbon yield of HZSM-5 without placement. In Comparative Examples 4 to 6, too little molecular sieve may not provide enough active sites to promote the reaction, thereby reducing the decomposition efficiency, but excessive molecular sieve may cause the reaction rate to be saturated and unable to be further improved.
Claims
1. A method for preparing carbon nanotubes using waste olefin plastics and waste carbon fibers as raw materials, characterized in that: The following steps are included: (1) introducing a mixed gas into a tubular furnace to pyrolyze the waste carbon fiber material to obtain desized carbon fiber; then placing the desized carbon fiber into a H2O2 solution for activation to obtain a pretreated carbon fiber; (2) preparing a metal ion solution, and then electroplating the pretreated carbon fiber to obtain a carbon fiber coated with metal nanoparticles; (3) Mixing the waste polyolefin material with the catalyst and placing it in the first temperature zone of the tubular furnace, followed by heating and decomposition to form small molecule compounds; under the impetus of protective gas, the small molecule compounds are input into the second temperature zone of the tubular furnace where carbon fibers coated with iron nanoparticles are placed to react and obtain carbon nanotubes.
2. The method according to claim 1, characterized in that The mixed gas described in step (1) contains oxygen and nitrogen.
3. The method according to claim 2, characterized in that The volume ratio of oxygen to nitrogen is 1:3-1:
6.
4. The method according to claim 1, characterized in that: The metal ion solution described in step (2) specifically refers to a solution containing Fe 2+ with Fe 3+ of solution.
5. The method according to claim 4, characterized in that The Fe-containing 2+ with Fe 3+ Fe in solution 2+ with Fe 3+ The concentrations are 1 to 3 mol / L respectively.
6. The method according to claim 5, characterized in that Formulated Fe 2+ with Fe 3+ The solution is specifically prepared with ferric chloride and ferrous chloride.
7. The method according to claim 1, characterized in that The metal nanoparticle-coated carbon fiber is specifically iron nanoparticle-coated carbon fiber.
8. The method according to claim 1, characterized in that The catalyst described in step (3) is HZSM-5; wherein the weight ratio of the catalyst to the waste polyolefin material is 1:18-1:
31.
9. The method according to claim 1, characterized in that: The waste polyolefin materials include waste petroleum wax, waste packaging film, waste lunch box and waste mask.
10. Use of the carbon nanotubes prepared by the method according to any one of claims 1 to 9 in supercapacitors.
Citation Information
Patent Citations
Carbon fiber substrates having carbon nanotubes grown thereon and processes for production thereof
CN103118975A
Preparation method of nano SiBNC fiber growing on surfaces of carbon fiber
CN108532296A
Device and method for uniformly growing carbon nanotubes on surface of carbon fiber cloth
CN108625159A
Surface treatment method at earlier stage of even growth of carbon nanotubes (CNTs) on surface of carbon cloth
CN109750492A
Method for preparing high value-added hydrocarbon from waste plastic under mild condition
CN115322803A
Cited By
Preparation method of soft and hard heterostructure porous carbon and application of soft and hard heterostructure porous carbon in supercapacitor
CN119683626A
Preparation method of soft-hard heterostructure porous carbon and application thereof in supercapacitor
CN119683626B