Cellulose nanocrystal solvent-free fluid, preparation method thereof and application of cellulose nanocrystal solvent-free fluid in adhesive

By grafting flexible oligomers on the surface of cellulose nanocrystals to form a solvent-free fluid, the problems of cellulose nanocrystal aggregation and hydrophilicity limitations in adhesives are solved, and the performance improvement and application expansion of epoxy adhesives are achieved.

CN118745250AActive Publication Date: 2024-10-08HARBIN INST OF TECH

Patent Information

Application Number
CN202410825263.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-08
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

The hydrophilicity and strong hydrogen bonding of cellulose nanocrystals lead to their agglomeration during processing, which limits their excellent performance as a filling phase in adhesives. Existing surface modification methods require the assistance of solvents, and in epoxy adhesives Field applications have not been reported.

Method used

Design a solvent-free fluid for cellulose nanocrystals. Flexible long-chain oligomers are grafted on the surface of cellulose nanocrystals to form a core-corona structure. Covalently bonded organosilanes and amino-terminated polyethers are used as the corona layer. , eliminate the amorphous area in cellulose, and prepare spherical, rod-shaped or needle-shaped nanocrystals without solvent assistance, giving it excellent fluidity and dispersion.

Benefits of technology

It achieves uniform dispersion and interfacial interaction of cellulose nanocrystals in epoxy adhesive, significantly improves the adhesive performance and toughness of the adhesive, solves the agglomeration problem, and broadens the application scope of cellulose nanocrystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745250A_ABST
    Figure CN118745250A_ABST
Patent Text Reader

Abstract

The invention provides a cellulose nanocrystal solvent-free fluid, a preparation method thereof and an application of the cellulose nanocrystal solvent-free fluid in an adhesive, the cellulose nanocrystal solvent-free fluid is of a core-canopy structure, a cellulose nanocrystal serves as a core, a flexible long-chain oligomer is grafted on the surface to serve as a canopy, and the cellulose nanocrystal is spherical, rod-shaped or needle-shaped. According to the cellulose nanocrystal solvent-free fluid prepared by the preparation method disclosed by the invention, the nanocrystal is converted from a solid phase to a liquid phase at room temperature, a novel bio-based nano functional material with excellent dispersion stability and room-temperature fluidity is obtained, and the cellulose nanocrystal solvent-free fluid is easily and uniformly dispersed in an epoxy resin matrix due to the excellent fluidity; the rigid core and the flexible canopy enable the spherical cellulose nanocrystal to be soft and hard at the same time, the spherical cellulose nanocrystal serving as a single modifier can reinforce and toughen epoxy resin, meanwhile, active amino in the oligomer canopy and epoxy groups in a matrix are subjected to a cross-linking reaction, the interface interaction between the spherical cellulose nanocrystal and the epoxy matrix is improved, and therefore the spherical cellulose nanocrystal has the good mechanical property. Therefore, the adhesive property of the epoxy glue is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer functional materials, and in particular relates to a cellulose nanocrystal solvent-free fluid, a preparation method thereof, and application thereof in an adhesive. Background Art

[0002] With the increasing depletion of non-renewable resources such as petroleum, making full use of natural polymer materials has become an inevitable trend. Cellulose nanocrystals are a new type of green and environmentally friendly material. They come from cellulose, the most abundant renewable resource in nature. Generally, the amorphous region (non-crystalline region) of cellulose is destroyed by acid hydrolysis to release the crystalline region, and obtain cellulose nanocrystals with smaller size and higher aspect ratio, which show significant advantages in applications in the fields of biomedicine and nanocomposites. Cellulose nanocrystals are composed of dehydrated glucose connected by β-1,4 glycosidic bonds, in which each repeated glucose unit contains three hydroxyl groups, making it extremely hydrophilic. This property will weaken the interfacial interaction with the polymer matrix and reduce the stress transfer efficiency from the reinforcing filler to the matrix. In addition, strong hydrogen bonds will cause cellulose nanocrystals to agglomerate during processing, which seriously restricts the excellent performance of cellulose nanocrystals when used as a filling phase.

[0003] At present, the main method to prevent this from happening is to modify the surface of cellulose nanocrystals and reduce the number of surface hydroxyl groups through silanization treatment, thereby improving the dispersibility in the polymer matrix. However, the surface-modified cellulose nanocrystals are solid powders on a macro scale, and still need the assistance of solvents when used as a filling phase. Solvent-free nanofluids are a new type of organic-inorganic hybrid material. As the name suggests, they can give solid nanoparticles good flowability in the absence of solvents. They are generally composed of core particles and a canopy. This core-shell structure can remain stable under physical disturbances, so the entire system is considered to be a single component and is macroscopically uniform. When it is mixed with a polymer matrix, it can effectively solve the problem of nanoparticle agglomeration. However, there are currently no reports on cellulose nanocrystal solvent-free fluids and their applications in the field of epoxy adhesives. Summary of the invention

[0004] In order to solve the above problems, the present invention proposes a cellulose nanocrystal solvent-free fluid, a preparation method thereof, and an application thereof in an adhesive.

[0005] The present invention firstly proposes a cellulose nanocrystal solvent-free fluid, which is a core-crown structure, with cellulose nanocrystals as cores and flexible long-chain oligomers grafted on the surface as a crown. The cellulose nanocrystals are spherical, rod-shaped or needle-shaped.

[0006] Furthermore, the flexible long-chain oligomer is bonded by an organic silane and an amino-terminated polyether through a covalent bond, and the organic silane is γ-glycidyloxypropyltrimethoxysilane or β-(3,4-epoxycyclohexane)ethyltrimethoxysilane.

[0007] Furthermore, the amino-terminated polyether is one of polyetheramine M-2070, polyetheramine M-1000 and polyetheramine D-2000.

[0008] Furthermore, the cellulose nanocrystals are spherical cellulose nanocrystals after eliminating the amorphous regions in the cellulose fibers, and have a diameter of 20 to 100 nm.

[0009] The method for preparing the above-mentioned cellulose nanocrystal solvent-free fluid comprises the following steps:

[0010] Step 1: Preparation of the flexible long-chain oligomer canopy

[0011] Dissolve equimolar amounts of organosilane and amino-terminated polyether in an alcohol solvent, respectively, and react at 30-60° C. for 12-24 hours with stirring to obtain an alcohol solution of an oligomer canopy;

[0012] Step 2: Preparation of solvent-free fluid of cellulose nanocrystals

[0013] The cellulose nanocrystals are dispersed in deionized water, and the cellulose nanocrystal dispersion is added to the alcohol solution of the oligomer canopy. Most of the solvent is removed after reacting at 35-50°C for 8-12 hours. The unreacted canopy material is dialyzed in deionized water and dried to obtain a cellulose nanocrystal solvent-free fluid.

[0014] Furthermore, the alcohol solvent in step 1 is methanol or ethanol.

[0015] Furthermore, the dialysis operation in step 2 uses a dialysis bag with a molecular weight of 3500 to 5000 Da.

[0016] Furthermore, the mass ratio of the cellulose nanocrystals to the oligomer canopy in step 2 is 1:10-30.

[0017] Further, the core of the cellulose nanocrystal solvent-free fluid is a spherical cellulose nanocrystal after eliminating the amorphous region in the cellulose. The method for eliminating the amorphous region in the cellulose is an ultrasonic-assisted acid hydrolysis method, specifically: treating the microcrystalline cellulose with an alkali solution, filtering, washing, and drying to obtain a white powder; treating the alkali-treated white powder with dimethyl sulfoxide, filtering, washing, and obtaining a slurry; adding the slurry to the acid hydrolysis solution, heating at 55 to 75°C and acid hydrolyzing for 8 to 10 hours under ultrasonic stirring; adding deionized water to terminate the reaction, removing the upper layer liquid, repeating the operation of adding deionized water and removing the upper layer liquid until the upper layer liquid is turbid, and dialyzing in deionized water until the pH is constant to obtain a spherical cellulose nanocrystal water dispersion. Further, the dialysis operation uses a dialysis bag with a molecular weight of 8000 to 14000Da.

[0018] Furthermore, the alkali solution is a sodium hydroxide aqueous solution with a concentration of 5 to 6 mol / L, and the ratio of microcrystalline cellulose to the alkali solution is 100 to 120 g:1L.

[0019] Furthermore, the ratio of microcrystalline cellulose to dimethyl sulfoxide is 100-120 g:1L.

[0020] Furthermore, the acid hydrolysis solution is a mixture of concentrated hydrochloric acid, concentrated sulfuric acid and deionized water in a ratio of 1-2:2-3:6-7; the ratio of the acid hydrolysis solution to microcrystalline cellulose is 20-30 mL / g.

[0021] The present invention further proposes the application of cellulose nanocrystal solvent-free fluid in adhesives. The cellulose nanocrystal solvent-free fluid is used as a raw material, and a cellulose nanocrystal solvent-free fluid modified epoxy adhesive is obtained by mixing the cellulose nanocrystal solvent-free fluid, epoxy resin and amine curing agent. The content of the cellulose nanocrystal solvent-free fluid in the adhesive is 0 to 1 wt.%.

[0022] Furthermore, the epoxy resin is bisphenol A type E51 epoxy resin.

[0023] Furthermore, the amine curing agent is one of triethylenetetramine, isophoronediamine and polyamide.

[0024] The principle of the present invention is as follows:

[0025] The nano-size effect and good mechanical properties of cellulose nanocrystals make them potential bio-based nanomaterials for polymer reinforcement, but the filler agglomeration and weakened interfacial interaction caused by hydrophilicity greatly limit their application in the field of epoxy adhesives. Therefore, a cellulose nanocrystal solvent-free fluid was prepared by grafting flexible long-chain oligomers on the surface of cellulose nanocrystals, which was used as a single modifier to achieve comprehensive improvement of epoxy adhesive performance.

[0026] Microcrystalline cellulose was pretreated with NaOH aqueous solution and DMSO to make the fiber surface rough and even crack, exposing the internal fiber filaments, which was conducive to the acid hydrolysis solution entering the amorphous region (non-crystalline region) of cellulose during subsequent acid hydrolysis. Then, the amorphous region (non-crystalline region) with poor acid resistance in cellulose was removed by ultrasonic-assisted acid hydrolysis, and the crystalline region was released to prepare spherical cellulose nanocrystals with small size and large specific surface area. Then, a covalent corona was prepared by the ring-opening reaction of organic silane and amino-terminated polyether, and the corona was grafted to the surface of the nanocrystal by the condensation reaction of hydroxyl and silanol on the surface of cellulose nanocrystal to prepare cellulose nanocrystal solvent-free fluid. The flexible oligomer corona was used as a flow medium to give cellulose nanocrystals excellent flow properties. The amorphous region (non-crystalline region) with poor acid resistance in cellulose was removed, and the crystalline region was released to prepare spherical cellulose nanocrystals with small size and large specific surface area, which further improved the grafting density of the oligomer corona and gave the cellulose nanocrystal solvent-free fluid better fluidity.

[0027] Good dispersibility and strong filler / matrix interfacial interaction are the key to improving the performance of nanoparticle-modified epoxy adhesives. Nanofluids have good fluidity at room temperature, which promotes their uniform dispersion in the epoxy matrix and avoids agglomeration. The active amine groups in the oligomer corona will also undergo cross-linking reactions with the epoxy groups in the epoxy matrix, greatly improving the interfacial interaction between cellulose nanocrystals and the epoxy matrix. In addition, cellulose nanocrystal solvent-free fluids have a special core-corona structure. Cellulose nanocrystals play a reinforcing role as rigid organic nanoparticles. The long-chain flexible oligomer corona not only increases the dispersibility of cellulose nanocrystals in the epoxy matrix, but also has a toughening effect. When cellulose nanocrystals are introduced into the epoxy system as a single-component functional nanofiller, they also play a reinforcing and toughening role, thereby further improving the performance of epoxy adhesives.

[0028] Beneficial effects:

[0029] 1. The flexible long-chain oligomers in the solvent-free fluid of cellulose nanocrystals prepared by the present invention are bonded by organic silane and terminal amino polyether through covalent bonds. Compared with ionic bonds, the amine groups exist in protonated form. When covalently bonded, the amine groups in the form of secondary amines can react during polymer modification. In addition, covalent bonds have relatively higher bond energy than ionic bonds, and the relatively stable structure has a positive effect on improving the thermal properties of polymer composites.

[0030] 2. The solvent-free cellulose nanocrystal fluid prepared by the present invention has excellent fluidity without the aid of solvent, solves the problem of easy agglomeration of cellulose nanocrystals, can maintain a fluid state at room temperature, and improves the processing performance of cellulose nanocrystals.

[0031] 3. The present invention uses cellulose nanocrystal solvent-free fluid as the functional filler of epoxy adhesive and shows a significant modification effect. The liquid-like behavior enables it to be evenly dispersed in the epoxy matrix. The active amine groups in the canopy can enhance the interfacial interaction between cellulose nanocrystals and the epoxy matrix, and can effectively improve the bonding performance of the adhesive at a low loading amount.

[0032] 4. The cellulose nanocrystal solvent-free fluid provided by the present invention has a special core-crown structure. When introduced into the epoxy system as a single-component functional nanofiller, it can simultaneously play a role in strengthening and toughening, thereby broadening the application range of cellulose nanocrystals. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the synthesis route of cellulose nanocrystal solvent-free fluid in Examples 1 and 2 of the present invention;

[0034] Figure 2 This is the SEM image of the spherical cellulose nanocrystals of Example 1;

[0035] Figure 3 The macroscopic physical picture of the cellulose nanocrystal solvent-free fluid in Examples 2, 3 and 4;

[0036] Figure 4 This is an infrared comparative analysis of the spherical cellulose nanocrystals of Example 1 and the spherical cellulose nanocrystals of Example 2 in solvent-free fluid;

[0037] Figure 5 This is the solvent-free fluid XPS structural analysis of spherical cellulose nanocrystals in Example 2;

[0038] Figure 6 is the DSC curve of the cellulose nanocrystal solvent-free fluid of Example 2;

[0039] Figure 7 This is the thermogravimetric curve of the solvent-free fluid of cellulose nanocrystals in Example 2;

[0040] Figure 8 It is a comparison chart of the bonding strength of the epoxy adhesives of Example 13, Example 14 and Comparative Example 1;

[0041] Fig. 9 It is a comparison chart of the bonding strength of the epoxy adhesives of Example 15, Example 16 and Comparative Example 2;

[0042] Fig.10 It is a comparison chart of the bonding strength of the epoxy adhesives of Example 17, Example 18 and Comparative Example 3;

[0043] Fig.11 This is a SEM photo of the cross section of the epoxy adhesive of Comparative Example 3;

[0044] Fig.12This is a SEM photograph of the cross-section of the cellulose nanocrystal solvent-free fluid modified epoxy adhesive in Example 18. DETAILED DESCRIPTION

[0045] The invention provides a cellulose nanocrystal solvent-free fluid, a preparation method thereof, and application thereof in an adhesive.

[0046] The present invention first proposes a cellulose nanocrystal solvent-free fluid, which is a core-crown structure, with cellulose nanocrystals as the core, and flexible long-chain oligomers grafted on the surface as the crown, and the cellulose nanocrystals are spherical, rod-shaped or needle-shaped. The flexible long-chain oligomers are covalently bonded by organic silane and terminal amino polyether, and the organic silane is γ-glycidyloxypropyltrimethoxysilane or β-(3,4-epoxycyclohexane)ethyltrimethoxysilane. The terminal amino polyether is one of polyetheramine M-2070, polyetheramine M-1000 and polyetheramine D-2000. Optionally, the cellulose nanocrystals are spherical cellulose nanocrystals after eliminating the amorphous region in the cellulose fiber, and the diameter is 20 to 100 nm.

[0047] The method for preparing the above-mentioned cellulose nanocrystal solvent-free fluid comprises the following steps:

[0048] Step 1: Preparation of the flexible long-chain oligomer canopy

[0049] Equimolar amounts of organosilane and amino-terminated polyether are dissolved in an alcohol solvent respectively, and stirred at 30-60° C. for 12-24 hours to obtain an alcohol solution of an oligomer canopy; the alcohol solvent is methanol or ethanol.

[0050] Step 2: Preparation of solvent-free fluid of cellulose nanocrystals

[0051] The cellulose nanocrystals are dispersed in deionized water, and the cellulose nanocrystal dispersion is added to the alcohol solution of the oligomer canopy. After reacting at 35-50°C for 8-12 hours, most of the solvent is removed, and the unreacted canopy material is dialyzed in deionized water, and the cellulose nanocrystal solvent-free fluid is obtained by drying. The molecular weight of the dialysis bag used in the dialysis operation is 3500-5000Da. The mass ratio of the cellulose nanocrystal to the oligomer canopy is 1:10-30.

[0052] When the core of the cellulose nanocrystal solvent-free fluid is a spherical cellulose nanocrystal after eliminating the amorphous region in cellulose, the method for eliminating the amorphous region in cellulose is an ultrasonic-assisted acid hydrolysis method, specifically: treating the microcrystalline cellulose with an alkali solution, filtering, washing and drying to obtain a white powder; treating the alkali-treated white powder with dimethyl sulfoxide, filtering and washing to obtain a slurry; adding the slurry to the acid hydrolysis solution, heating at 55 to 75°C and acid hydrolyzing for 8 to 10 hours under ultrasonic stirring; adding deionized water to terminate the reaction, removing the upper layer liquid, repeating the operation of adding deionized water and removing the upper layer liquid until the upper layer liquid is turbid, dialyzing in deionized water until the pH is constant, and obtaining a spherical cellulose nanocrystal water dispersion. Further, the dialysis operation uses a dialysis bag with a molecular weight of 8000 to 14000Da. The alkali solution is a sodium hydroxide aqueous solution with a concentration of 5 to 6 mol / L, and the ratio of microcrystalline cellulose to the alkali solution is 100 to 120 g:1L. The ratio of microcrystalline cellulose to dimethyl sulfoxide is 100 to 120 g:1L.

[0053] Furthermore, the acid hydrolysis solution is a mixture of concentrated hydrochloric acid, concentrated sulfuric acid and deionized water in a ratio of 1-2:2-3:6-7; the ratio of the acid hydrolysis solution to microcrystalline cellulose is 20-30 mL / g.

[0054] Example 1 is a specific example of the method for preparing spherical cellulose nanocrystals; Examples 2 to 9 are specific examples of preparing solvent-free fluids using pretreated spherical cellulose nanocrystals; and Examples 10 to 12 are specific examples of preparing solvent-free fluids using cellulose nanocrystals that have not been pretreated.

[0055] Embodiment 1:

[0056] Step 1: 3g of microcrystalline cellulose was treated with 25mL of 5mol / L sodium hydroxide solution at 80℃ for 3h under mechanical stirring, filtered and washed with water until pH=7, and dried at 40℃ for 24h to obtain a white powder. The alkali-treated powder was treated with 25mL of dimethyl sulfoxide at 80℃ for 3h under mechanical stirring, filtered and washed with water 3 times to obtain a slurry. The slurry was added to 78mL of acid hydrolysis solution (concentrated hydrochloric acid, concentrated sulfuric acid and deionized water were prepared in a ratio of 1:3:6), and acid hydrolyzed for 8h at 65℃ by mechanical stirring and ultrasonic treatment, and then deionized water was added to terminate the reaction. After centrifugation at 9000r / min for 10min, the supernatant was poured out, water was added for oscillation and centrifugation was repeated until the upper layer was turbid, and dialyzed in deionized water with a dialysis bag with a molecular weight of 10000Da until the pH was constant to obtain a spherical cellulose nanocrystal aqueous dispersion.

[0057] Embodiment 2:

[0058] Step 1: Add 7.5 mmol of γ-glycidyloxypropyltrimethoxysilane to 35.45 g of methanol, then add dropwise to a methanol solution of 7.5 mmol of polyetheramine M-2070 (150 g of methanol), and react at 50° C. with magnetic stirring for 12 h to obtain an alcohol solution of the oligomer corona.

[0059] Step 2: Add the aqueous dispersion containing 0.2 g of spherical cellulose nanocrystals obtained in Example 1 to the alcohol solution of the oligomer canopy, react at 35°C for 12 h, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 3500 Da, and dry to obtain a solvent-free fluid of spherical cellulose nanocrystals.

[0060] Embodiment 3:

[0061] Step 1: Add 10 mmol of γ-glycidyloxypropyltrimethoxysilane to 47.27 g of methanol, then add dropwise to a methanol solution of 10 mmol of polyetheramine M-2070 (200 g of methanol), and react with magnetic stirring at 50° C. for 12 h to obtain an alcohol solution of the oligomer corona.

[0062] Step 2: Add the aqueous dispersion containing 0.2 g of spherical cellulose nanocrystals obtained in Example 1 to the alcohol solution of the oligomer canopy, react at 35°C for 12 h, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 3500 Da, and dry to obtain a solvent-free fluid of spherical cellulose nanocrystals.

[0063] Embodiment 4:

[0064] Step 1: Add 12.5 mmol of γ-glycidyloxypropyltrimethoxysilane to 59.09 g of methanol, then add dropwise to a methanol solution of 12.5 mmol of polyetheramine M-2070 (250 g of methanol), and react with magnetic stirring at 50° C. for 12 h to obtain an alcohol solution of the oligomer corona.

[0065] Step 2: Add the aqueous dispersion containing 0.2 g of spherical cellulose nanocrystals obtained in Example 1 to the alcohol solution of the oligomer canopy, react at 35°C for 12 h, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 3500 Da, and dry to obtain a solvent-free fluid of spherical cellulose nanocrystals.

[0066] Embodiment 5:

[0067] Step 1: Add 12.5 mmol of γ-glycidyloxypropyltrimethoxysilane to 59.09 g of methanol, then add dropwise to a methanol solution of 12.5 mmol of polyetheramine M-2070 (250 g of methanol), and react with magnetic stirring at 30° C. for 12 h to obtain an alcohol solution of the oligomer corona.

[0068] Step 2: Add the aqueous dispersion containing 0.2 g of spherical cellulose nanocrystals obtained in Example 1 to the alcohol solution of the oligomer canopy, react at 35°C for 12 h, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 3500 Da, and dry to obtain a solvent-free fluid of spherical cellulose nanocrystals.

[0069] Embodiment 6:

[0070] Step 1: Add 12.5 mmol of β-(3,4-epoxycyclohexane)ethyltrimethoxysilane to 59.09 g of methanol, then add dropwise to a methanol solution of 12.5 mmol of polyetheramine M-2070 (250 g of methanol), and react with magnetic stirring at 40°C for 12 h to obtain an alcohol solution of the oligomer corona.

[0071] Step 2: Add the aqueous dispersion containing 0.2 g of spherical cellulose nanocrystals obtained in Example 1 to the alcohol solution of the oligomer canopy, react at 35°C for 12 h, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 3500 Da, and dry to obtain a solvent-free fluid of spherical cellulose nanocrystals.

[0072] Embodiment 7:

[0073] Step 1: Add 12.5 mmol of γ-glycidyloxypropyltrimethoxysilane to 59.09 g of methanol, then add dropwise to a methanol solution of 12.5 mmol of polyetheramine M-2070 (250 g of methanol), and react at 50° C. with magnetic stirring for 24 h to obtain an alcohol solution of the oligomer corona.

[0074] Step 2: Add the aqueous dispersion containing 0.2 g of spherical cellulose nanocrystals obtained in Example 1 to the alcohol solution of the oligomer canopy, react at 35°C for 12 h, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 3500 Da, and dry to obtain a solvent-free fluid of spherical cellulose nanocrystals.

[0075] Embodiment 8:

[0076] Step 1: Add 12.5 mmol of γ-glycidyloxypropyltrimethoxysilane to 59.09 g of methanol, then add dropwise to a methanol solution of 12.5 mmol of polyetheramine M-1000 (250 g of methanol), and react at 60° C. with magnetic stirring for 24 h to obtain an alcohol solution of the oligomer corona.

[0077] Step 2: Add the aqueous dispersion containing 0.2 g of spherical cellulose nanocrystals obtained in Example 1 to the alcohol solution of the oligomer canopy, react at 35°C for 12 h, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 3500 Da, and dry to obtain a solvent-free fluid of spherical cellulose nanocrystals.

[0078] Embodiment 9:

[0079] Step 1: Add 12.5 mmol of γ-glycidyloxypropyltrimethoxysilane to 59.09 g of methanol, then add dropwise to a methanol solution of 12.5 mmol of polyetheramine D-2000 (250 g of methanol), and react at 60° C. with magnetic stirring for 24 h to obtain an alcohol solution of the oligomer corona.

[0080] Step 2: Add the aqueous dispersion containing 0.2 g of spherical cellulose nanocrystals obtained in Example 1 to the alcohol solution of the oligomer canopy, react at 35°C for 8 hours, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 4000Da, and dry to obtain a solvent-free fluid of spherical cellulose nanocrystals.

[0081] Embodiment 10:

[0082] Step 1: Add 12.5 mmol of γ-glycidyloxypropyltrimethoxysilane to 59.09 g of methanol, then add dropwise to a methanol solution of 12.5 mmol of polyetheramine M-2070 (250 g of methanol), and react at 60° C. with magnetic stirring for 24 h to obtain an alcohol solution of the oligomer corona.

[0083] Step 2: Add an aqueous dispersion containing 0.2 g of rod-shaped cellulose nanocrystals to an alcohol solution of the oligomer canopy, react at 45°C for 9 h, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 5000 Da, and dry to obtain a rod-shaped cellulose nanocrystal solvent-free fluid.

[0084] Embodiment 11:

[0085] Step 1: Add 12.5 mmol of γ-glycidyloxypropyltrimethoxysilane to 59.09 g of methanol, then add dropwise to a methanol solution of 12.5 mmol of polyetheramine M-1000 (250 g of methanol), and react at 60° C. with magnetic stirring for 24 h to obtain an alcohol solution of the oligomer corona.

[0086] Step 2: Add an aqueous dispersion containing 0.2 g of rod-shaped cellulose nanocrystals to an alcohol solution of the oligomer canopy, react at 50°C for 10 h, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 3500 Da, and dry to obtain a rod-shaped cellulose nanocrystal solvent-free fluid.

[0087] Embodiment 12:

[0088] Step 1: Add 12.5 mmol of γ-glycidyloxypropyltrimethoxysilane to 59.09 g of methanol, then add dropwise to a methanol solution of 12.5 mmol of polyetheramine D-2000 (250 g of methanol), and react at 60° C. with magnetic stirring for 24 h to obtain an alcohol solution of the oligomer corona.

[0089] Step 2: Add an aqueous dispersion containing 0.2 g of needle-shaped cellulose nanocrystals to an alcohol solution of the oligomer canopy, react at 50°C for 11 h, remove most of the solvent, remove unreacted canopy material in deionized water using a dialysis bag with a molecular weight of 3500 Da, and dry to obtain a needle-shaped cellulose nanocrystal solvent-free fluid.

[0090] The present invention also proposes the application of the cellulose nanocrystal solvent-free fluid prepared by the above method in the field of epoxy adhesives, comprising the following steps:

[0091] The cellulose nanocrystal solvent-free fluid is used as a raw material, and a cellulose nanocrystal solvent-free fluid, an epoxy resin and an amine curing agent are mixed to obtain a cellulose nanocrystal solvent-free fluid modified epoxy adhesive, wherein the content of the cellulose nanocrystal solvent-free fluid in the adhesive is 0-1wt.%. The epoxy resin is bisphenol A type E51 epoxy resin. The amine curing agent is one of triethylenetetramine, isophorone diamine and polyamide.

[0092] Examples 13 to 18 are application examples of cellulose nanocrystal solvent-free fluid in epoxy adhesives.

[0093] Embodiment 13:

[0094] The solvent-free cellulose nanocrystal fluid obtained in Example 2 was added to 10 g of epoxy resin E51 and 1.24 g of triethylenetetramine, with the added amount controlled to be 0.5 wt.%, and after stirring and mixing evenly, vacuuming to remove bubbles to obtain an epoxy adhesive.

[0095] Embodiment 14:

[0096] The cellulose nanocrystal solvent-free fluid obtained in Example 2 was added to 10 g of epoxy resin E51 and 1.24 g of triethylenetetramine, with the added amount controlled to be 1 wt.%, and after stirring and mixing evenly, the mixture was vacuumed to remove bubbles, thereby obtaining an epoxy adhesive.

[0097] Embodiment 15:

[0098] The cellulose nanocrystal solvent-free fluid obtained in Example 2 was added to 10 g of epoxy resin E51 and 2.17 g of isophorone diamine, with the added amount controlled to be 0.5 wt.%, and after stirring and mixing evenly, the air bubbles were removed by vacuum to obtain an epoxy adhesive.

[0099] Embodiment 16:

[0100] The solvent-free cellulose nanocrystal fluid obtained in Example 2 was added to 10 g of epoxy resin E51 and 2.17 g of isophorone diamine, with the added amount controlled to be 1 wt.%, and after stirring and mixing evenly, the air bubbles were removed by vacuum to obtain an epoxy adhesive.

[0101] Embodiment 17:

[0102] The cellulose nanocrystal solvent-free fluid obtained in Example 2 was added to 10 g of epoxy resin E51 and 5 g of polyamide, with the added amount controlled to be 0.5 wt.%, and after stirring and mixing evenly, the mixture was vacuumed to remove bubbles, thereby obtaining an epoxy adhesive.

[0103] Embodiment 18:

[0104] The cellulose nanocrystal solvent-free fluid obtained in Example 2 was added to 10 g of epoxy resin E51 and 5 g of polyamide, with the added amount being controlled to be 1 wt.%, and after stirring and mixing evenly, the mixture was vacuumed to remove bubbles, thereby obtaining an epoxy adhesive.

[0105] Comparative Example 1: 10 g of epoxy resin E51 and 1.24 g of triethylenetetramine were compounded to obtain an epoxy adhesive.

[0106] Comparative Example 2: 10 g of epoxy resin E51 and 2.17 g of isophorone diamine were compounded to obtain an epoxy adhesive.

[0107] Comparative Example 3: 10 g of epoxy resin E51 and 5 g of polyamide were compounded to obtain an epoxy adhesive.

[0108] Analysis and testing

[0109] Figure 1 The schematic diagram of the synthesis route of cellulose nanocrystal solvent-free fluid in Examples 1 and 2 of the present invention is as follows: Figure 1 It can be seen that the microcrystalline cellulose is subjected to swelling treatment and ultrasonic-assisted acid hydrolysis in step 1 to remove the surface amorphous area, thereby obtaining spherical cellulose nanocrystals. In step 2, the organosilane and the amino-terminated polyether generate a flexible long-chain oligomer corona through the ring-opening reaction of the amine group and the epoxy group. In step 3, the oligomer corona undergoes a dehydration condensation reaction with the hydroxyl group on the surface of the cellulose nanocrystal, and is grafted on the surface of the cellulose nanocrystal through covalent action, giving it excellent fluidity.

[0110] Figures 2 to 7 These are the test results related to Examples 1 to 4.

[0111] Figure 2 This is the SEM image of the spherical cellulose nanocrystals of Example 1. It can be seen that the appearance of all cellulose nanocrystals is approximately spherical, and the size distribution is concentrated below 100 nm, indicating that the target product spherical cellulose nanocrystals have been successfully prepared.

[0112] Figure 3 This is a macroscopic picture of the cellulose nanocrystal solvent-free fluid in Examples 2, 3 and 4. It can be seen that after being placed vertically on a glass plate, the three products all exhibit excellent flow properties, and with the increase of the flexible oligomer canopy content, the fluidity of the product is better, which preliminarily indicates the successful synthesis of the cellulose nanocrystal solvent-free fluid.

[0113] Figure 4 This is the infrared comparative analysis of the spherical cellulose nanocrystals of Example 1 and the spherical cellulose nanocrystals of Example 2 without solvent. It can be seen that at 1100 cm -1 and 845cm -1 The absorption peaks at are caused by Si-O-Si and O-Si-O, indicating that the flexible cap layer is successfully grafted on the surface of cellulose nanocrystals.

[0114] Figure 5 This is the XPS structural analysis of the spherical cellulose nanocrystal solvent-free fluid of Example 2. The chemical composition of the product was further analyzed. Four elements, namely oxygen, nitrogen, carbon and silicon, were present in the cellulose nanocrystal solvent-free fluid. The C1s fine spectrum showed significant CO bonds, CC bonds, C-Si bonds and CN bonds, representing cellulose nanocrystals and flexible oligomer coronas, indicating the successful synthesis of the cellulose nanocrystal solvent-free fluid.

[0115] Figure 6 This is the DSC curve of the solvent-free fluid of cellulose nanocrystals in Example 2. It can be clearly seen that there is a melting peak at 3°C, indicating that the product exhibits a liquid-like state at room temperature.

[0116] Figure 7 This is the thermogravimetric curve of the cellulose nanocrystal solvent-free fluid of Example 2. At 200°C, the product has no significant weight loss and there is no solvent in the system, which proves that the fluidity of the cellulose nanocrystal solvent-free fluid is inherent.

[0117] Figures 8 to 12 This is an analysis and test of the adhesive properties and toughening mechanism of the cellulose nanocrystal solvent-free fluid modified epoxy adhesive of Examples 13 to 18.

[0118] Figure 8 This is a comparison chart of the bonding strength of the epoxy adhesives of Example 13, Example 14 and Comparative Example 1, which are 5.30 MPa, 4.94 MPa and 4.29 MPa, respectively.

[0119] Fig. 9 This is a comparison chart of the bonding strength of the epoxy adhesives of Example 15, Example 16 and Comparative Example 2, which are 12.52 MPa, 11.36 MPa and 9.88 MPa, respectively.

[0120] Fig.10 The bonding strength comparison chart of the epoxy adhesives of Example 17, Example 18 and Comparative Example 3 is 12.62 MPa, 14.70 MPa and 10.86 MPa respectively, indicating that the cellulose nanocrystal solvent-free fluid has a significant reinforcing effect on the epoxy adhesive, greatly improving the bonding strength of the epoxy adhesive.

[0121] Fig.11 This is a SEM photograph of the cross section of the epoxy adhesive in comparative example 3. The cross section of the pure epoxy adhesive exhibits typical brittle fracture, the cross section is very smooth, and river-like cracks appear.

[0122] Fig.12 This is a SEM photo of the cross section of the epoxy adhesive modified by the cellulose nanocrystal solvent-free fluid in Example 18. It can be seen that the cross section of the modified epoxy adhesive is very rough, and due to the crack deflection effect of the cellulose nanocrystal solvent-free fluid, the adhesive absorbs more energy to produce crisscross cracks. This proves that the uniform dispersion of the spherical cellulose nanocrystal solvent-free fluid and the enhanced interfacial interaction with the epoxy matrix effectively improve the transmission of the destructive load when the adhesive is subjected to force.

Claims

1. A cellulose nanocrystal solvent-free fluid, characterized in that: The core-crown structure is a cellulose nanocrystal as the core, and a flexible long-chain oligomer is grafted on the surface as a crown. The cellulose nanocrystal is spherical, rod-shaped or needle-shaped.

2. The cellulose nanocrystal solvent-free fluid according to claim 1, characterized in that: The flexible long-chain oligomer is bonded by organic silane and amino-terminated polyether through covalent bonds, and the organic silane is γ-glycidyloxypropyltrimethoxysilane or β-(3,4-epoxycyclohexane)ethyltrimethoxysilane.

3. The cellulose nanocrystal solvent-free fluid according to claim 2, characterized in that: The amino-terminated polyether is one of polyetheramine M-2070, polyetheramine M-1000 and polyetheramine D-2000.

4. The cellulose nanocrystal solvent-free fluid according to claim 1, characterized in that: The cellulose nanocrystals are spherical cellulose nanocrystals obtained by eliminating the amorphous regions in the cellulose fibers, and have a diameter of 20 to 100 nm.

5. The method for preparing a cellulose nanocrystal solvent-free fluid according to any one of claims 1 to 3, characterized in that: The steps include: Step 1: Preparation of the flexible long-chain oligomer canopy Dissolve equimolar amounts of organosilane and amino-terminated polyether in an alcohol solvent, respectively, and react at 30-60° C. with stirring for 12-24 hours to obtain an alcohol solution of an oligomer canopy; Step 2: Preparation of solvent-free fluid of cellulose nanocrystals The cellulose nanocrystals are dispersed in deionized water, and the cellulose nanocrystal dispersion is added to the alcohol solution of the oligomer canopy. Most of the solvent is removed after reacting at 35-50°C for 8-12 hours. The unreacted canopy material is dialyzed in deionized water and dried to obtain a cellulose nanocrystal solvent-free fluid.

6. The method for preparing a cellulose nanocrystal solvent-free fluid according to claim 5, characterized in that: The core is a spherical cellulose nanocrystal after the amorphous region in the cellulose is eliminated. The method for eliminating the amorphous region in the cellulose is an ultrasonic-assisted acid hydrolysis method, specifically: treating the microcrystalline cellulose with an alkali solution, filtering, washing, and drying to obtain a white powder; treating the alkali-treated white powder with dimethyl sulfoxide, filtering, washing, and obtaining a slurry; adding the slurry to the acid hydrolysis solution, heating at 55 to 75° C. and acid hydrolyzing for 8 to 10 hours under ultrasonic stirring; adding deionized water to terminate the reaction, removing the upper liquid, repeating the operation of adding deionized water and removing the upper liquid until the upper liquid becomes turbid, and dialyzing in deionized water until the pH is constant to obtain an aqueous dispersion of spherical cellulose nanocrystals.

7. The method for preparing a cellulose nanocrystal solvent-free fluid according to claim 5, characterized in that: The mass ratio of the cellulose nanocrystals to the oligomer canopy in step 2 is 1:10 to 30.

8. The method for preparing a cellulose nanocrystal solvent-free fluid according to claim 6, characterized in that: The acid hydrolysis solution is a mixture of concentrated hydrochloric acid, concentrated sulfuric acid and deionized water in a ratio of 1-2:2-3:6-7; the ratio of the acid hydrolysis solution to microcrystalline cellulose is 20-30 mL / g.

9. The method for preparing a cellulose nanocrystal solvent-free fluid according to claim 5, characterized in that: The alcohol solvent in step 1 is methanol or ethanol.

10. Application of cellulose nanocrystal solvent-free fluid in adhesive, characterized in that: The cellulose nanocrystal solvent-free fluid according to any one of claims 1 to 4 is used as a raw material, and a cellulose nanocrystal solvent-free fluid modified epoxy adhesive is obtained by mixing the cellulose nanocrystal solvent-free fluid, epoxy resin and amine curing agent, wherein the content of the cellulose nanocrystal solvent-free fluid in the adhesive is 0-1wt.%.

Citation Information

Patent Citations

  • Preparation method of composite material with fiber surface coated with cellulose nano crystals and used for multi-scale enhancement

    CN105131529A

  • Solvent-free nano-cellulose fluid and preparation method thereof

    CN110003919A

Cited By

  • Method for forming petal-shaped nano particles with high dispersibility in situ and application of petal-shaped nano particles

    CN116874824A