Lithium slag-based alkali-activated cementing material as well as preparation method and application thereof
Through the combined use of solid waste such as lithium slag with alkali activators, silica fume, etc., lithium slag-based alkali-activated cementitious materials with high flexural strength, short setting time, and good stability are prepared, which solves the problem of high energy consumption and high stability of cement-based materials. It solves the problem of carbon emissions and realizes the utilization of solid waste resources to meet the needs of sustainable development.
Patent Information
- Application Number
- CN202410926188.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-08
AI Technical Summary
Existing cement-based materials have high energy consumption, carbon emissions and environmental pollution problems during the production process, as well as the brittleness and insufficient mechanical properties of alkali-activated cementitious materials, which limit their application.
The lithium slag-based alkali-activated gelling material is prepared by using solid wastes such as lithium slag and lepidolite mineral processing tailings together with alkali activators, silica fume, water-reducing agents and organic admixtures to improve material toughness and mechanics through inorganic-organic interactions. performance to achieve resource utilization of solid waste.
A cementitious material with high flexural strength, short setting time, high early strength, good stability, and low heavy metal leaching concentration has been achieved to meet the needs of sustainable development and reduce production costs.
Smart Images

Figure BDA0004938222470000061 
Figure BDA0004938222470000071 
Figure BDA0004938222470000081
Abstract
Description
Technical Field
[0001] The invention relates to the field of building materials, and in particular to a lithium slag-based alkali-activated gelling material and a preparation method and application thereof. Background Art
[0002] In the construction industry, cement-based materials are currently the main materials used to produce various infrastructures. However, the production of cement not only consumes high energy, but also emits a large amount of carbon dioxide and consumes a large amount of natural minerals, which cannot meet the needs of green and sustainable development of modern building materials.
[0003] Lithium slag is the waste residue produced in the process of lithium extraction from spodumene or lepidolite acid. The annual output of lithium slag is about 1.2 million tons, and the process of lithium extraction will cause the enrichment of heavy metal elements. The basic treatment methods of lithium slag are mostly landfill or open-air stacking, which will pollute the environment and groundwater. Tailing mud is the ore mud produced by the lepidolite beneficiation plant in the production process. The yield is about 20%, the activity is low, and the utilization value is low. After high-temperature roasting, mechanical grinding and chemical leaching, the lithium slag has a porous structure and contains a high SiO 2 and Al 2 O 3 , has certain volcanic ash activity, but adding a high proportion of lithium slag directly into cement will still lead to reduced mechanical properties of cement and reduced fluidity of mortar due to its insufficient activity. Therefore, the amount of lithium slag added to traditional cement should not be too large, and its comprehensive utilization effect is not ideal.
[0004] Alkali activated cementitious materials are made of SiO 2 and Al 2 O 3 The raw materials of CaO react with alkaline solution. Compared with the production process of cement, the carbon emission can be reduced by up to 80% according to the different raw materials and alkali activators used. Alkali-activated cementitious materials have the advantages of low production cost, wide range of raw material selection, early strength, corrosion resistance, good fire resistance, etc., but alkali-activated materials are mainly inorganic materials with covalent bonds and ionic bonds as the main and van der Waals bonds as the auxiliary. There are gaps between ionic bonds and covalent bonds. When subjected to external forces, ionic bonds and covalent bonds will not deform, but will directly break, so the material is brittle and has low flexural strength. In addition, the hydroxides in the activators currently used are mostly strong alkaline activators such as sodium hydroxide and potassium hydroxide. When the addition amount is low, the alkalinity is too low to effectively carry out the alkali activation reaction. When the addition amount is too high, there will be alkali-aggregate reaction, resulting in reduced mechanical properties of the material or expansion cracking. The existence of these problems has led to certain restrictions on the application of geopolymers. Therefore, it is urgent to develop a cementitious material with high flexural strength and good stability, and at the same time make full use of solid waste resources such as lithium slag and slag to meet the needs of sustainable development in contemporary society. Summary of the invention
[0005] In view of the defects in the prior art, the present invention provides a lithium slag-based alkali-activated gelling material and a preparation method thereof.
[0006] The present invention provides a lithium slag-based cementitious material, which comprises, by weight, 30-55 parts of lithium slag, such as 30, 32, 35, 40, 42, 45, 48, 50, 52, 55 parts; 0-20 parts of lithium mica ore dressing tailings, such as 0, 2, 4, 5, 6, 8, 10, 12, 15, 20 parts; 20-40 parts of slag, such as 20, 25, 30, 35, 40 parts; 0-20 parts of fly ash, such as 0, 5, 10, 15, 20 parts; silica fume 1-5 parts, such as 1, 2, 3, 4, 5 parts; alkali activator 5-12 parts, such as 5, 8, 10, 12 parts; water reducer 0.5-2 parts, such as 0.5, 1, 1.5, 2 parts; organic admixture 0.1-1 parts, such as 0.1, 0.3, 0.5, 0.7, 0.8, 1 parts; wherein the alkali activator is composed of 3-6 parts of hydroxide and 3-6 parts of silicate.
[0007] The present invention uses solid wastes such as lithium slag and ore dressing tailings as raw materials, and prepares alkali-activated cementitious materials together with alkali activator, silica fume, water reducer and organic admixture, which not only realizes the resource utilization of solid wastes, but also improves the toughness of the materials through the interaction between inorganic and organic matter, improves the mechanical properties of the materials, and is more conducive to the utilization of alkali-activated cementitious materials;
[0008] The hydroxide and silicate in the alkaline activator are both in powder form. The role of the hydroxide in the alkaline activating reaction is mainly to destroy the structure of the raw material and promote the formation of gel. When the hydroxide is added too little, the alkaline substance provided is not enough to depolymerize the aluminosilicate component in the raw material. When the hydroxide is added too much, due to the low solubility, the insufficiently dissolved hydroxide affects the internal structure of the material and thus also affects the mechanical properties of the material. Silicate forms SiO in the early stage of hydration. 4 4- , directly participate in the hydration reaction, increase the amount of gel generated in the system, and improve the early strength of the material. When the amount of silicate added is too little, the mechanical properties of the material will not be significantly improved, while excessive addition will increase the viscosity of the slurry, which is not conducive to stirring and the hydration reaction. Since the later strength growth of the material is mainly provided by the active aluminosilicate substances depolymerized in the raw materials, it is necessary to compound the silicate and the hydroxide to ensure the full progress of the reaction;
[0009] The solid waste raw materials are depolymerized into ionic states under the action of the alkaline activator, and then further form two-dimensional and three-dimensional gel-state aluminosilicates, which have a coating effect on heavy metal ions and raw materials with low reaction activity. The specific water reducer added in the present application will not reduce the working performance under alkaline conditions, and can reduce the amount of water required for mixing, reduce the porosity, thereby improving the mechanical properties and reducing the leaching of alkali metal ions. The addition of organic admixtures can penetrate and fill the cementitious material with the cementitious material during the hydration process of the raw materials to form a cross-linked network structure, and hydrogen bonds are formed between the organic matter and the cementitious material, and hydroxyl reactions occur at the same time. A more complex and dense structure is formed inside the material through hydrogen bonds, and an appropriate amount of organic matter added can also adhere to the surface of the cementitious material to act as a filler, fill the pores of the material to improve the density of the material, thereby improving the performance of the material.
[0010] Furthermore, the silicate is any one of sodium silicate and potassium silicate, preferably sodium silicate.
[0011] Furthermore, the hydroxide is any one of calcium hydroxide and lithium hydroxide, preferably calcium hydroxide. Calcium hydroxide and lithium hydroxide have low solubility in water, and adding an appropriate amount will not cause alkali-aggregate reaction, and adding calcium hydroxide can provide a certain amount of Ca in the system. 2+ , promote the reaction and improve early strength.
[0012] Furthermore, the water reducer is any one of a naphthalene-based water reducer, calcium lignin sulfonate, and a melamine water reducer, and is preferably a naphthalene-based water reducer.
[0013] Furthermore, the organic admixture is selected from any one or more of polyethylene glycol, polyvinyl alcohol, chitosan, and xanthan gum, preferably chitosan.
[0014] Furthermore, the particle size of the lithium slag and lithium mica ore dressing tailings is 45-74 μm, such as 45, 50, 55, 60, 65, 70, 74 μm. The lithium slag and lithium mica ore dressing tailings in this particle size range have relatively high volcanic ash activity and low water absorption. The particle size is tested according to the standard screening method for determination of particle size in inorganic chemical products GB / T 21524-2008.
[0015] Furthermore, the particle size of the slag and fly ash is ≤35 μm. The slag and fly ash within this particle size range have a large surface area and high activity, which is conducive to better depolymerization and reorganization in an alkaline environment and exerting gelling properties. The particle size is tested according to the standard screening method for determination of particle size in inorganic chemical products GB / T 21524-2008.
[0016] Furthermore, the particle size of the silica fume is 1-6μm, such as 1, 2, 3, 4, 5, 6μm. The silica fume in this particle size range is highly active and can not only generate more active gel components, but the unreacted silica fume can also fill the pores. However, excessive addition of silica fume will lead to a reduction in free water inside the material, and the rapid dissolution of a large amount of silica fume will reduce the alkalinity in the material slurry and affect the alkali-induced reaction. The preferred particle size is 2-3μm, and the particle size is tested according to the standard sieving method for determination of particle size in inorganic chemical products GB / T 21524-2008.
[0017] Furthermore, the organic admixture is 0.5-1 parts by weight, such as 0.5, 0.6, 0.7, 0.8, 0.9, 1 part.
[0018] Furthermore, the CaO content in the fly ash is ≤10%, and the CaO content is determined by X-ray fluorescence spectrometry (XRF).
[0019] Furthermore, SiO in silica fume 2 Content ≥94%, SiO 2 The content was determined using X-ray fluorescence spectrometry (XRF).
[0020] The present invention also provides a method for preparing the gelling material, comprising the following steps:
[0021] Drying: Dry lithium slag, slag, tailings, fly ash and silica fume in an oven at 100-110℃ for 12-24h to ensure that the moisture content of each raw material is ≤1%;
[0022] Ball milling: Use a ball mill to grind the dried lithium slag, slag, tailings and fly ash separately;
[0023] Screening: Screen the lithium slag, slag, tailings and fly ash after ball milling to select powder with appropriate particle size;
[0024] Mixing: weigh the dried ball-milled and sieved lithium slag, slag, tailings, fly ash, silica fume, alkali activator, water reducing agent, and organic admixture according to weight proportions and mix them evenly to obtain a solid waste-alkali activator mixture;
[0025] Stirring: Mix the solid waste-alkali activator mixture with water at a liquid-to-solid ratio of 0.3-0.4 to obtain a slurry;
[0026] Casting and molding: Pour the slurry into a 40×40×160mm triple steel mold, flatten the mold surface and cover it with plastic wrap;
[0027] Curing: After casting, cure in a standard curing box (temperature 20°C, relative humidity 95%) for 23-24 hours. Demould after the curing time, and then cure at room temperature and humidity to the specified age (3d, 28d) to obtain a lithium slag-based alkali-activated cementitious material.
[0028] The invention also provides application of the cementitious material as a building substrate.
[0029] In summary, compared with the prior art, the present invention achieves the following technical effects:
[0030] (1) The lithium slag-based cementitious material provided by the present invention has high flexural strength.
[0031] (2) The lithium slag-based cementitious material provided by the present invention has a short setting time and high early strength.
[0032] (3) The lithium slag-based cementitious material provided by the present invention has satisfactory stability.
[0033] (4) The lithium slag-based gelling material provided by the present invention has a low heavy metal leaching concentration.
[0034] (5) The raw materials used in the lithium slag-based cementitious material provided by the present invention are all solid waste materials, which can realize the resource utilization of solid waste.
[0035] (6) The lithium slag-based gelling material preparation method provided by the present invention has a simple process flow and low production cost. DETAILED DESCRIPTION
[0036] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0037] Example
[0038] The present invention is further described below in conjunction with specific examples and comparative examples. The following specific examples are all preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the following examples, and are particularly not limited to the types of the various component raw materials used in the following specific examples.
[0039] 1. Examples and Comparative Examples Sources of Raw Materials
[0040] The solid waste raw materials (lithium slag, lithium mica ore dressing tailings, slag, fly ash) used in the examples and comparative examples of the present application, wherein lithium slag and lithium mica ore dressing tailings were purchased from Jiangxi Lingneng Lithium Industry Co., Ltd., slag was purchased from Guizhou Riheng Resource Utilization Co., Ltd., fly ash was purchased from Guizhou Mingchuan Fly Ash Co., Ltd., and the different particle sizes of each solid waste raw material were obtained by ball milling and sieving, silica ash was purchased from Guizhou Baiwang Building Materials Technology Co., Ltd., and the alkali activator, water reducer, and organic admixture were all commercially available;
[0041] Table 1 Raw materials used in the examples and comparative examples
[0042]
[0043]
[0044] The preparation method of the lithium slag based alkali activated gelling material of the embodiment of the present invention and the comparative example comprises the following steps:
[0045] Drying: Dry lithium slag, slag, tailings, fly ash and silica fume in an oven at 110℃ for 24h to ensure that the moisture content of each substance is ≤1%;
[0046] Ball milling: Use a ball mill to grind the dried lithium slag, slag, tailings and fly ash separately;
[0047] Screening: Screen the lithium slag, slag, tailings and fly ash after ball milling to select powder with the required particle size;
[0048] Mixing: weigh the dried ball-milled and sieved lithium slag, slag, tailings, fly ash, silica fume, alkali activator, water reducing agent and organic admixture respectively according to weight proportions and mix them evenly to obtain a solid waste-alkali activator mixture;
[0049] Stirring: mixing the solid waste-alkali activator mixture with water to obtain a slurry;
[0050] Casting and molding: Pour the slurry into a 40×40×160mm triple steel mold, flatten the mold surface and cover it with plastic wrap;
[0051] Curing: After casting, it is cured in a standard curing box (temperature 20°C, relative humidity 95%) for 24 hours and then demoulded. It is then cured at room temperature and humidity to a specified age to obtain a lithium slag-based alkali-activated cementitious material.
[0052] 2. Various performance tests
[0053] (1) Stability and setting time determination: Test according to GB / T1346-2011 "Standard consistency, setting time and stability test method for cement";
[0054] (2) Determination of compressive and flexural strength of test blocks: Test according to GB / T17671-2021 “Test method for strength of cement mortar (ISO method)”;
[0055] (3) Determination of heavy metal leaching toxicity of 28-day-old samples: The test was carried out in accordance with the "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid and Nitric Acid Method" HJ / T299-2007.
[0056] Table 2 Technical solution of the embodiment (unit is weight part)
[0057]
[0058] Table 3 Comparative Example Technical Scheme (Units are parts by weight)
[0059]
[0060] Table 4 Technical effects of embodiments and comparative examples
[0061]
[0062] Table 5 Heavy metal ion leaching of examples and comparative examples
[0063]
[0064]
[0065] The lithium slag based alkali-activated cementitious materials prepared in Examples 1-8 have a short setting time, all less than 179 minutes, and high flexural strength and compressive strength. After a 3-day curing period, the flexural strength is higher than 4.0 MPa, and the compressive strength is higher than 20.1 MPa. After a 28-day curing period, the flexural strength is higher than 6.9 MPa, and the compressive strength is higher than 44.3 MPa. The detected heavy metal ion leaching detection values all meet the requirements of national standards. All cementitious materials in Examples 1-8 can maintain good compressive and flexural strength of the materials under the premise of short setting time, and the heavy metal ion leaching detection values are low, which truly realizes the resource utilization of solid waste materials and meets the needs of sustainable development.
[0066] Comparative Examples 1-5 are all compared with Example 1. In Comparative Example 1, too much silica fume is added, resulting in excessive water demand of the cementitious material, uneven mixing, and the setting time is too short, so the hydration reaction cannot proceed normally, and the stability is poor; in Comparative Example 2, too little hydroxide is added, so that the hydroxyl ions in the slurry are relatively small, and the structure of the aluminosilicate in the raw material cannot be destroyed, resulting in poor mechanical properties; in Comparative Example 3, too little silicate is added, resulting in poor mechanical properties; in Comparative Example 4, no organic admixture is added, resulting in greater material brittleness and lower flexural strength; in Comparative Example 5, no water reducer is added, resulting in poor early mechanical properties and a long setting time. All of the above comparative examples cannot simultaneously achieve good compressive and flexural properties under the premise of short setting time, so as to achieve effective utilization of solid waste raw materials.
[0067] Based on the test data of compressive strength, flexural strength, setting time, stability and heavy metal ion leaching value in Tables 4 and 5, the lithium slag-based alkali-activated cementitious material prepared by Examples 1-8 has obvious advantages over the comparative examples and can effectively meet the high standards of customers and the market.
[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A lithium slag-based gelling material, characterized in that: By weight, it includes 30-55 parts of lithium slag, 0-20 parts of lithium mica ore dressing tailings, 20-40 parts of slag, 0-20 parts of fly ash, 1-5 parts of silica fume, 5-12 parts of alkali activator, 0.5-2 parts of water reducing agent, and 0.1-1 parts of organic admixture; Wherein, the alkaline activator is composed of 3-6 parts of hydroxide and 3-6 parts of silicate.
2. The cementitious material according to claim 1, characterized in that The silicate is any one of sodium silicate and potassium silicate.
3. The cementitious material according to claim 1, characterized in that The hydroxide is any one of calcium hydroxide and lithium hydroxide.
4. The cementitious material according to claim 1, characterized in that The water reducer is any one of a naphthalene-based water reducer, calcium lignin sulfonate, and a melamine water reducer.
5. The cementitious material according to claim 1, characterized in that: The organic admixture is selected from any one or more of polyethylene glycol, polyvinyl alcohol, chitosan and xanthan gum.
6. The cementitious material according to claim 1, characterized in that The particle size of the lithium slag and the lithium mica ore dressing tailings is 45-74 μm.
7. The cementitious material according to claim 1, characterized in that The particle size of the slag and fly ash is ≤35 μm.
8. The cementitious material according to claim 1, characterized in that The particle size of the silica fume is 1-6 μm.
9. The method for preparing the gelling material according to any one of claims 1 to 8, characterized in that: The steps include: Drying: Dry lithium slag, slag, tailings, fly ash and silica ash to ensure that the moisture content of each raw material is ≤1%; Ball milling: ball mill the dried lithium slag, slag, tailings and fly ash respectively; Screening: Screen the lithium slag, slag, tailings and fly ash after ball milling; Mixing: weigh the dried ball-milled and sieved lithium slag, slag, tailings, fly ash, silica fume, alkali activator, water reducing agent and organic admixture respectively according to weight proportions and mix them evenly to obtain a solid waste-alkali activator mixture; Stirring: mixing the solid waste-alkali activator mixture with water to obtain a slurry; Casting and molding: Pour the slurry into a 40×40×160mm triple steel mold, flatten the mold surface and cover it with plastic wrap; Curing: After casting, it is cured in a standard curing box for 23-24 hours before demoulding, and then cured at normal temperature and humidity to the age to obtain a lithium slag based alkali-activated cementitious material.
10. Use of the cementitious material according to any one of claims 1 to 8 as a building substrate.
Citation Information
Patent Citations
Chitosan modified geopolymer cementing material
CN106746788A
Environment-friendly high-crack-resistance plastering mortar and preparation method thereof
CN115466098A
Cited By
Acid-excited lithium slag-based cementing material and preparation method thereof
CN119683879A
High-doping-amount lithium slag-based geopolymer and preparation method thereof
CN120136467A
Composite activator based on lithium slag as well as preparation method and application of composite activator
CN120647233A
Comprehensive recovery method of lithium slag
CN120714773A