Preparation method of glass-based composite material and high-performance glass product

By combining waste glass fibers with bisphenol A diglycidyl ether and ethylene-tetrafluoroethylene copolymer, and adding composite functional agents, high-performance glass products are formed, which solves the problems of aging and poor thermal performance of epoxy resin under ultraviolet light. , achieving long-term absorption of ultraviolet light and high-temperature flame retardancy, and is suitable for automobiles, construction, electronic components and other fields.

CN118745280AInactive Publication Date: 2024-10-08SHANGHAI INGENUITY GLASS DECORATION ENG CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411068493.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Glass fiber reinforced epoxy resin-based composite materials age under ultraviolet sunlight, have poor thermal properties, and are difficult to reprocess, resulting in resource waste and solid waste pollution, limiting their wide application.

Method used

Using waste glass fiber, bisphenol A diglycidyl ether, ethylene-tetrafluoroethylene copolymer and composite functional agent, high-performance glass products are formed through heat treatment and pressing to increase its ultraviolet light absorption capacity and flame retardancy.

Benefits of technology

It improves the mechanical strength, dimensional stability and electrical insulation of glass products, can effectively absorb ultraviolet light and form an isolation film in high-temperature fires, extending the service life and reducing resource waste.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a glass-based composite material preparation method and a high-performance glass product, and belongs to the field of glass-based epoxy resin composites.The glass-based composite material is prepared from, by mass, 55-60 parts of waste glass fibers, 18-23 parts of bisphenol A diglycidyl ether, 5-10 parts of ethylene-tetrafluoroethylene copolymer, 6-7 parts of organic acid curing agent and 6-10 parts of composite functional agent; the invention also discloses a production process of the glass product, which comprises the following steps: screening, weighing, cleaning and thermally treating the waste glass fibers, stretching, fully mixing the bisphenol A diglycidyl ether epoxy resin, the ethylene-tetrafluoroethylene copolymer, the composite functional agent and the organic acid curing agent, preparing the mixture and the arranged glass fibers into a preform, and carrying out heat treatment on the preform to obtain the glass product. And finally, introducing the prefabricated body into a mold, and carrying out compression molding to obtain the glass product. The glass product disclosed by the invention can effectively absorb ultraviolet rays for a long time, is good in mechanical strength, further has flame retardance, and can form an isolating membrane to protect life and property safety in a fire disaster.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass-based epoxy resin composite materials, and in particular to a method for preparing a glass-based composite material and a high-performance glass product. Background Art

[0002] Glass fiber reinforced epoxy resin-based composite material is an excellent new type of structural material, which has the characteristics of glass and epoxy resin. It is light, corrosion-resistant, easy to process, and has insulation properties. Therefore, it can be widely used in construction, automobiles, electronic components and other fields. However, epoxy resin has poor heat resistance and mechanical strength, especially weak resistance to ultraviolet sunlight. Under long-term sunlight exposure, the amine part of the epoxy polymer will be oxidized to form a conjugated system of colored substances. The aged epoxy resin is not beautiful and cannot protect people. In addition, since the chemical structure of the epoxy resin itself is easily deformed at high temperatures, its service life is generally not high, which is very unfavorable for process production. It will also burn in a fire, endangering people's life and property safety. Not only that, the degraded glass fiber reinforced epoxy resin-based composite material is also difficult to reprocess due to the characteristics of epoxy resin that cannot be melted and dissolved, resulting in waste of resources and solid waste pollution. The above shortcomings are not conducive to the promotion of glass fiber reinforced epoxy resin-based composite materials. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a glass-based composite material and a high-performance glass product. By adding a composite functional agent during the glass production process, ultraviolet light can be effectively absorbed for a long time, and an isolation film can be formed in the event of a high-temperature fire to have a flame retardant effect.

[0004] The purpose of the present invention can be achieved through the following technical solutions: A high-performance glass product, comprising the following raw materials in parts by weight: 55-60 parts of waste glass fiber, 18-23 parts of bisphenol A diglycidyl ether, 5-10 parts of ethylene-tetrafluoroethylene copolymer, 6-7 parts of organic acid curing agent, and 6-10 parts of composite functional agent; The method for preparing the glass-based composite material comprises the following steps: Step 1: Screen, weigh, clean, heat treat at 240-280°C for 35-45min, and stretch the waste glass fibers; Step 2: Cut the stretched glass fiber into strips of 30-50 cm and dry them; Step 3: Fully mix bisphenol A diglycidyl ether epoxy resin, ethylene-tetrafluoroethylene copolymer, composite functional agent, and organic acid curing agent, and prepare a preform together with the obtained mixture and the arranged glass fibers; Step 4: introduce the preform into the mold and press it at 220-270°C and 1-15MPa for 45-120min to form it; Furthermore, the organic acid curing agent is one of citric acid, malic acid, quinic acid, and tartaric acid; Further, the composite functional agent is prepared by the following steps: Step 1, dimethyl phosphite, sulfonyl chloride and carbon tetrachloride are mixed in a three-necked flask, and stirred at 45° C. for 2 h; after the reaction is completed, excess sulfonyl chloride and carbon tetrachloride are removed by rotary evaporation to obtain intermediate 1; Step 2, adding phthalic anhydride, toluene, and m-aminophenol into a three-necked flask, stirring for 3 hours, filtering, recrystallizing the obtained solid with 95% by mass ethanol, and drying under reduced pressure, adding the dried product, toluene, and phosphotungstic heteropoly acid into a three-necked flask, stirring, reacting at 100° C. for 4 hours, cooling to room temperature, filtering to remove the phosphotungstic heteropoly acid, and distilling the filtrate under reduced pressure to obtain intermediate 2; Step 3, add intermediate 1 and intermediate 2 and sodium hydroxide solution into a three-necked flask, stir, slowly heat to 70°C, stir and react for 8 hours, cool, add carbon tetrachloride into the three-necked flask, separate the organic layer with a separatory funnel, and obtain intermediate 3 after rotary evaporation; Step 4, adding intermediate 3 and ferric chloride into a stainless steel reactor, stirring, continuously introducing nitrogen into the reactor for protection, heating to 180°C, and then adding benzoyl chloride dropwise with a high-pressure dropping pump 6 times, with an interval of 3 hours between each addition. After the addition is completed, react for another 3 hours, cool, filter to remove ferric chloride, perform acid washing, alkali washing, and layering of the filtrate, remove excess intermediate 3 from the organic phase, and obtain the composite functional agent after distillation; Furthermore, the usage ratio of dimethyl phosphite, sulfonyl chloride and carbon tetrachloride in step 1 is 11g:13.5g:130-150g; Furthermore, the dosage ratio of phthalic anhydride in step 2, toluene added for the first time, m-aminophenol, toluene added for the second time, and phosphotungstic heteropoly acid is 14.8g:144-174g:7.75g:180-217g:2.6-3.1g; Furthermore, the sodium hydroxide solution used in step 3 is a sodium hydroxide aqueous solution with a mass fraction of 45-50%, the amount of which is 35-40 g, and the mass ratio of the intermediate 1 to the intermediate 2 used is 7.2 g:12.8 g; Furthermore, in step 4, the pressure range in the stainless steel reactor is 0.35-0.45 MPa, and the amount ratio of the intermediate 3, ferric chloride, and benzoyl chloride used is 9g:4g:7g.

[0005] Beneficial effects of the present invention: The present invention uses waste glass fiber, bisphenol A diglycidyl ether, ethylene-tetrafluoroethylene copolymer, organic acid curing agent, and composite functional agent as raw materials to prepare a high-performance glass product. The glass product of the present invention is combined with epoxy resin by glass fiber, and the glass after curing and molding has excellent electrical insulation and dimensional stability. Conventional epoxy resin has poor toughness. Therefore, the present invention improves the poor toughness of epoxy resin by uniformly mixing the glass with ethylene-tetrafluoroethylene copolymer during the manufacturing process, and the mechanical properties of the prepared glass are greatly improved. The present invention uses dimethyl phosphite as a raw material and sulfonyl chloride as a halogenating agent to obtain a halogenated intermediate 1 of phosphite, uses phthalic anhydride and meta-aminophenol as raw materials, and uses phosphotungstic heteropoly acid as a catalyst to obtain an intermediate 2 connected with an organic heterocyclic structure, and then allows the intermediate 1 and the intermediate 2 to undergo a nucleophilic substitution reaction in a strong alkaline environment to obtain an intermediate 3, and finally allows benzoyl chloride and the intermediate 3 to react under the catalysis of ferric chloride to obtain a composite functional agent. The benzophenone compound has the ability to absorb ultraviolet light due to the presence of keto / enol isomers in the molecule. The present invention modifies the benzophenone compound, and uses the characteristic that the phosphite forms an isolation film at high temperature to impart flame retardancy to the phosphite compound for the production and application of glass. The organic heterocyclic compound has large cohesive energy and high thermal decomposition temperature to increase the rigidity of the system, improve the thermal properties of the compound, and allow the compound to stably exist under ultraviolet light irradiation, so as to achieve the effect of absorbing ultraviolet light for a long time. Although the composite functional agent finally obtained has multiple isomers, the actual effect is not changed. The glass product of the present invention has good mechanical strength, stable dimensions, and excellent electrical insulation. Due to the addition of the composite functional agent, it can effectively absorb ultraviolet light for a long time, has stable thermal properties, and can form an isolation film in the event of a fire to protect property and personal safety. It can be widely used in the fields of automobiles, buildings, electronic components, touch panels, etc. DETAILED DESCRIPTION

[0006] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0007] Example 1 The composite functional agent is prepared by the following steps: Step 1, 11 g of dimethyl phosphite, 13.5 g of sulfuryl chloride, and 130 g of carbon tetrachloride are mixed in a container, and stirred at 45° C. for 2 h; after the reaction is completed, excess sulfuryl chloride and carbon tetrachloride are removed by rotary evaporation to obtain intermediate 1; Step 2, add 14.8g of phthalic anhydride, 144g of toluene, and 7.75g of m-aminophenol into a container, stir for 3h, filter, recrystallize the obtained solid with 95% by mass ethanol, dry under reduced pressure, add the dried product, 180g of toluene, and 2.6g of phosphotungstic heteropoly acid into a container, stir, react at 100°C for 4h, cool to room temperature, filter to remove the phosphotungstic heteropoly acid, and distill the filtrate under reduced pressure to obtain intermediate 2; Step 3, add 7.2 g of intermediate 1, 12.8 g of intermediate 2 and 35 g of 45% by mass sodium hydroxide solution into a container, stir, slowly heat to 70°C, stir and react for 8 hours, cool, add carbon tetrachloride into the container, separate the organic layer with a separatory funnel, and obtain intermediate 3 after rotary evaporation; Step 4, add 9g of intermediate 3 and 4g of ferric chloride into a container, stir, continuously introduce nitrogen into the container for protection, control the pressure in the container to 0.35MPa, heat to 180°C and then add 7g of benzoyl chloride dropwise thereto in 6 times, with an interval of 3h between each addition. After the addition is completed, react for another 3h, cool and filter to remove ferric chloride, perform acid washing, alkali washing, and layering of the filtrate, remove excess intermediate 3 from the organic phase, and obtain the composite functional agent after distillation.

[0008] Example 2 The composite functional agent is prepared by the following steps: Step 1, 11 g of dimethyl phosphite, 13.5 g of sulfuryl chloride, and 140 g of carbon tetrachloride are mixed in a container, and stirred at 45° C. for 2 h; after the reaction is completed, excess sulfuryl chloride and carbon tetrachloride are removed by rotary evaporation to obtain intermediate 1; Step 2, add 14.8g of phthalic anhydride, 160g of toluene, and 7.75g of m-aminophenol into a container, stir for 3h, filter, recrystallize the obtained solid with 95% by mass ethanol, dry under reduced pressure, add the dried product, 200g of toluene, and 2.8g of phosphotungstic heteropoly acid into a container, stir, react at 100°C for 4h, cool to room temperature, filter to remove the phosphotungstic heteropoly acid, and distill the filtrate under reduced pressure to obtain intermediate 2; Step 3, add 7.2 g of intermediate 1, 12.8 g of intermediate 2 and 37 g of 47% sodium hydroxide solution into a container, stir, slowly heat to 70°C, stir and react for 8 hours, cool, add carbon tetrachloride into the container, separate the organic layer with a separatory funnel, and obtain intermediate 3 after rotary evaporation; Step 4, add 9g of intermediate 3 and 4g of ferric chloride into a container, stir, continuously introduce nitrogen into the container for protection, control the pressure in the container to 0.40MPa, heat to 180°C and then add 7g of benzoyl chloride dropwise thereto in 6 times, with an interval of 3h between each addition. After the addition is completed, react for another 3h, cool and filter to remove ferric chloride, perform acid washing, alkali washing, and layering of the filtrate, remove excess intermediate 3 from the organic phase, and obtain the composite functional agent after distillation.

[0009] Example 3 The composite functional agent is prepared by the following steps: Step 1, 11 g of dimethyl phosphite, 13.5 g of sulfonyl chloride, and 150 g of carbon tetrachloride are mixed in a container, and stirred at 45° C. for 2 h; after the reaction is completed, excess sulfonyl chloride and carbon tetrachloride are removed by rotary evaporation to obtain intermediate 1; Step 2, add 14.8g of phthalic anhydride, 174g of toluene, and 7.75g of m-aminophenol into a container, stir for 3h, filter, recrystallize the obtained solid with 95% by mass ethanol, dry under reduced pressure, add the dried product, 217g of toluene, and 3.1g of phosphotungstic heteropoly acid into a container, stir, react at 100°C for 4h, cool to room temperature, filter to remove the phosphotungstic heteropoly acid, and distill the filtrate under reduced pressure to obtain intermediate 2; Step 3, add 7.2g of intermediate 1 and 12.8g of intermediate 2 and 40g of 50% by mass sodium hydroxide solution into a container, stir, slowly heat to 70°C, react for 8h, cool, add carbon tetrachloride into a three-necked flask, separate the organic layer with a separatory funnel, and obtain intermediate 3 after rotary evaporation; Step 4, add 9g of intermediate 3 and 4g of ferric chloride into a container, stir, continuously introduce nitrogen into the container for protection, control the pressure in the container to 0.45MPa, heat to 180°C and then add 7g of benzoyl chloride dropwise thereto in 6 times, with an interval of 3h between each addition. After the addition is completed, react for another 3h, cool and filter to remove ferric chloride, perform acid washing, alkali washing, and layering of the filtrate, remove excess intermediate 3 from the organic phase, and obtain the composite functional agent after distillation.

[0010] Comparative Example 1 This comparative example is a UV absorber sold by Tianjin Lianlong New Materials Co., Ltd.; The composite functional agent obtained in Example 1, Example 2 and Example 3 was tested for ultraviolet absorption performance with the ultraviolet absorber sold by Tianjin Lianlong New Materials Co., Ltd., and 8g was taken and evenly added to 92g of epoxy resin to make epoxy resin cured plates, wherein the epoxy resin cured plate with Example 1 added was No. 1, the epoxy resin cured plate with Example 2 added was No. 2, the epoxy resin cured plate with Example 3 added was No. 3, the epoxy resin cured plate with the ultraviolet absorber sold by Tianjin Lianlong New Materials Co., Ltd. added was No. 4, and the epoxy resin cured plate without any substance added was the blank control group, and 300W ultraviolet light was emitted to the above 5 groups, and the discoloration of each group of epoxy cured plates was observed after ultraviolet irradiation for 24 hours, and the ultraviolet irradiation was 72 hours. Re-observe each group of epoxy cured plates, and the final results are shown in Table 1: Table 1 It can be seen from Table 1 that the ultraviolet absorption effect of Example 1, Example 2, and Example 3 within 24 hours is greater than that of Comparative Example 1, and the long-term absorption effect of ultraviolet rays is much greater than that of Comparative Example 1, indicating that the composite functional agent prepared by the present invention not only has excellent ultraviolet absorption capacity, but also can stably and continuously exert its effect under long-term ultraviolet irradiation.

[0011] Example 4 A high-performance glass product, comprising the following raw materials in parts by weight: 55 parts of waste glass fiber, 18 parts of bisphenol A diglycidyl ether, 5 parts of ethylene-tetrafluoroethylene copolymer, 6 parts of quinic acid, and 6 parts of a composite functional agent; A method for preparing a glass-based composite material comprises the following steps: Step 1: Screen the waste glass fibers, wash them, treat them at 240°C for 35 minutes, and stretch them; Step 2: Cut the stretched glass fiber into 30 cm strips and dry them; Step 3: Fully mix bisphenol A diglycidyl ether epoxy resin, ethylene-tetrafluoroethylene copolymer, composite functional agent, and quinic acid, and prepare a preform together with the obtained mixture and the glass fiber of the arrangement number; Step 4: introducing the preform into a mold, and pressing for 45 minutes under the conditions of 220° C. and 1 MPa to obtain the high-performance glass product.

[0012] Example 5 A high-performance glass product, comprising the following raw materials in parts by weight: 57 parts of waste glass fiber, 19 parts of bisphenol A diglycidyl ether, 9 parts of ethylene-tetrafluoroethylene copolymer, 6 parts of malic acid, and 9 parts of a composite functional agent; A method for preparing a glass-based composite material comprises the following steps: Step 1: Screen the waste glass fibers, wash them, treat them at 260°C for 40 minutes, and stretch them; Step 2: Cut the stretched glass fiber into 40 cm strips and dry them; Step 3: Fully mix the glass fiber, bisphenol A diglycidyl ether epoxy resin, ethylene-tetrafluoroethylene copolymer, composite functional agent, and malic acid to form a preform together with the glass fiber; Step 3: introducing the preform into a mold, and pressing at 250° C. and 8 MPa for 85 min to obtain the high-performance glass product.

[0013] Example 6 A high-performance glass product, comprising the following raw materials in parts by weight: 60 parts of waste glass fiber, 18 parts of bisphenol A diglycidyl ether, 6 parts of ethylene-tetrafluoroethylene copolymer, 6 parts of tartaric acid, and 10 parts of a composite functional agent; A method for preparing a glass-based composite material comprises the following steps: Step 1: Screen the waste glass fibers, wash them, treat them at 280°C for 45 minutes, and stretch them; Step 2: Cut the stretched glass fiber into 50 cm strips and dry them; Step 3: Fully mix bisphenol A diglycidyl ether epoxy resin, ethylene-tetrafluoroethylene copolymer, composite functional agent and tartaric acid, and prepare a preform together with the obtained mixture and the arranged glass fibers; Step 3: introducing the preform into a mold, and pressing at 270° C. and 15 MPa for 120 min to obtain the high-performance glass product.

[0014] Comparative Example 2 The composite functional agent in Example 4 was removed, and the other raw materials and preparation process remained unchanged.

[0015] Comparative Example 3 This comparative example is a vacuum-introduced carbon fiber and glass fiber composite resin board sold by Shijiazhuang Yinhupo New Material Technology Co., Ltd.; The fire resistance limit test was carried out on Example 4, Example 5, Example 6, Comparative Example 2 and Comparative Example 3 of the same thickness, and the fire resistance limit temperature was recorded. The test results are shown in Table 2: Table 2 The impact resistance test was carried out, and the fracture area and impact energy were recorded. The test results are shown in Table 3: Table 3 It can be seen from Table 2 that the glasses of Example 4, Example 5 and Example 6 not only have a fire resistant temperature much higher than that of Comparative Example 2 and Comparative Example 3, but can also form an isolation film at high temperature to prevent combustion. It can be seen from Table 3 that the impact strength of Example 4, Example 5, Example 6 and Comparative Example 2 is much higher than that of Comparative Example 3, indicating that the glass of the present invention has excellent mechanical strength, thermal stability and flame retardancy, and can be widely used in the fields of automobiles, construction, electronic components, touch panels, etc.

[0016] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A high-performance glass product, characterized in that: The invention comprises the following raw materials in parts by weight: 55-60 parts of waste glass fiber, 18-23 parts of bisphenol A diglycidyl ether, 5-10 parts of ethylene-tetrafluoroethylene copolymer, 6-7 parts of organic acid curing agent, and 6-10 parts of composite functional agent; Wherein, the composite functional agent is prepared by following steps: Step 1, dimethyl phosphite, sulfuryl chloride and carbon tetrachloride are mixed in a container, and reacted at 45° C. for 2 h to obtain intermediate 1; Step 2, adding phthalic anhydride, toluene, and m-aminophenol into a container, stirring for 3 hours, filtering the obtained product, stirring with toluene and phosphotungstic heteropoly acid, and reacting at 100° C. for 4 hours to obtain intermediate 2; Step 3, adding intermediate 1 and intermediate 2 and sodium hydroxide solution into a container, slowly heating to 70° C., stirring and reacting for 8 hours to obtain intermediate 3; Step 4, add intermediate 3 and ferric chloride into a container, continue to introduce inert gas protection into the reactor, heat to 180°C and then add benzoyl chloride dropwise therein in batches, with an interval of 3 hours between each addition. After the addition is completed, react for another 3 hours to obtain the composite functional agent.

2. A high performance glass product according to claim 1, characterized in that: The usage ratio of dimethyl phosphite, sulfonyl chloride and carbon tetrachloride in step 1 is 11g:13.5g:130-150g.

3. A high performance glass product according to claim 1, characterized in that: The dosage ratio of phthalic anhydride in step 2, toluene added for the first time, m-aminophenol, toluene added for the second time, and phosphotungstic heteropoly acid is 14.8g:144-174g:7.75g:180-217g:2.6-3.1g.

4. The high performance glass product according to claim 1, characterized in that: The sodium hydroxide solution used in step 3 is a sodium hydroxide aqueous solution with a mass fraction of 45-50%, and its dosage is 35-40g. The dosage ratio of the intermediate 1 and the intermediate 2 used is 7.2g:12.8g.

5. The high performance glass product according to claim 1, characterized in that: The pressure range in the container in step 4 is 0.35-0.45 MPa, and the amount ratio of the intermediate 3, ferric chloride and benzoyl chloride used is 9g:4g:7g.

6. A method for preparing a glass-based composite material, characterized in that: The production of glass products includes the following steps: Step 1: Screening, weighing, cleaning, heat treating and stretching the waste glass fibers; Step 2: Cut the stretched glass fiber and dry it; Step 3: Fully mix bisphenol A diglycidyl ether epoxy resin, ethylene-tetrafluoroethylene copolymer, composite functional agent, and organic acid curing agent, and prepare a preform together with the obtained mixture and the arranged glass fibers; Step 4: The preform is introduced into a mold for compression molding.

7. The method for preparing a glass-based composite material according to claim 6, characterized in that: In step 1, the temperature condition of the heat treatment is 240-280° C., and the time condition of the heat treatment is 35-45 min.

8. The method for preparing a glass-based composite material according to claim 6, characterized in that: The standard length of glass fiber cut in step 2 is 30-50cm.

9. The method for preparing a glass-based composite material according to claim 6, characterized in that: The organic acid curing agent used in step 3 is one of citric acid, malic acid, quinic acid and tartaric acid.

10. The method for preparing a glass-based composite material according to claim 6, characterized in that: In step 4, the preform is pressed at a temperature of 220-270° C., at a pressure of 1-15 MPa, and for a time of 45-120 min.

Citation Information

Patent Citations

  • Glass reinforced plastic composite coating material with good anti-corrosion effect and preparation method thereof

    CN103773090A

  • Glass fiber reinforced plastic panel material for power cabinet of power distribution station and preparation method of glass fiber reinforced plastic panel material

    CN107090162A

  • Corrosion-resistant glass fiber reinforced plastic composite material, and preparation method thereof

    CN110467788A

  • Resin composition, and prepreg and copper-clad plate prepared from same

    CN113583383A

  • Thrust knuckle bearing and preparation method thereof

    CN114085493A