Corrosion-resistant and wear-resistant material for computer bracket and preparation method thereof
By adding glass fiber, anti-UV agent and toughening agent to the ABS plastic bracket material, combined with efficient processing, the shortcomings of the ABS plastic bracket in UV aging, heat resistance and fire resistance are solved, and higher material performance is achieved. and security.
Patent Information
- Application Number
- CN202410806764.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing ABS plastic bracket materials have deficiencies in UV aging, heat resistance and fire resistance, resulting in shortened service life and potential safety hazards.
Using a combination of ABS resin, glass fiber, compatibilizer, anti-UV agent, toughening agent and processing stabilizer, anti-corrosion and wear-resistant materials for computer brackets are prepared through efficient mixing and injection molding processes. The anti-UV agent contains hindered amine and thiophene ring Structure, the toughening agent contains DOPO structure to improve material performance.
Significantly improve the material's UV aging resistance, fire resistance and heat resistance, meet the use requirements of computer brackets, extend the service life and reduce safety hazards.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, and in particular to an anticorrosion and wear-resistant material for a computer bracket and a preparation method thereof. Background Art
[0002] At present, the materials commonly used for computer monitor heightening brackets on the market include aluminum alloy, iron, ABS plastic and wood. ABS plastic brackets are widely used due to their advantages such as light weight and firmness. ABS resin is composed of three monomers: acrylonitrile, butadiene and styrene, which give ABS resin excellent comprehensive properties. However, the ABS resin molecular chain contains phenyl, unsaturated carbon-carbon double bonds and cyano groups, which make it susceptible to degradation due to aging effects such as ultraviolet rays. Moreover, as a general engineering plastic, ABS plastic has insufficient heat resistance. When the temperature exceeds the tolerance range, due to the poor adhesion of the ABS molecular chain, it will soften and deform, shortening its service life. In addition, ABS resin is flammable, and the materials made from it have safety hazards such as insufficient fire resistance during transportation, storage and use.
[0003] In summary, developing a suitable modification method to improve the UV aging resistance, heat resistance and fire resistance of ABS resin is necessary and important in practical use. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides an anti-corrosion and wear-resistant material for a computer bracket and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions: A corrosion-resistant and wear-resistant material for a computer bracket, comprising the following raw materials in parts by weight: 55-65 parts of ABS resin, 8-12 parts of glass fiber (supplier: Hangzhou Gaoke Composite Materials Co., Ltd.), 8-12 parts of a compatibilizer, 0.5-0.8 parts of an anti-ultraviolet agent, 3-5 parts of a toughening agent, 0.1-0.2 parts of a processing stabilizer, and 0.05-0.08 parts of a coupling agent; the compatibilizer is a styrene maleic anhydride copolymer (supplier: Shenzhen Yingqun Chemical Co., Ltd.), the processing stabilizer is triphenyl phosphite, and the coupling agent is KH550; The preparation of the anticorrosion and wear-resistant material for a computer bracket comprises the following steps: Add ABS resin, glass fiber, compatibilizer, UV inhibitor, toughening agent, processing stabilizer and coupling agent into a high-speed mixer, stir and mix at room temperature for 10-15 minutes, take out and transfer to a screw extruder, mix and granulate at 160-170°C, and then make a finished product by injection molding, that is, the anti-corrosion and wear-resistant material for computer bracket is obtained.
[0006] The preparation of the anti-ultraviolet agent comprises the following steps: Step A1: 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol and acetic acid are added to a reaction bottle, and stirred at 60° C. for 10-15 minutes; then a nitric acid-acetic acid mixed solution is quickly added, and stirring is continued for 30-40 minutes to obtain a reaction solution, and then the reaction solution is added to ice water, filtered, washed with water, and vacuum dried to obtain a reaction product 1; Further, the dosage ratio of 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol, acetic acid, nitric acid-acetic acid mixed solution and ice water is 0.03 mol: 200 mL: 60-70 mL: 300 mL, and the nitric acid-acetic acid mixed solution is prepared by mixing nitric acid and acetic acid in a dosage ratio of 0.36 g: 6 mL; During the reaction of step A1, the ortho position of the phenolic hydroxyl group in 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol is replaced by a nitro group to obtain a reaction product 1; Step A2: Add the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add the above 2,5-thiophene dicarbonyl chloride into dimethyl sulfoxide to obtain a mixed solution b, slowly dropwise add the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, stir and react at a constant temperature for 8-10 hours, and distill under reduced pressure to obtain a reaction product 2; Further, the dosage ratio of the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide is 0.2 mol: 0.01-0.015 mol: 0.2 mol: 70-80 mL; the dosage ratio of 2,5-thiophene dicarbonyl chloride and dimethyl sulfoxide is 0.1 mol: 40-50 mL; the dosage ratio of the mixed solution a and the mixed solution b is 75-85 mL: 45-55 mL; During the reaction of step A2, the alcoholic hydroxyl group of the reaction product 1 reacts with 2,5-thiophenedicarbonyl chloride to generate the reaction product 2; Step A3: Add the reaction product 2 and zinc powder to a reaction bottle filled with a mixed solvent, start stirring, slowly add ammonium chloride to the reaction bottle, stir and react at room temperature for 2-3 hours, and obtain the reaction product 3 after suction filtration, extraction, drying and reduced pressure distillation; Furthermore, the amount ratio of the reaction product 2, zinc powder, mixed solvent, and ammonium chloride is 0.1 mol: 0.5 mol: 900-1000 mL: 0.9-1.0 mol, and the mixed solvent is prepared by mixing ethyl acetate and water in a volume ratio of 1:1; During the reaction of step A3, the nitro group in the reaction product 2 is reduced to an amino group to obtain the reaction product 3; Step A4: adding 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid to DMF, adding dichlorothionyl under stirring, and reacting under reflux and stirring at 50° C. for 4-5 hours to obtain 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride; then adding the reaction product 3, potassium carbonate and dimethyl sulfoxide to a flask to obtain a mixed solution c, and then adding the above 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride to dimethyl sulfoxide to obtain a mixed solution d, slowly dropping the mixed solution d into the mixed solution c in an ice-water bath at 0° C., after the dropping is completed, heating to 40° C., stirring at a constant temperature for 8-10 hours, and distilling under reduced pressure to obtain an anti-ultraviolet agent; Further, the amount ratio of the reaction product 3, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.01-0.015 mol: 115-125 mL; the amount ratio of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride and dimethyl sulfoxide is 0.1 mol: 45-55 mL; the amount ratio of the mixed solution c and the mixed solution d is 120-130 mL: 50-60 mL; During the reaction of step A4, the amino group of the reaction product 3 reacts with 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride to generate an anti-ultraviolet agent; The toughening agent is prepared by the following steps: Step B1: Add monoethyl fumarate and DOPO into a flask, start stirring, raise the temperature to 125-135°C, and stir at constant temperature for 3-4 hours to obtain reaction product a; Furthermore, the dosage ratio of monoethyl fumarate and DOPO is 0.1 mol:0.1 mol; During the reaction of step B1, DOPO adds to the carbon-carbon double bond of monoethyl fumarate to obtain a reaction product a; Step B2: In a nitrogen atmosphere, add the reaction product a and ethyl acetate into a flask, start stirring, raise the temperature to 40-50° C., add pyridine and glycidyl methacrylate, and react with constant temperature stirring for 8-10 hours to obtain the reaction product b; Further, the usage ratio of the reaction product a, ethyl acetate, pyridine and glycidyl methacrylate is 0.1 mol: 90-100 mL: 0.001-0.0012 mol: 0.1 mol; During the reaction of step B2, the carboxyl group of the reaction product a reacts with the epoxy group of glycidyl methacrylate to generate a reaction product b containing a terminal double bond; Step B3: Add methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid into a reaction bottle, start stirring, then add dibenzoyl peroxide and solvent S, stir and react at 100° C. for 7-8 hours to obtain a toughening agent; Furthermore, the usage ratio of methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid, dibenzoyl peroxide, and solvent S is 45g:40g:5-6g:4-5g:5g:1g:250mL; solvent S is prepared by mixing xylene and butyl acetate in a volume ratio of 3:2; During the reaction of step B3, under the initiation of dibenzoyl peroxide, methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid are copolymerized to obtain a toughening agent; Beneficial effects of the invention: The invention discloses an anticorrosion and wear-resistant material for a computer bracket, comprising the following raw materials: ABS resin, glass fiber, compatibilizer, anti-ultraviolet agent, toughening agent, processing stabilizer and coupling agent. ABS resin has good tolerance to common acid and alkali corrosive media, and ABS has good wear resistance, so the anticorrosion and wear resistance of the computer bracket material meets the use requirements. The synthesized UV inhibitor contains hindered amine structure, o-hydroxybenzotriazole structure, thiophene ring and the like in the molecule; the ortho-hydroxyl group in the o-hydroxybenzotriazole structure and the nitrogen atom on the triazole ring form a six-membered chelate ring through intramolecular hydrogen bonding to play the role of UV absorption, and based on the tautomerism in the compound molecule, the absorbed UV energy is converted into other forms of energy release to protect the matrix from UV damage; the introduction of the thiophene ring not only broadens the UV absorption range, but also increases the molar absorption coefficient, further enhancing the UV absorption function of the UV inhibitor; the hindered amine structure can capture the active free radicals generated by the matrix under the action of ultraviolet rays, play a photostabilizing role, and synergistically improve the anti-ultraviolet aging performance of the material with the o-hydroxybenzotriazole structure and the thiophene ring; the UV inhibitor molecule also contains a polar carbonyl group, which has good compatibility with the polar cyano group in the ABS resin and is more evenly dispersed in the matrix, and the molecular weight of the UV inhibitor increases, and its stability increases, which can better play the role of improving the anti-ultraviolet aging performance of the material.
[0007] The synthesized toughening agent is an acrylic copolymer obtained by copolymerizing methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid, and contains DOPO structure, carboxyl group, hydroxyl group and the like in the molecule. The DOPO structure can dehydrate and degrade the polymer surface to form a carbon layer when the matrix burns, and the phosphorus-containing derivatives produced at the same time cover the polymer surface, isolate the combustible gas, block the heat transfer, form a physical shield, and play a flame retardant and fireproof role; the acrylic copolymer has good compatibility with ABS resin due to the carboxyl and hydroxyl polar groups contained, and can be evenly dispersed in the matrix, and the rigid cold-drawing toughening effect produced by the acrylic copolymer in the system improves the heat resistance of the system; therefore, adding the toughening agent improves the fire resistance and heat resistance of the material. DETAILED DESCRIPTION
[0008] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0009] Embodiment 1: A kind of anti-ultraviolet agent, its preparation comprises the following steps: Step A1: 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol and acetic acid are added to a reaction bottle, and stirred at 60° C. for 10 min; then a nitric acid-acetic acid mixed solution is quickly added, and stirring is continued for 30 min to obtain a reaction solution, and then the reaction solution is added to ice water, filtered, washed with water, and vacuum dried to obtain a reaction product 1; the amount ratio of 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol, acetic acid, nitric acid-acetic acid mixed solution and ice water is 0.03 mol: 200 mL: 60 mL: 300 mL, and the nitric acid-acetic acid mixed solution is prepared by mixing nitric acid and acetic acid in an amount ratio of 0.36 g: 6 mL; Step A2: adding the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution a, then adding the above 2,5-thiophene dicarbonyl chloride into dimethyl sulfoxide to obtain a mixed solution b, slowly dropping the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropping is completed, heating to 40°C, stirring at a constant temperature for 8 hours, and distilling under reduced pressure to obtain a reaction product 2; the amount ratio of the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide is 0.2 mol: 0.01 mol: 0.2 mol: 70 mL; the amount ratio of 2,5-thiophene dicarbonyl chloride and dimethyl sulfoxide is 0.1 mol: 40 mL; the amount ratio of the mixed solution a to the mixed solution b is 75 mL: 45 mL; Step A3: adding the reaction product 2 and zinc powder to a reaction bottle filled with a mixed solvent, starting stirring, slowly adding ammonium chloride to the reaction bottle, stirring and reacting at room temperature for 2 hours, and obtaining the reaction product 3 after suction filtration, extraction, drying, and reduced pressure distillation; the amount ratio of the reaction product 2, zinc powder, mixed solvent, and ammonium chloride is 0.1 mol: 0.5 mol: 900 mL: 0.9 mol, and the mixed solvent is prepared by mixing ethyl acetate and water in a volume ratio of 1:1; Step A4: 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid was added to DMF, and dichlorothionyl was added under stirring, and the mixture was refluxed and stirred at 50°C for 4 h to obtain 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride; the reaction product 3, potassium carbonate and dimethyl sulfoxide were added to a flask to obtain a mixed solution c, and the above 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride was added to dimethyl sulfoxide to obtain a mixed solution d, and the mixture was heated in an ice-water bath at 0°C. , slowly drop the mixed solution d into the mixed solution c, after the addition is completed, the temperature is raised to 40°C, the reaction is stirred at a constant temperature for 8 hours, and the anti-ultraviolet agent is obtained by distillation under reduced pressure; the dosage ratio of the reaction product 3, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.01 mol: 115 mL; the dosage ratio of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride and dimethyl sulfoxide is 0.1 mol: 45 mL; the dosage ratio of the mixed solution c and the mixed solution d is 120 mL: 50 mL.
[0010] Embodiment 2: A kind of anti-ultraviolet agent, its preparation comprises the following steps: Step A1: 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol and acetic acid are added to a reaction bottle, and stirred at 60° C. for 12 minutes; then a nitric acid-acetic acid mixed solution is quickly added, and stirring is continued for 35 minutes to obtain a reaction solution, and then the reaction solution is added to ice water, filtered, washed with water, and vacuum dried to obtain a reaction product 1; the amount ratio of 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol, acetic acid, nitric acid-acetic acid mixed solution and ice water is 0.03 mol: 200 mL: 65 mL: 300 mL, and the nitric acid-acetic acid mixed solution is prepared by mixing nitric acid and acetic acid in an amount ratio of 0.36 g: 6 mL; Step A2: Add the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add the above 2,5-thiophene dicarbonyl chloride into dimethyl sulfoxide to obtain a mixed solution b, slowly dropwise add the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, stir and react at a constant temperature for 9 hours, and distill under reduced pressure to obtain a reaction product 2; the amount ratio of the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide is 0.2 mol: 0.012 mol: 0.2 mol: 75 mL; the amount ratio of 2,5-thiophene dicarbonyl chloride and dimethyl sulfoxide is 0.1 mol: 45 mL; the amount ratio of the mixed solution a to the mixed solution b is 80 mL: 50 mL; Step A3: Add the reaction product 2 and zinc powder to a reaction bottle filled with a mixed solvent, start stirring, slowly add ammonium chloride to the reaction bottle, stir and react at room temperature for 2.5 hours, and obtain the reaction product 3 after suction filtration, extraction, drying and reduced pressure distillation; the amount ratio of the reaction product 2, zinc powder, mixed solvent and ammonium chloride is 0.1 mol: 0.5 mol: 950 mL: 0.95 mol, and the mixed solvent is prepared by mixing ethyl acetate and water in a volume ratio of 1:1; Step A4: 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid was added to DMF, and dichlorothionyl was added under stirring, and the mixture was refluxed and stirred at 50°C for 4.5 h to obtain 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride; the reaction product 3, potassium carbonate and dimethyl sulfoxide were added to a flask to obtain a mixed solution c, and the above 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride was added to dimethyl sulfoxide to obtain a mixed solution d, and the mixture was heated in an ice-water bath at 0°C. , slowly drop the mixed solution d into the mixed solution c, after the addition is completed, the temperature is raised to 40°C, the reaction is stirred at a constant temperature for 9 hours, and the anti-ultraviolet agent is obtained by distillation under reduced pressure; the dosage ratio of the reaction product 3, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.012 mol: 120 mL; the dosage ratio of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride and dimethyl sulfoxide is 0.1 mol: 50 mL; the dosage ratio of the mixed solution c and the mixed solution d is 125 mL: 55 mL.
[0011] Embodiment 3: A kind of anti-ultraviolet agent, its preparation comprises the following steps: Step A1: 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol and acetic acid are added to a reaction bottle, and stirred at 60° C. for 15 minutes; then a nitric acid-acetic acid mixed solution is quickly added, and stirring is continued for 40 minutes to obtain a reaction solution, and then the reaction solution is added to ice water, filtered, washed with water, and vacuum dried to obtain a reaction product 1; the amount ratio of 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol, acetic acid, nitric acid-acetic acid mixed solution and ice water is 0.03 mol: 200 mL: 70 mL: 300 mL, and the nitric acid-acetic acid mixed solution is prepared by mixing nitric acid and acetic acid in an amount ratio of 0.36 g: 6 mL; Step A2: adding the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution a, then adding the above 2,5-thiophene dicarbonyl chloride into dimethyl sulfoxide to obtain a mixed solution b, slowly dropping the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropping is completed, heating to 40°C, stirring and reacting at a constant temperature for 10 hours, and distilling under reduced pressure to obtain a reaction product 2; the amount ratio of the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide is 0.2 mol: 0.015 mol: 0.2 mol: 80 mL; the amount ratio of 2,5-thiophene dicarbonyl chloride and dimethyl sulfoxide is 0.1 mol: 50 mL; the amount ratio of the mixed solution a to the mixed solution b is 85 mL: 55 mL; Step A3: adding the reaction product 2 and zinc powder to a reaction bottle filled with a mixed solvent, starting stirring, slowly adding ammonium chloride to the reaction bottle, stirring and reacting at room temperature for 3 hours, and obtaining the reaction product 3 after suction filtration, extraction, drying, and reduced pressure distillation; the amount ratio of the reaction product 2, zinc powder, mixed solvent, and ammonium chloride is 0.1 mol: 0.5 mol: 1000 mL: 1.0 mol, and the mixed solvent is prepared by mixing ethyl acetate and water in a volume ratio of 1:1; Step A4: 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid was added to DMF, and dichlorothionyl was added under stirring, and the mixture was refluxed and stirred at 50°C for 5 h to obtain 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride; the reaction product 3, potassium carbonate and dimethyl sulfoxide were added to a flask to obtain a mixed solution c, and the above 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride was added to dimethyl sulfoxide to obtain a mixed solution d, which was then heated in an ice-water bath at 0°C. , slowly add mixed solution d to mixed solution c, after the addition is completed, heat to 40°C, stir and react at constant temperature for 10 hours, and distill under reduced pressure to obtain an anti-ultraviolet agent; the dosage ratio of reaction product 3, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.015 mol: 125 mL; the dosage ratio of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride and dimethyl sulfoxide is 0.1 mol: 55 mL; the dosage ratio of mixed solution c and mixed solution d is 130 mL: 60 mL.
[0012] Embodiment 4: A toughening agent, the preparation of which comprises the following steps: Step B1: Add monoethyl fumarate and DOPO to a flask, start stirring, heat to 125°C, and react at constant temperature and stirring for 3 hours to obtain reaction product a; the dosage ratio of monoethyl fumarate to DOPO is 0.1 mol:0.1 mol; Step B2: In a nitrogen atmosphere, add the reaction product a and ethyl acetate into a flask, start stirring, heat to 40°C, add pyridine and glycidyl methacrylate, and react at a constant temperature with stirring for 8 hours to obtain the reaction product b; the amount ratio of the reaction product a, ethyl acetate, pyridine and glycidyl methacrylate is 0.1 mol: 90 mL: 0.001 mol: 0.1 mol; Step B3: Add methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid into a reaction bottle, start stirring, then add dibenzoyl peroxide and solvent S, and stir the reaction at 100°C for 7 hours to obtain a toughening agent; the amount ratio of methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid, dibenzoyl peroxide, and solvent S is 45g:40g:5g:5g:5g:1g:250mL; solvent S is prepared by mixing xylene and butyl acetate in a volume ratio of 3:2.
[0013] Embodiment 5: A toughening agent, the preparation of which comprises the following steps: Step B1: Add monoethyl fumarate and DOPO to a flask, start stirring, heat to 130°C, and react with constant temperature stirring for 3.5 hours to obtain reaction product a; the dosage ratio of monoethyl fumarate to DOPO is 0.1 mol:0.1 mol; Step B2: In a nitrogen atmosphere, add the reaction product a and ethyl acetate into a flask, start stirring, heat to 45°C, add pyridine and glycidyl methacrylate, and react at a constant temperature with stirring for 9 hours to obtain the reaction product b; the amount ratio of the reaction product a, ethyl acetate, pyridine and glycidyl methacrylate is 0.1 mol: 95 mL: 0.0011 mol: 0.1 mol; Step B3: Add methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid into a reaction bottle, start stirring, then add dibenzoyl peroxide and solvent S, and stir the reaction at 100°C for 7.5 hours to obtain a toughening agent; the amount ratio of methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid, dibenzoyl peroxide, and solvent S is 45g:40g:5.5g:4.5g:5g:1g:250mL; solvent S is prepared by mixing xylene and butyl acetate in a volume ratio of 3:2.
[0014] Embodiment 6: A toughening agent, the preparation of which comprises the following steps: Step B1: Add monoethyl fumarate and DOPO to a flask, start stirring, heat to 135°C, and react at constant temperature and stirring for 4 hours to obtain reaction product a; the dosage ratio of monoethyl fumarate to DOPO is 0.1 mol:0.1 mol; Step B2: In a nitrogen atmosphere, add the reaction product a and ethyl acetate into a flask, start stirring, heat to 50°C, add pyridine and glycidyl methacrylate, and react at a constant temperature with stirring for 10 hours to obtain the reaction product b; the amount ratio of the reaction product a, ethyl acetate, pyridine and glycidyl methacrylate is 0.1 mol: 100 mL: 0.0012 mol: 0.1 mol; Step B3: Add methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid into a reaction bottle, start stirring, then add dibenzoyl peroxide and solvent S, and stir the reaction at 100°C for 8 hours to obtain a toughening agent; the amount ratio of methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid, dibenzoyl peroxide, and solvent S is 45g:40g:6g:4g:5g:1g:250mL; solvent S is prepared by mixing xylene and butyl acetate in a volume ratio of 3:2.
[0015] Example 7: A corrosion-resistant and wear-resistant material for a computer bracket, comprising the following raw materials in parts by weight: 55 parts of ABS resin, 8 parts of glass fiber (supplier: Hangzhou Gaoke Composite Materials Co., Ltd.), 8 parts of compatibilizer, 0.5 parts of anti-ultraviolet agent, 3 parts of toughening agent, 0.1 parts of processing stabilizer and 0.05 parts of coupling agent; the compatibilizer is styrene maleic anhydride copolymer (supplier: Shenzhen Yingqun Chemical Co., Ltd.), the processing stabilizer is triphenyl phosphite, and the coupling agent is KH550; The preparation of the anticorrosion and wear-resistant material for a computer bracket comprises the following steps: ABS resin, glass fiber, compatibilizer, UV inhibitor, toughening agent, processing stabilizer and coupling agent are added to a high-speed mixer, stirred and mixed at room temperature for 10 minutes, taken out and transferred to a screw extruder, mixed and granulated at 160°C, and then injection molded into a finished product, that is, an anti-corrosion and wear-resistant material for a computer bracket.
[0016] Example 8: A corrosion-resistant and wear-resistant material for a computer bracket, comprising the following raw materials in parts by weight: 60 parts of ABS resin, 10 parts of glass fiber (supplier: Hangzhou Gaoke Composite Materials Co., Ltd.), 10 parts of a compatibilizer, 0.65 parts of an anti-ultraviolet agent, 4 parts of a toughening agent, 0.15 parts of a processing stabilizer, and 0.06 parts of a coupling agent; the compatibilizer is a styrene maleic anhydride copolymer (supplier: Shenzhen Yingqun Chemical Co., Ltd.), the processing stabilizer is triphenyl phosphite, and the coupling agent is KH550; The preparation of the anticorrosion and wear-resistant material for a computer bracket comprises the following steps: ABS resin, glass fiber, compatibilizer, anti-ultraviolet agent, toughening agent, processing stabilizer and coupling agent are added to a high-speed mixer, stirred and mixed at room temperature for 12 minutes, taken out and transferred to a screw extruder, mixed and granulated at 165°C, and then injection molded into a finished product, that is, an anti-corrosion and wear-resistant material for a computer bracket.
[0017] Example 9: A corrosion-resistant and wear-resistant material for a computer bracket, comprising the following raw materials in parts by weight: 65 parts of ABS resin, 12 parts of glass fiber (supplier: Hangzhou Gaoke Composite Materials Co., Ltd.), 12 parts of a compatibilizer, 0.8 parts of an anti-ultraviolet agent, 5 parts of a toughening agent, 0.2 parts of a processing stabilizer, and 0.08 parts of a coupling agent; the compatibilizer is a styrene maleic anhydride copolymer (supplier: Shenzhen Yingqun Chemical Co., Ltd.), the processing stabilizer is triphenyl phosphite, and the coupling agent is KH550; The preparation of the anticorrosion and wear-resistant material for a computer bracket comprises the following steps: ABS resin, glass fiber, compatibilizer, anti-ultraviolet agent, toughening agent, processing stabilizer and coupling agent are added to a high-speed mixer, stirred and mixed at room temperature for 15 minutes, taken out and transferred to a screw extruder, mixed and granulated at 170°C, and then injection molded into a finished product, that is, an anti-corrosion and wear-resistant material for a computer bracket is obtained.
[0018] Comparative Example 1: This comparative example is a commercially available computer bracket made of ordinary ABS material.
[0019] Comparative Example 2: Compared with Example 9, the anti-ultraviolet agent is replaced with reaction product 3, that is, no hindered amine structure is introduced, and the rest is exactly the same as Example 9 to obtain an anti-corrosion and wear-resistant material for a computer bracket.
[0020] Comparative Example 3: Compared with Example 9, the toughening agent is replaced with a common acrylic copolymer, that is, the DOPO structure is not introduced, and the rest is exactly the same as Example 9 to prepare an anticorrosive and wear-resistant material for a computer bracket.
[0021] The anti-corrosion and wear-resistant material for the computer bracket disclosed in the present invention is further tested for its effect, and the test results are as follows.
[0022] The tensile strength of the material was measured according to GB / T1040-2018 "Determination of tensile properties of plastics"; UV aging conditions: 0.89W / m 2 , temperature is 50℃, aging time is 480h, after the material is aged by ultraviolet light, the change rate of tensile strength is determined according to the method of GB / T1040-2018; the combustion grade of the material is determined according to the UL-94 combustion standard; the Vicat softening point temperature of the material specimen is tested by a thermal deformation tester, and the results are recorded in Table 1; Table 1: Test results According to the data in Table 1, compared with Example 1, Example 7, Example 8 and Example 9, it can be seen that the anti-corrosion and wear-resistant material for computer brackets of the present invention has better anti-ultraviolet aging performance, fire resistance and heat resistance than the common ABS material for computer brackets on the market; compared with Example 2, Example 9 shows that the use of a synthetic anti-ultraviolet agent, the introduction of a hindered amine structure, and the synergistic effect of the o-hydroxybenzotriazole structure and the thiophene ring on the anti-ultraviolet aging performance of the material can be improved; compared with Example 3, Example 9 shows that the use of a synthetic toughening agent, the introduction of a DOPO structure into the acrylic copolymer can improve the heat resistance of the material while having good fire resistance.
[0023] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. An anti-corrosion and wear-resistant material for a computer bracket, Features: The invention comprises the following raw materials in parts by weight: 55-65 parts of ABS resin, 8-12 parts of glass fiber, 8-12 parts of compatibilizer, 0.5-0.8 parts of UV inhibitor, 3-5 parts of toughening agent, 0.1-0.2 parts of processing stabilizer and 0.05-0.08 parts of coupling agent; The preparation of the anti-ultraviolet agent comprises the following steps: Step A1: 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol and acetic acid are added to a reaction bottle, and stirred at 60° C. for 10-15 minutes; then a nitric acid-acetic acid mixed solution is quickly added, and stirring is continued for 30-40 minutes to obtain a reaction solution, and then the reaction solution is added to ice water, filtered, washed with water, and vacuum dried to obtain a reaction product 1; Step A2: Add the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add the above 2,5-thiophene dicarbonyl chloride into dimethyl sulfoxide to obtain a mixed solution b, slowly dropwise add the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, stir and react at a constant temperature for 8-10 hours, and distill under reduced pressure to obtain a reaction product 2; Step A3: Add the reaction product 2 and zinc powder to a reaction bottle filled with a mixed solvent, start stirring, slowly add ammonium chloride to the reaction bottle, stir and react at room temperature for 2-3 hours, and obtain the reaction product 3 after suction filtration, extraction, drying and reduced pressure distillation; Step A4: 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetic acid is added to DMF, and dichlorothionyl is added under stirring, and the mixture is refluxed and stirred at 50°C for 4-5h to obtain 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride; the reaction product 3, potassium carbonate and dimethyl sulfoxide are added to a flask to obtain a mixed solution c, and then the above 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride is added to dimethyl sulfoxide to obtain a mixed solution d, and the mixed solution d is slowly added dropwise to the mixed solution c in an ice-water bath at 0°C. After the addition is completed, the mixture is heated to 40°C, stirred at a constant temperature for 8-10h, and distilled under reduced pressure to obtain an anti-ultraviolet agent.
2. The anti-corrosion and wear-resistant material for a computer bracket according to claim 1, Features: In step A1, the dosage ratio of 3-(2H-benzotriazole-2-yl)-4-hydroxyphenylethanol, acetic acid, nitric acid-acetic acid mixed solution and ice water is 0.03 mol: 200 mL: 60-70 mL: 300 mL, and the nitric acid-acetic acid mixed solution is prepared by mixing nitric acid and acetic acid in a dosage ratio of 0.36 g: 6 mL.
3. The anticorrosion and wear-resistant material for a computer bracket according to claim 1, Features: In step A2, the amount ratio of reaction product 1, pyridine, triethylamine and dimethyl sulfoxide is 0.2 mol: 0.01-0.015 mol: 0.2 mol: 70-80 mL; the amount ratio of 2,5-thiophene dicarbonyl chloride and dimethyl sulfoxide is 0.1 mol: 40-50 mL; the amount ratio of mixed solution a and mixed solution b is 75-85 mL: 45-55 mL.
4. The anticorrosion and wear-resistant material for a computer bracket according to claim 1, Features: In step A3, the usage ratio of the reaction product 2, zinc powder, mixed solvent and ammonium chloride is 0.1 mol: 0.5 mol: 900-1000 mL: 0.9-1.0 mol, and the mixed solvent is prepared by mixing ethyl acetate and water in a volume ratio of 1:
1.
5. The anti-corrosion and wear-resistant material for a computer bracket according to claim 1, Features: In step A4, the amount ratio of the reaction product 3, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.01-0.015 mol: 115-125 mL; the amount ratio of 2-(2,2,6,6-tetramethylpiperidin-4-yl)acetyl chloride and dimethyl sulfoxide is 0.1 mol: 45-55 mL; the amount ratio of the mixed solution c and the mixed solution d is 120-130 mL: 50-60 mL.
6. The anticorrosion and wear-resistant material for a computer bracket according to claim 1, Features: The toughening agent is prepared by the following steps: Step B1: Add monoethyl fumarate and DOPO into a flask, start stirring, raise the temperature to 125-135°C, and stir at constant temperature for 3-4 hours to obtain reaction product a; Step B2: In a nitrogen atmosphere, add the reaction product a and ethyl acetate into a flask, start stirring, raise the temperature to 40-50° C., add pyridine and glycidyl methacrylate, and react with constant temperature stirring for 8-10 hours to obtain the reaction product b; Step B3: Add methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid into a reaction bottle, start stirring, then add dibenzoyl peroxide and solvent S, stir and react at 100° C. for 7-8 hours to obtain a toughening agent.
7. The anticorrosion and wear-resistant material for a computer bracket according to claim 6, Features: In step B1, the usage ratio of monoethyl fumarate and DOPO is 0.1 mol:0.1 mol; in step B2, the usage ratio of reaction product a, ethyl acetate, pyridine and glycidyl methacrylate is 0.1 mol:90-100 mL:0.001-0.0012 mol:0.1 mol.
8. The anticorrosion and wear-resistant material for a computer bracket according to claim 6, Features: In step B3, the usage ratio of methyl methacrylate, butyl acrylate, hydroxyethyl methacrylate, reaction product b and acrylic acid, dibenzoyl peroxide, and solvent S is 45g:40g:5-6g:4-5g:5g:1g:250mL; solvent S is prepared by mixing xylene and butyl acetate in a volume ratio of 3:
2.
9. The anticorrosion and wear-resistant material for a computer bracket according to claim 1, Features: The compatibilizer is styrene maleic anhydride copolymer, the processing stabilizer is triphenyl phosphite, and the coupling agent is KH550.
10. The method for preparing the anticorrosion and wear-resistant material for a computer bracket according to claim 1, Features: The steps include: Add ABS resin, glass fiber, compatibilizer, UV inhibitor, toughening agent, processing stabilizer and coupling agent into a high-speed mixer, stir and mix at room temperature for 10-15 minutes, take out and transfer to a screw extruder, mix and granulate at 160-170°C, and then make a finished product by injection molding, that is, the anti-corrosion and wear-resistant material for computer bracket is obtained.
Citation Information
Patent Citations
Method for stabilizing organic material
JP1994025430A
Process for the preparation of novel vinylic hindered amine light stabilizers
US20020115754A1
Flameproof acrylate
US20230219987A1
Polycarbonate / ABS composition, preparation method therefor and automobile pillar protective panel
WO2021128965A1
Anti-deformation plastic and preparation process therefor
WO2023123076A1