Preparation method and application of PCL / CS-ZnO composite film
Through the preparation of PCL/CS-ZnO composite film, the problems of difficult biodegradation and poor antibacterial effect of food packaging materials are solved, long-term antibacterial effect on microorganisms is achieved and the shelf life of food is extended, providing a degradable and environmentally friendly packaging Material.
Patent Information
- Application Number
- CN202410830558.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-08
AI Technical Summary
Existing food packaging materials are difficult to biodegrade, causing environmental pollution, and traditional antibacterial agents are inconvenient to use, making it difficult to effectively extend the shelf life of food.
Using the preparation method of PCL/CS-ZnO composite film, ultrasonically dispersed ZnO nanoparticles are mixed with PCL and CS solutions, and the casting method is used to prepare a composite film with good compatibility, flexibility and hydrophobicity for food packaging.
It achieves long-term antibacterial effects on microorganisms, extends the shelf life of food, and provides a degradable, environmentally friendly bio-based polymer packaging material to replace traditional plastics.
Smart Images

Figure CN118745260A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite film preparation, and in particular to a preparation method of a PCL / CS-ZnO composite film and application thereof. Background Art
[0002] Polymers used in food packaging widely rely on non-biodegradable petroleum-based products, such as polypropylene (PP), polyethylene (PE), polyvinyl chloride (PVC), etc. These polymers have the advantages of low cost, light density, and corrosion resistance. However, these products are difficult to decompose in the natural environment and will continue to exist in our ecosystem, causing serious environmental problems. Therefore, people began to look for new green and environmentally friendly materials to replace traditional plastics. The preparation of degradable bio-based polymer (BP) packaging materials has become the focus of research in various countries and has received great attention in recent decades.
[0003] Polycaprolactone (PCL) (CAS No. 24980-41-4) is prepared by ring-opening polymerization of ε-caprolactone and has a structure of [CH2-(CH2)4-COO] nPCL is a thermoplastic polyester, a chemically synthesized biodegradable polymer material and medical material. n is approximately between 100 and 1000. It is a colorless crystalline solid with a low molecular weight and looks like wax. The glass transition temperature (Tg) is minus 60°C, the melting temperature is 63°C, and it begins to decompose at 250°C. PCL has good compatibility with a variety of polymers, strong adhesion to a variety of materials, and excellent thermal stability, hydrolysis stability and low-temperature properties. In recent years, with the strengthening of people's awareness of environmental protection, biodegradable materials have become a very active research direction in materials science. PCL is very similar to general plastics in many physical properties, and has good compatibility with many polymers. Therefore, it has great potential application value in the field of biodegradable materials. The presence of ester groups makes PCL biocompatible. In vivo and in vitro degradation tests of PCL homopolymers show that PCL degradation goes through at least two distinct processes: the first stage is the random hydrolysis of the ester groups catalyzed by the carboxyl end groups on the PCL chain, which is a non-enzymatic process. During this stage, the molecular weight and chemical structure of PCL change, but the weight loss is not obvious. When the molecular weight drops to 5000, the second stage begins, the chain cleavage rate slows down, but the oligomers diffuse away from the PCL body, so a significant weight loss can be observed. Since the PCL molecular chain is relatively regular and flexible, with strong crystallinity, the presence of five methylene groups makes PCL less hydrophilic, which is not conducive to the occurrence of main chain ester hydrolysis reaction, so the degradation rate is much slower than polyglycolic acid (PGA) and polylactic acid (PLA).
[0004] Chitosan (CS) is a deacetylated derivative of chitin. It is widely used in food packaging and other fields because of its wide source, non-toxicity, good biodegradability and easy film formation. Studies have shown that the introduction of plasticizers and other biopolymers (such as chitosan, CS) blended with PCL is a preferred method, which has biodegradability, improved stiffness and glass transition temperature (T g) and other mechanical properties, reduced water vapor permeability and oxygen permeability (OP). Sarasam et al. studied the effect of mixing CS with PCL on its biomechanical properties. Homogeneous blends of 25%, 50% and 75% PCL were formed by dissolving CS and 80kD PCL in a common solvent of about 77% acetic acid aqueous solution. Taking advantage of the low melting point of PCL, the blended films were processed into thin films in a water bath or oven. Compared with CS, the 50:50 mixture showed significantly improved mechanical properties and support for cell activity when processed in an oven. MA et al. prepared blended films by casting water-soluble hydroxyethyl acrylic acid-chitosan (HEA-CS) and polyvinyl alcohol (PVA) solutions. Water swelling performance analysis showed that HEA-CS in the blend promoted water absorption due to its porous structure and retained the antibacterial ability of the blended film. In summary, the compounding of PCL with CS not only retains the biodegradable properties of the material, but also has excellent mechanical properties and good thermal stability of the composite material.
[0005] In addition, the addition of nanoparticles (NPs) to BP packaging materials not only enhances mechanical properties but also improves the antimicrobial activity of polymers in food packaging. Films as carriers of antimicrobial agents allow the active substances to be gradually released to the surface of the product, where they can effectively function for a longer period of time. The use of active films reduces the disadvantages of applying antimicrobial agents directly to food by spraying or dipping, thereby improving the antimicrobial effect. Therefore, the use of active films in food packaging is a good choice to extend the shelf life of food.
[0006] Nano-zinc oxide (ZnO-NPs) has a huge specific surface area, excellent thermal conductivity, low thermal expansion coefficient, and outstanding mechanical properties. The incorporation of ZnO NPs into PCL produces antimicrobial activity, thereby extending the shelf life of food. For example, PCL / ZnONPs exhibit antimicrobial activity against pathogenic bacteria such as Escherichia coli and Staphylococcus aureus. Moreover, the addition of ZnO positively affects the barrier properties and hydrophilicity of the polymer blend coating. In addition, the addition of ZnO can improve the tensile strength and Young's elastic modulus of PCL and increase its maximum decomposition temperature.
[0007] Based on the above, the present invention proposes a method for preparing a PCL / CS-ZnO composite film and its application to prepare a green and environmentally friendly new degradable bio-based polymer (BP) packaging material. Summary of the invention
[0008] The purpose of the present invention is to solve the shortcomings of the prior art, and to propose a method for preparing a PCL / CS-ZnO composite film and its application. The composite film prepared by this technology has good compatibility, flexibility and hydrophobicity, has long-lasting antibacterial effect on microorganisms, and has advantages and feasibility in food packaging and replacing conventional polymers.
[0009] To achieve the above object, the present invention adopts the following technical solution.
[0010] A method for preparing a PCL / CS-ZnO composite film comprises the following steps:
[0011] ① Take a certain amount of ZnO nanoparticles and disperse them in a co-solvent, and perform ultrasonic dispersion treatment for 30 minutes to obtain a ZnO nanoparticle dispersion system;
[0012] ② Take a certain amount of PCL particles and dissolve them in the ZnO nanoparticle dispersion system, stir for 4 hours and then ultrasonicate for 30 minutes to obtain solution A;
[0013] ③ Take a certain amount of CS and dissolve it in 80% co-solvent, stir it thoroughly to obtain CS solution;
[0014] ④ Add CS solution dropwise into solution A, stir, sonicate and degas again;
[0015] ⑤Then stir at about 50℃ until it becomes a viscous gel mixture;
[0016] ⑥ Cast the gel-like mixture on a tempered glass plate, apply a uniform film with a coating machine, and then move the glass plate into a constant temperature ventilation chamber, control the evaporation rate of the solvent by adjusting the wind speed, and obtain a PCL / CS-ZnO composite film.
[0017] As a further description of the above technical solution: the mass ratio of PCL to CS in the PCL / CS-ZnO composite film is one of 9:1, 8:2, 7:3, 6:4, 1:1, 1:2, 1:3, 1:4, 1:5 or 1:6.
[0018] As a further description of the above technical solution: the co-solvent is glacial acetic acid or glacial acetic acid / water.
[0019] As a further description of the above technical solution: the mass ratio of the PCL particles to the ZnO nanoparticle dispersion system is 1:8, and the mass ratio of the CS to the co-solvent is 1:40.
[0020] As a further description of the above technical solution: the CS solution is added dropwise to solution A to make the ZnO NPs content be 1.0 wt%, 2.0 wt%, 3.0 wt% and or 4.0 wt% of the sum of the mass of PCL and CS.
[0021] As a further description of the above technical solution: the average thickness of the PCL / CS-ZnO composite film is about 0.15 to 0.20 mm.
[0022] An application of a PCL / CS-ZnO composite film, wherein the PCL / CS-ZnO composite film is applied in food packaging.
[0023] Compared with the prior art, the advantages of the present invention are:
[0024] In this scheme, degradable bio-based plastics PCL and CS are used as raw materials, and ZnO-NPs are added to prepare PCL / CS-ZnO composite films by solvent casting. The PCL / CS-ZnO composite films have good compatibility, flexibility and hydrophobicity, and have long-lasting antibacterial effects on microorganisms. They have advantages and feasibility in food packaging and in replacing conventional polymers, providing a scientific basis and theoretical support for the preparation of biocomposite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The ratio of PCL to CS and the phase separation in the embodiment of the present invention;
[0026] Figure 2 This is a graph showing the effect of film composition on water absorption in an experimental example of the present invention;
[0027] Figure 3 This is a graph showing the effect of ZnO content on water absorption in an experimental example of the present invention;
[0028] Figure 4 FTIR spectrum of the PCL-CS / ZnO composite film in the experimental example of the present invention;
[0029] Figure 5 It is the antibacterial activity diagram of the PCL / CS-ZnO composite film in the experimental example of the present invention;
[0030] Figure 6 It is the dispersion and agglomeration diagram of ZnO NPs in the PCL-CS composite film in the experimental example of the present invention;
[0031] Figure 7 This is a diagram showing the antibacterial effect of the PCL-CS composite membrane (3 wt% ZnO) in different time periods in the experimental example of the present invention. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments, and all other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making creative work are within the scope of protection of the present invention.
[0033] Embodiment 1
[0034] The preparation method of PCL / CS composite membrane comprises the following steps:
[0035] Take an appropriate amount of PCL and dissolve it in glacial acetic acid (m:v=1:8), take an appropriate amount of CS and dissolve it in 80% glacial acetic acid (m:v=1:40), and stir them thoroughly. The two solutions were mixed in different proportions, and the PCL mass ratio ranged from 10.0 to 90.0wt%. Then stir at about 50°C until it becomes a viscous gel. Each gel-like mixture was cast on a tempered glass plate and evenly coated with a coating machine (the limit height was 1.00mm). Then the glass plate was moved into a constant temperature ventilation chamber, and the evaporation rate of the solvent was controlled by adjusting the wind speed. The average thickness of the uniform film obtained was about 0.15 to 0.20mm. The mass ratios of PCL to CS in the prepared blended films were 9:1, 8:2, 7:3, 6:4, 1:1, 1:2, 1:3, 1:4, 1:5 and 1:6, respectively. Pure PCL or CS films were prepared in the same way as controls.
[0036] The properties of the blended membranes were determined, and the ratio with better membrane performance was selected. ZnO NPs were incorporated into the PCL matrix as a filler and activator to prepare PCL-CS / ZnO composite membranes.
[0037] The study found that the PCL solution prepared by using glacial acetic acid or 80% glacial acetic acid / water as the co-solvent can be well mixed with the CS solution. If the concentration of the solvent is significantly lower than this value, the PCL or CS component may precipitate from the mixture during the blending process. Figure 1 It can be seen that there are three situations on the surface of the composite membrane: one is that when the CS ratio is 20% to 30%, the membrane surface is honeycomb-shaped. When PCL:CS is between 6:4 and 1:3, the surface of the membrane is convex. When PCL:CS is less than 9:1 or greater than 1:4, the surface of the membrane is relatively flat. The honeycomb area is the membrane produced by CS, and the flat area is the PCL phase. On the contrary, the protruding area on the surface of the membrane is the PCL phase, and the flat area is the CS membrane. Some other researchers have also obtained similar morphological results. The phase separation phenomenon of the composite membrane is the result of the combined action of the hydrophilic CS phase and the hydrophobic PCL phase. That is, there is a certain interaction between PCL and CS, but the compatibility between the components in the blended membrane is very limited.
[0038] Embodiment 2
[0039] Based on the above embodiment, a method for preparing a PCL / CS-ZnO composite film comprises the following steps:
[0040] ① Take a certain amount of ZnO nanoparticles and disperse them in a co-solvent, and perform ultrasonic dispersion treatment for 30 minutes to obtain a ZnO nanoparticle dispersion system;
[0041] ② Take a certain amount of PCL particles and dissolve them in the ZnO nanoparticle dispersion system (m:v=1:8), stir for 4 hours and then ultrasonicate for 30 minutes to obtain solution A;
[0042] ③ Take a certain amount of CS and dissolve it in 80% co-solvent (m:v=1:40), stir it thoroughly to obtain a CS solution; wherein the co-solvent is glacial acetic acid or glacial acetic acid / water;
[0043] ④ Add the CS solution dropwise into solution A to make the ZnO NPs content 1.0wt%, 2.0wt%, 3.0wt% and or 4.0wt% of the total mass of PCL and CS, and stir, sonicate and degas again;
[0044] ⑤Then stir at about 50℃ until it becomes a viscous gel mixture;
[0045] ⑥ Cast the gel-like mixture on a tempered glass plate, apply a uniform coating with a coating machine (limit height is 1.00 mm), then move the glass plate into a constant temperature ventilation chamber, and adjust the wind speed to control the evaporation rate of the solvent to obtain a PCL / CS-ZnO composite film. The mass ratio of PCL to CS in the prepared PCL / CS-ZnO composite film is 9:1. The average thickness of the PCL / CS-ZnO composite film is about 0.15-0.20 mm.
[0046] Experimental example: Performance analysis of composite membranes
[0047] Experimental Example 3: Mechanical properties of PCL / CS composite membrane
[0048] Mechanical properties are one of the important properties of edible films, among which rigidity, Young's modulus and elongation at break are very important parameters of packaging materials. Rigidity is the ability to resist deformation, and Young's modulus is a physical quantity that describes the ability of solid materials to resist deformation. A large Young's modulus indicates that the deformation of the material is small when the material is compressed or stretched. Elongation at break is related to the tensile strength of the film when it breaks, which makes the film soft. Therefore, rigidity, Young's modulus and elongation at break are selected as evaluation indicators to optimize the process conditions of CS composite film. Each film is cut into a film of 80mm×30mm in size, and the "Plastic Bending Performance Test Method" (GB / T9341-2000) is used to evaluate the mechanical properties of the prepared film. The film is measured using a static mechanical tester to measure the mechanical properties of the composite film. The ambient temperature is 20℃ and the relative humidity is 50%. The initial distance between the moving and fixed clamps is 40mm, and the stretching rate is 10mm / min. The instrument can obtain the Young's modulus and elongation at break of the composite film according to the film thickness. For all samples, the arithmetic mean of three groups of parallel test values was taken as the final result.
[0049]
[0050] Wherein: EB is the elongation at break / %; L0 is the initial length of the film / mm; L1 is the length of the film when it breaks / mm.
[0051] The stiffness, Young's modulus and elongation at break of each film sample are shown in Table 1. As can be seen from the table, with the increase of CS content, the film stiffness increases from 3351N / m to 15257N / m; the Young's modulus increases from 27.6MPa to 91.3MPa; however, the elongation at break of the composite film is reduced to about 9.6% of the PCL film. Stiffness is a macroscopic property of a substance, which measures the ability of the film to resist elastic deformation. The Young's modulus is a measure of the size of the object's ability to resist elastic deformation. From a microscopic perspective, it is a reflection of the bond strength between atoms, ions or molecules. Any factor that affects the bond strength can affect the elastic modulus of the material, such as bonding method, crystal structure, chemical composition, microstructure, temperature, etc. PCL has high crystallinity and low melting point, Tg is -60℃, is very soft, and has great stretchability. CS macromolecules contain a large number of ring structures, and the -OH and -NH2 on the ring can form intermolecular hydrogen bonds, which hinder the rotation and movement of the molecular chain. Therefore, as the PCL content decreases, the flexibility of the PCL / CS membrane becomes worse, the brittleness increases, and the mechanical strength increases.
[0052] Table 1 Mechanical properties of PCL / CS composite membranes
[0053]
[0054] Experimental Example 4: Water absorption of PCL / CS composite membrane
[0055] In the field of food packaging, in addition to being transparent, safe and environmentally friendly, and meeting the requirements of food shelf life, the ideal packaging film should also have low swelling, water absorption and wettability. If the water vapor permeability of the film is high, the water absorption is strong, and it swells as the amount of water absorbed gradually increases, its gas barrier and moisture barrier properties will drop sharply. In addition, the mechanical strength of the film and the stability of the packaging size will also be affected by its water absorption and swelling. Therefore, it is necessary to analyze the water absorption rate of the film. Weigh a certain mass of the composite film and dry it in a dryer (0% relative humidity) for 7 days. After taking it out, place it in a container with a relative humidity of 100%. Fully absorb water until the mass is constant.
[0056] The water absorption of the membrane was calculated by the following formula:
[0057] Where m0 and m1 are the membrane masses g before and after water absorption, respectively.
[0058] Figure 2The figure shows the water absorption rate of the PCL / CS composite membrane in 100% humidity. As can be seen from the figure, the water absorption capacity of the composite membrane increases with the increase of CS content in the membrane. When the CS content is greater than 20%, the increase in water absorption rate slows down. This is related to the fact that CS contains more water-absorbing groups such as -NH2 and -OH. With the addition of ZnO NPs, the water absorption rate of the composite membrane decreases, that is, the water absorption of the PCL-CS membrane is greatly improved after the introduction of ZnONPs, but with the increase of the amount of nano ZnO NPs, the water absorption rate of the membrane does not change significantly ( Figure 3 ). It can be seen that whether the nanocomposite material is prepared by direct dispersion of nanoparticles, or by intercalation composite method, in-situ composite method, in-situ polymerization method, sol-gel method, microemulsion polymerization method, etc., the volume fraction of the polymer matrix in the membrane system can be reduced, the solubility of the membrane components can be reduced, and the diffusion rate of the penetrating molecules can be reduced, so that the barrier performance can be improved.
[0059] Experimental Example 5: Structure and morphology of PCL / CS-ZnO polymer
[0060] ATR-FTIR was used at 450-4000 cm -1 Infrared spectra were obtained in the range of 1000 nm to identify unknown functional groups in the material. Scanning electron microscopy (SEM) was used to study the surface morphology at an accelerating voltage of 5-10 kV. Energy dispersive spectroscopy (EDS) was used to characterize the element content of the sample surface.
[0061] 3-1. FTIR analysis
[0062] The FT-IR spectrum of the prepared nanocomposite material is shown in Figure 3 The spectra of PCL, CS and ZnO are shown in Figure 4 The groups corresponding to the absorption peaks a to c are shown in Table 2. Figure 4 In d, the FTIR spectrum of the composite film is between 2800 and 3500 cm -1 、900~1800cm -1 and 400~600cm -1 The absorption peaks are shown in the range of 10.47 nm and 10.77 nm, indicating that the composite film has the same absorption vibration peaks as the original components, indicating that it contains PCL, CS and ZnO components. It is also found that the -NH2 and -OH association peaks, the characteristic absorption peaks of β-glycosidic bonds, amide I and amide II bands of the PCL / CS-ZnO composite film all move to low wavenumbers, which are 3367 cm -1 、1045cm -1 、1642cm -1 、1557cm -1, indicating that there is a strong hydrogen bonding between the two components, that is, PCL and CS have a certain compatibility. These results show that through the composite process, PCL molecules and CS molecules have a certain compatibility, and ZnO NPs are successfully functionalized on the surface of the composite material.
[0063] Table 2 Analysis of FTIR absorption peaks of membrane materials
[0064]
[0065]
[0066] 3-2. SEM-EDS analysis
[0067] SEM micrographs show that the surface of pure PCL membrane and pure CS membrane is smooth and particle-free, and has good polymerization performance. From its low-magnification image, it can be seen that the surface structure of PCL / CS composite membrane is relatively uniform, but there are some stripes, indicating that PCL and CS have a certain compatibility, and there is no obvious phase separation phenomenon when PCL:CS=1:9. High-magnification electron microscopy photos show that the surface of the composite membrane is relatively smooth and ZnO NPs are evenly distributed. However, due to the presence of ZnO nanoparticles, the composite membrane presents white aggregates and small pores dispersed on the surface of the membrane. This is due to the large content of ZnO. In addition, the EDS spectrum shows sharp peaks of C, O, N and Zn on the surface of the composite membrane, confirming the presence of ZnO in the composite membrane.
[0068] Experimental Example 6: Antibacterial Activity
[0069] Escherichia coli and Staphylococcus aureus are the most important human pathogens, which are directly transmitted from poultry to humans and threaten human health. Therefore, in this study, we selected these two bacteria. All samples were sterilized in an autoclave before antimicrobial activity analysis. The antimicrobial activity of the prepared composite films was evaluated by the inhibition zone method. 0.1 mL of different bacterial suspensions (about 10 6 CFU / mL) was inoculated into plate count agar medium (PCA), and the dilution was evenly spread on the surface of the plate with a sterile glass spreader. After standing for 15 minutes, the test antibacterial film (10 mm square) was placed in the center of the culture dish. The antibacterial zone diameter was measured after culturing at 37°C for 24 hours and 48 hours, respectively. Each film was tested in parallel for 3 times.
[0070] Due to their high specific surface area and high surface activity, nano-antimicrobial agents are able to restrict the growth of pathogenic and spoilage microorganisms more effectively than other antimicrobial agents. Recently, the addition of nano-antimicrobial compounds to food packaging materials has received widespread attention. Metal nanoparticles (Ag, Cu, Au), metal oxide nanomaterials (TiO2, ZnO, MgO) and carbon nanotubes are the most commonly used nanofillers for developing antimicrobial effects. Nano-Ag particles have been widely demonstrated to be antimicrobial agents in food and beverage storage, but ZnO NPs are expected to provide more economical and safer food packaging solutions in the future. In this study, we evaluated the antimicrobial effects of PCL / CS-ZnO composites against three human pathogens, including Escherichia coli (Gram-negative), Staphylococcus aureus (Gram-positive) and Bacillus subtilis (Gram-positive). The results are as follows: Figure 5 As shown. From the size of the inhibition zone, it can be seen that when the ZnO addition in the PCL / CS composite membrane is 1%, a slight antibacterial phenomenon occurs around the composite membrane. When the ZnO addition is 2% to 4%, the antibacterial phenomenon around the membrane is obvious, and the inhibition of Escherichia coli and Staphylococcus aureus is more significant compared with Bacillus subtilis. Therefore, it can be concluded that there are differences in the growth inhibition and antibacterial activity of PCL / CS-ZnO composites on different cells. The significant bacterial inactivation can be explained by the uniform dispersion of nanoparticles in the composite material, and a larger addition amount has a larger antibacterial surface and concentration driving force. However, for Escherichia coli and Staphylococcus aureus, the antibacterial effect is limited when the loading amount is 4.0% compared with the composite membrane with a ZnO addition of 3.0%, which should be related to its poor nanoparticle dispersion ( Figure 6 ). In fact, the antimicrobial properties of polymer nanocomposites are affected by various factors, such as particle size, distribution, and interaction with the polymer matrix. In order to fully exert the antimicrobial properties of nanoparticles, they must be uniformly dispersed without forming aggregates. Therefore, small clusters in the composite containing 4.0wt% ZnO can behave as larger particles, thereby showing less antimicrobial activity than individual nanoparticles.
[0071] In order to better evaluate the timeliness of the antibacterial effect of nanoparticles, we also tested the antibacterial effect of nanocomposites with a loading of 3 wt% ZnO within 96 h. Figure 7 It shows that as time goes by, the composite film only has antibacterial activity in a certain area. This may be due to the limitation of the migration range of ZnO nanoparticles, and the dissolution range has a certain limit. In addition, after 96 hours of cultivation, it was found that the inhibition zone did not shrink significantly, indicating that the composite material has significant antibacterial and long-term effect on microorganisms.
[0072] In summary: Uniformly dispersed PCL / CS-ZnO composites were prepared by solution casting. ZnO-NPs have huge specific surface area, excellent thermal conductivity, low thermal expansion coefficient and outstanding mechanical properties, and have bioactivity to inhibit pathogenic and spoilage microorganisms, thereby extending the shelf life. In particular, the biodegradable substrate can be suitable for disposable applications. Sustainable bio-nanocomposites with antimicrobial functions show great potential as an alternative to synthetic plastic packaging materials.
[0073] The conclusion is as follows:
[0074] (1) PCL / CS composite membranes with different mixing ratios were prepared, and their morphology and mechanical analysis were performed. The results showed that when PCL:CS was in the range of 8:2 to 1:3, a more obvious phase separation phenomenon occurred. This indicates that there is a certain interaction between PCL and CS, but the compatibility between the components in the blended membrane is very limited. In addition, the membrane thickness affects its flatness. As the PCL content decreases, the flexibility of the PCL / CS membrane deteriorates, the brittleness increases, and the mechanical strength increases. When PCL:CS=9:1, the Young's modulus is 27.6N / m, the elongation at break is 40.5%, and the water absorption is 45.7%, showing good compatibility, flexibility and hydrophobicity. Taking all factors into consideration, PCL:CS=9:1 was selected as the optimal ratio for subsequent membrane preparation.
[0075] (2) FTIR spectrum analysis showed that the composite film had the same absorption vibration peaks as the original components, indicating that it contained PCL, CS and ZnO components. The -NH2 and -OH association peaks, the characteristic absorption peaks of β-glycosidic bonds, amide I and amide II bands of the composite film all shifted to low wavenumbers, indicating that PCL molecules and CS molecules had a certain compatibility, and ZnO NPs were successfully functionalized on the surface of the composite material.
[0076] (3) SEM-EDS analysis showed that the surface structure of the PCL / CS composite membrane (3wt% ZnO, PCL:CS=1:9) was relatively uniform and smooth, ZnO NPs were evenly distributed, and PCL and CS had a certain compatibility. High-content ZnO nanoparticles would aggregate, resulting in small pores on the membrane surface.
[0077] (4) All samples have good antibacterial activity and can effectively inhibit the growth of bacterial cells. When the ZnO addition amount in the composite film is 2% to 4%, the antibacterial phenomenon is obvious. Among them, the inhibition against Bacillus subtilis, Escherichia coli and Staphylococcus aureus is more significant. When the loading amount is 4.0%, the antibacterial effect is limited, showing less antibacterial activity than single nanoparticles, which may be related to its poor nanoparticle dispersibility. In addition, the composite material has a long-lasting antibacterial effect on microorganisms.
[0078] The above is only a preferred specific implementation of the present invention; however, the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solution and its improved conception of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a PCL / CS-ZnO composite film, characterized in that: The following steps are involved: ① Take a certain amount of ZnO nanoparticles and disperse them in a co-solvent, and perform ultrasonic dispersion treatment for 30 minutes to obtain a ZnO nanoparticle dispersion system; ② Take a certain amount of PCL particles and dissolve them in the ZnO nanoparticle dispersion system, stir for 4 hours and then ultrasonicate for 30 minutes to obtain solution A; ③ Take a certain amount of CS and dissolve it in 80% co-solvent, stir it thoroughly to obtain CS solution; ④ Add CS solution dropwise into solution A, stir, sonicate and degas again; ⑤Then stir at about 50℃ until it becomes a viscous gel mixture; ⑥ Cast the gel-like mixture on a tempered glass plate, apply a uniform film with a coating machine, and then move the glass plate into a constant temperature ventilation chamber, control the evaporation rate of the solvent by adjusting the wind speed, and obtain a PCL / CS-ZnO composite film.
2. The method for preparing a PCL / CS-ZnO composite film according to claim 1, characterized in that: The mass ratio of PCL to CS in the PCL / CS-ZnO composite film is one of 9:1, 8:2, 7:3, 6:4, 1:1, 1:2, 1:3, 1:4, 1:5 or 1:
6.
3. The method for preparing a PCL / CS-ZnO composite film according to claim 1, characterized in that: The co-solvent is glacial acetic acid or glacial acetic acid / water.
4. The method for preparing a PCL / CS-ZnO composite film according to claim 1, characterized in that: The mass ratio of the PCL particles to the ZnO nanoparticle dispersion system is 1:8, and the mass ratio of the CS to the co-solvent is 1:
40.
5. The method for preparing a PCL / CS-ZnO composite film according to claim 1, characterized in that: The CS solution was added dropwise to solution A to make the ZnO NPs content be 1.0 wt%, 2.0 wt%, 3.0 wt% and or 4.0 wt% of the sum of the mass of PCL and CS.
6. The method for preparing a PCL / CS-ZnO composite film according to claim 1, characterized in that: The average thickness of the PCL / CS-ZnO composite film is about 0.15-0.20 mm.
7. The use of a PCL / CS-ZnO composite membrane according to any one of claims 1 to 6, characterized in that: The PCL / CS-ZnO composite film is used in food packaging.
Citation Information
Patent Citations
Biodegradable antibacterial composite fibers and preparation method thereof
CN104328530A
Method for preparing PCL / CS-TiO2 composite film by modifying surfaces of TiO2 nanoparticles with APTES
CN118185088A
Biodegradable piezoelectric composite materials
US20210379249A1