Insulating oil-resistant coating for storage tank and preparation method of insulating oil-resistant coating

Through the combination of modified basalt fiber and modified water-based epoxy resin, polyurea nanofibers are formed, which solves the problems of insufficient insulation performance, oil-resistant strength and anti-corrosion and wear resistance of existing insulating oil-resistant coatings, and achieves high-performance insulating and oil-resistant coatings. Coating, suitable for protection of storage tank environment.

CN118745313APending Publication Date: 2024-10-08QINGDAO ZHONGFU FLUOROCARBON MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411012088.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing insulating oil-resistant coatings have shortcomings in insulation performance, oil-resistant strength, and anti-corrosion and wear-resistance properties, especially in storage tank environments, which are difficult to meet the high protection needs.

Method used

Using modified basalt fiber and modified water-based epoxy resin as the main components, acid treatment and ultrasonic suspension technology are used to increase the roughness and reaction sites of the fiber surface, and polyurea nanofibers are formed through addition polymerization, combined with water-based epoxy Resin curing agent and additives form high-performance insulating and oil-resistant coatings.

Benefits of technology

Significantly improves the insulation performance, anti-corrosion and wear resistance, oil resistance and chemical stability of the coating, forming a high-strength and durable coating that can effectively prevent corrosion and wear in the storage tank environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964677870000121
    Figure BDA0004964677870000121
Patent Text Reader

Abstract

The invention discloses an insulating oil-resistant coating for a storage tank and a preparation method of the insulating oil-resistant coating. The insulating oil-resistant coating for the storage tank is prepared from the following raw materials in parts by weight: 10 to 20 parts of modified basalt fiber, 70 to 90 parts of modified water-borne epoxy resin, 2 to 4 parts of an auxiliary agent, 80 to 160 parts of water and 10 to 30 parts of a water-borne epoxy resin curing agent. Compared with the prior art, the insulating oil-resistant coating for the storage tank prepared by the invention has the advantages of good insulating property, high oil-resistant strength, high corrosion-resistant and wear-resistant strength and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to an insulating oil-resistant coating for a storage tank and a preparation method thereof. Background Art

[0002] At present, the application areas of coatings are mainly concentrated in the following aspects: environmental sustainability, smart coatings, nanotechnology, digital technology, self-healing technology and multifunctional coatings. Among them, multifunctional coatings have special properties such as corrosion resistance, fire resistance, conductivity or insulation. In addition to coatings for single-functional environments, they also include composite functions. In this field, insulating oil-resistant coatings are one of the special coatings worthy of attention. They can meet people's demand for functional diversification and also promote the development of the coatings industry towards composite innovation and sustainability.

[0003] CN117487460A discloses an insulating coating with good dielectric properties and a preparation method thereof, wherein the insulating properties are improved by adding epoxy-modified silicone resin. The direct addition of wear-resistant particles to the insulating coating prepared by the method may cause the coating to delaminate. CN117683432A discloses a fast-drying thick slurry water-based epoxy two-component anticorrosive coating and a preparation method thereof, wherein the fast-drying properties of the coating are improved by adding modified sepiolite and modified basalt fiber. The modified basalt fiber and mica powder-modified sepiolite components added by the method are relatively independent and cannot form a cross-linked network structure. Summary of the invention

[0004] In view of the above-mentioned defects of the prior art, the object of the present invention is to provide an insulating oil-resistant coating for storage tanks, which has good insulation performance, high oil resistance and high corrosion resistance.

[0005] To achieve the above object, the present invention provides an insulating oil-resistant coating for a storage tank and a preparation method thereof.

[0006] The detailed technical scheme of the present invention is as follows:

[0007] The present invention provides an insulating oil-resistant coating for a storage tank, comprising the following raw materials:

[0008] By mass, the modified basalt fiber is 10-20 parts, the modified water-based epoxy resin is 70-90 parts, the auxiliary agent is 2-4 parts, the water is 80-160 parts, and the water-based epoxy resin curing agent is 10-30 parts.

[0009] The modified basalt fiber is prepared by the following method: by weight:

[0010] (1) Weighing 5-15 parts of chopped basalt fibers, adding them to 400-600 parts of 5-15wt% hydrochloric acid, stirring at 600-800 rpm and room temperature for 16-24 hours, then ultrasonically cleaning them in anhydrous ethanol for 10-30 minutes, filtering, and drying the filter cake at 40-60° C. for later use to obtain acid-treated chopped basalt fibers;

[0011] (2) ultrasonically dissolving 5-15 parts of octadecylamine and 3-8 parts of cyclohexylamine in 150-300 parts of anhydrous ethanol; adding 5-15 parts of the acid-treated chopped basalt fibers of step (1), and then stirring at 40-60° C. and 800-1200 rpm for 20-40 min, removing the basalt fibers and placing them in 100-300 parts of water and continuing to stir to obtain a basalt fiber suspension;

[0012] (3) dissolving 15-20 parts of 4,4'-methylenebis(phenyl isocyanate) in 200-400 parts of ethyl acetate, and then slowly dropping it into the basalt fiber suspension of step (2) within 40-80 minutes. After the dropping is completed, the temperature of the mixed solution is raised to 70-90°C. After reacting for 4-6 hours, the basalt fiber is fished out and dried at 40-60°C for 4-6 hours to obtain the modified basalt fiber.

[0013] As a further illustration of the present invention: the acid-treated chopped basalt fibers can increase the roughness of the fiber surface and increase the reaction sites. Placing the fibers in octadecylamine and cyclohexylamine can attach amino chemical functional groups to the surface of the acid-treated chopped basalt fibers, and react with 4,4'-methylenebis(phenyl isocyanate) to form polyurea nanofibers that wrap the basalt fibers.

[0014] The modified waterborne epoxy resin is prepared by the following method: by weight:

[0015] S1: Dissolve 5-10 parts of 2-aminoethanesulfonic acid in 100-200 parts of water, and add 30-40 wt% NaOH aqueous solution to adjust the pH to 8-10;

[0016] S2: Add 10-15 parts of epoxy resin and 1-3 parts of phase transfer catalyst to 20-40 parts of water, stir at 60-80°C and 800-1200 rpm for 5-10 min, then add to the solution obtained in step S1 and react for 6-8 h.

[0017] As a further illustration of the present invention: 2-aminoethanesulfonic acid can introduce hydrophilic sulfonic acid groups on the main chain of epoxy resin.

[0018] The auxiliary agent is at least one of a defoamer, a dispersant, and an antioxidant. Preferably, the defoamer is at least one of polydimethylsiloxane, polyoxyethylene, and polyacrylate.

[0019] Preferably, the dispersant is at least one of tributyl phosphate, polyoxyethylene, polydimethylsiloxane and polyvinyl pyrrolidone.

[0020] Preferably, the antioxidant is at least one of bis(2,4-di-tert-butylphenyl) disulfide and 2-mercaptobenzothiazole.

[0021] The waterborne epoxy resin curing agent is at least one of polyetheramine and waterborne amine curing agent.

[0022] The present invention provides a method for preparing an insulating oil-resistant coating for a storage tank, and the preparation method is as follows:

[0023] Step 1: Ultrasonic disperse 10-20 parts of modified basalt fiber in 40-80 parts of water, then add 70-90 parts of modified waterborne epoxy resin, stir evenly and set aside;

[0024] Step 2: Mix 10-30 parts of waterborne epoxy resin curing agent, 2-4 parts of auxiliary agent and 40-80 parts of water and stir evenly for later use;

[0025] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain the insulating oil-resistant coating for the storage tank.

[0026] Beneficial effects of the present invention:

[0027] Compared with the existing technology, modified basalt fiber and modified water-based epoxy resin are used in the coating. These ingredients work together to improve the insulation performance, corrosion resistance, wear resistance, oil resistance and chemical stability of the coating. DETAILED DESCRIPTION

[0028] Insulating oil-resistant coating for storage tanks, including the following raw materials:

[0029] By mass, the modified basalt fiber is 10-20 parts, the modified water-based epoxy resin is 70-90 parts, the auxiliary agent is 2-4 parts, the water is 80-160 parts, and the water-based epoxy resin curing agent is 10-30 parts.

[0030] The modified basalt fiber is prepared by the following method: by weight:

[0031] (1) Weighing 5-15 parts of chopped basalt fibers, adding them to 400-600 parts of 5-15wt% hydrochloric acid, stirring at 600-800 rpm and room temperature for 16-24 hours, then ultrasonically cleaning them in anhydrous ethanol for 10-30 minutes, filtering, and drying the filter cake at 40-60° C. for later use to obtain acid-treated chopped basalt fibers;

[0032] (2) ultrasonically dissolving 5-15 parts of octadecylamine and 3-8 parts of cyclohexylamine in 150-300 parts of anhydrous ethanol; adding 5-15 parts of the acid-treated chopped basalt fibers of step (1), and then stirring at 40-60° C. and 800-1200 rpm for 20-40 min, removing the basalt fibers and placing them in 100-300 parts of water and continuing to stir to obtain a basalt fiber suspension;

[0033] (3) Dissolve 15-20 parts of 4,4'-methylenebis(phenyl isocyanate) in 200-400 parts of ethyl acetate, and then slowly add it dropwise to the basalt fiber suspension of step (2) within 40-80 minutes. After the addition is completed, raise the temperature of the mixed solution to 70-90°C. After reacting for 4-6 hours, remove the basalt fiber and dry it at 40-60°C for 4-6 hours to obtain the modified basalt fiber.

[0034] The modified basalt fiber retains the excellent physical and chemical properties of basalt fiber and can improve the mechanical properties of the coating. Stirring and soaking basalt fiber in hydrochloric acid solution can remove the surface oxide layer and impurities, increase the surface roughness of the fiber and increase the reaction sites. Add octadecylamine and cyclohexylamine and stir to attach amino chemical functional groups to its surface. Then add 4,4'-methylenebis(phenyl isocyanate) and use addition polymerization to achieve in-situ growth of polyurea nanofibers on the surface of basalt fiber.

[0035] The modified waterborne epoxy resin is prepared by the following method: by weight:

[0036] S1: Dissolve 5-10 parts of 2-aminoethanesulfonic acid in 100-200 parts of water, and add 30-40 wt% NaOH aqueous solution to adjust the pH to 8-10;

[0037] S2: Add 10-15 parts of epoxy resin and 1-3 parts of phase transfer catalyst to 20-40 parts of water, stir at 60-80°C, 800-1200 rpm for 5-10 min, then add S1 and react for 6-8 hours to obtain the product.

[0038] The obtained modified waterborne epoxy resin has good hydrophilicity, small particle size and good dispersion effect of the colloid particles. The colloid particles have a regular spherical structure and can be in a nano-dispersed state. The colloid solution remains stable after long-term placement.

[0039] The auxiliary agent is at least one of a defoamer, a dispersant, and an antioxidant. Preferably, the defoamer is at least one of polydimethylsiloxane, polyoxyethylene, and polyacrylate.

[0040] Preferably, the dispersant is at least one of tributyl phosphate, polyoxyethylene, polydimethylsiloxane and polyvinyl pyrrolidone.

[0041] Preferably, the antioxidant is at least one of bis(2,4-di-tert-butylphenyl) disulfide and 2-mercaptobenzothiazole.

[0042] The water-based epoxy resin curing agent is at least one of polyetheramine, polyethanolamine and water-based amine curing agents.

[0043] The present invention provides a method for preparing an insulating oil-resistant coating for a storage tank, and the preparation method is as follows:

[0044] Step 1: Ultrasonic disperse 10-20 parts of modified basalt fiber in 40-80 parts of water, then add 70-90 parts of modified waterborne epoxy resin, stir evenly and set aside;

[0045] Step 2: Mix 10-30 parts of waterborne epoxy resin curing agent, 2-4 parts of auxiliary agent and 40-80 parts of water and stir evenly for later use;

[0046] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain the insulating oil-resistant coating for the storage tank.

[0047] The sources and parameters of some chemical substances in the examples are as follows:

[0048] Chopped basalt fiber, with a single fiber diameter of 5.5μm to 25μm and a length of 6mm to 100mm, comes from Jiangsu Tianlong Basalt Continuous Fiber Co., Ltd.

[0049] 4,4'-Methylenebis(phenyl isocyanate), referred to as MDI in English, CAS number: 101-68-8.

[0050] Polyetheramine D230, CAS number: 9046-10-0.

[0051] Bisphenol A epoxy resin, model E51, epoxy equivalent 183 ~ 190g / eq, viscosity (25 ℃) 10000 ~ 14000mPa.s, source Guangzhou Wei Chuang High-tech Materials Technology Co., Ltd.

[0052] SH-201-1000 dimethyl silicone oil, viscosity 1000±50cs, comes from Shanghai Chuyijia Silicone Materials Co., Ltd.

[0053] Nano-silicon dioxide, purity > 99.5%, average particle size 30 ± 5nm, comes from Chengdu Huaxia Chemical Reagent Co., Ltd.

[0054] N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, purity 97%, CAS number: 1760-24-3, from Shanghai Myrel Biochemical Technology Co., Ltd.

[0055] Example 1

[0056] A method for preparing an insulating oil-resistant coating for a storage tank comprises the following steps:

[0057] Step 1: Ultrasonic disperse 10g of modified basalt fiber in 60g of water, then add 90g of modified waterborne epoxy resin, stir evenly and set aside;

[0058] Step 2: Mix 30g of water-based epoxy resin curing agent, 2g of auxiliary agent and 60g of water and stir evenly for later use;

[0059] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain the insulating oil-resistant coating for the storage tank.

[0060] The modified basalt fiber in step 1 is prepared by the following method:

[0061] (1) Weighing 10 g of chopped basalt fibers, adding them to 400 g of 15 wt% hydrochloric acid, stirring at 600 rpm and room temperature for 24 h, then ultrasonically cleaning them in anhydrous ethanol for 30 min, filtering, and drying the filter cake at 50° C. for later use to obtain acid-treated chopped basalt fibers;

[0062] (2) dissolving 11 g of octadecylamine and 4 g of cyclohexylamine in 300 g of anhydrous ethanol by ultrasonication; adding 10 g of the acid-treated chopped basalt fibers of step (1); stirring at 50° C. and 800 rpm for 30 min, removing the basalt fibers and placing them in 100 g of water and continuing to stir to obtain a basalt fiber suspension;

[0063] (3) 15 g of 4,4'-methylenebis(phenyl isocyanate) was dissolved in 400 g of ethyl acetate, and then slowly added dropwise to the basalt fiber suspension of step (2) within 60 min. After the addition was completed, the temperature of the mixed solution was raised to 80° C. After reacting for 4 h, the basalt fiber was removed and dried at 50° C. for 4 h to obtain the modified basalt fiber.

[0064] The modified waterborne epoxy resin in step 1 is prepared by the following method:

[0065] S1: Dissolve 10 g of 2-aminoethanesulfonic acid in 100 g of water, and add 40 wt % NaOH aqueous solution to adjust the pH to 9;

[0066] S2: Add 10 g of bisphenol A epoxy resin and 1 g of tetrabutylammonium bromide into 40 g of water, stir at 80° C. and 800 rpm for 5 min, then add into the solution obtained in step S1 and react for 6 h.

[0067] The auxiliary agent is dispersant SH-201-1000 dimethyl silicone oil.

[0068] The waterborne epoxy resin curing agent is polyetheramine D230.

[0069] Example 2

[0070] A method for preparing an insulating oil-resistant coating for a storage tank comprises the following steps:

[0071] Step 1: Ultrasonic disperse 10g of modified basalt fiber in 60g of water, then add 90g of modified waterborne epoxy resin, stir evenly and set aside;

[0072] Step 2: Mix 30g of water-based epoxy resin curing agent, 2g of auxiliary agent and 60g of water and stir evenly for later use;

[0073] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain the insulating oil-resistant coating for the storage tank.

[0074] The modified basalt fiber in step 1 is prepared by the following method:

[0075] (1) Dissolve 11 g of octadecylamine and 4 g of cyclohexylamine in 300 g of anhydrous ethanol by ultrasonication. Weigh 10 g of basalt fiber and add it to the above solution. Then, stir at 50°C and 800 rpm for 30 min, remove the basalt fiber and place it in 100 g of water and continue stirring to obtain a basalt fiber suspension.

[0076] (2) 15 g of 4,4'-methylenebis(phenyl isocyanate) was dissolved in 400 g of ethyl acetate, and then slowly added dropwise to the basalt fiber suspension of step (1) within 60 min. After the addition was completed, the temperature of the mixed solution was raised to 80° C. After reacting for 4 h, the basalt fiber was removed and dried at 50° C. for 4 h to obtain the modified basalt fiber.

[0077] The modified waterborne epoxy resin in step 1 is prepared by the following method:

[0078] S1: Dissolve 10 g of 2-aminoethanesulfonic acid in 100 g of water, and add 40 wt % NaOH aqueous solution to adjust the pH to 9;

[0079] S2: Add 10 g of bisphenol A epoxy resin and 1 g of tetrabutylammonium bromide into 40 g of water, stir at 80° C. and 800 rpm for 5 min, and then add the mixture into the solution obtained in step S1 and react for 6 h to obtain the product.

[0080] The auxiliary agent is dispersant SH-201-1000 dimethyl silicone oil.

[0081] The waterborne epoxy resin curing agent is polyetheramine D230.

[0082] Example 3

[0083] A method for preparing an insulating oil-resistant coating for a storage tank comprises the following steps:

[0084] Step 1: Ultrasonic disperse 10g of basalt fiber in 60g of water, then add 90g of modified waterborne epoxy resin, stir evenly and set aside;

[0085] Step 2: Mix 30g of water-based epoxy resin curing agent, 2g of auxiliary agent and 60g of water and stir evenly for later use;

[0086] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain the insulating oil-resistant coating for the storage tank.

[0087] The modified waterborne epoxy resin in step 1 is prepared by the following method:

[0088] S1: Dissolve 10 g of 2-aminoethanesulfonic acid in 100 g of water, and add 40 wt % NaOH aqueous solution to adjust the pH to 9;

[0089] S2: Add 10 g of bisphenol A epoxy resin and 1 g of tetrabutylammonium bromide into 40 g of water, stir at 80° C. and 800 rpm for 5 min, then add into the solution obtained in step S1 and react for 6 h.

[0090] The auxiliary agent is dispersant SH-201-1000 dimethyl silicone oil.

[0091] The waterborne epoxy resin curing agent is polyetheramine D230.

[0092] Example 4

[0093] A method for preparing an insulating oil-resistant coating for a storage tank comprises the following steps:

[0094] Step 1: Ultrasonic disperse 10g of modified basalt fiber in 60g of water, then add 90g of bisphenol A epoxy resin, stir evenly and set aside;

[0095] Step 2: Mix 30g of water-based epoxy resin curing agent, 2g of auxiliary agent and 60g of water and stir evenly for later use;

[0096] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain the insulating oil-resistant coating for the storage tank.

[0097] The modified basalt fiber in step 1 is prepared by the following method:

[0098] (1) Weighing 10 g of chopped basalt fibers, adding them to 400 g of 15 wt% hydrochloric acid, stirring at 600 rpm at room temperature for 24 h, then ultrasonically cleaning them in anhydrous ethanol for 30 min, filtering, and drying the filter cake at 50° C. for later use to obtain acid-treated chopped basalt fibers;

[0099] (2) dissolving 11 g of octadecylamine and 4 g of cyclohexylamine in 300 g of anhydrous ethanol by ultrasonication; adding 10 g of the acid-treated chopped basalt fibers of step (1); stirring at 50° C. and 800 rpm for 30 min, removing the basalt fibers and placing them in 100 g of water and continuing to stir to obtain a basalt fiber suspension;

[0100] (3) 15 g of 4,4'-methylenebis(phenyl isocyanate) was dissolved in 400 g of ethyl acetate, and then slowly added dropwise to the basalt fiber suspension of step (2) within 60 min. After the addition was completed, the temperature of the mixed solution was raised to 80° C. After reacting for 4 h, the basalt fiber was removed and dried at 50° C. for 4 h to obtain the modified basalt fiber.

[0101] The auxiliary agent is dispersant SH-201-1000 dimethyl silicone oil.

[0102] The waterborne epoxy resin curing agent is polyetheramine D230.

[0103] Example 5

[0104] A method for preparing an insulating oil-resistant coating for a storage tank comprises the following steps:

[0105] Step 1: Ultrasonic disperse 10g of basalt fiber in 60g of water, then add 90g of bisphenol A epoxy resin, stir evenly and set aside;

[0106] Step 2: Mix 30g of water-based epoxy resin curing agent, 2g of auxiliary agent and 60g of water and stir evenly for later use;

[0107] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain the insulating oil-resistant coating for the storage tank.

[0108] The auxiliary agent is dispersant SH-201-1000 dimethyl silicone oil.

[0109] The waterborne epoxy resin curing agent is polyetheramine D230.

[0110] Example 6

[0111] A method for preparing an insulating oil-resistant coating for a storage tank comprises the following steps:

[0112] Step 1: Ultrasonic disperse 10g of modified nanopowder in 60g of water, then add 90g of modified waterborne epoxy resin, stir evenly and set aside;

[0113] Step 2: Mix 30g of water-based epoxy resin curing agent, 2g of auxiliary agent and 60g of water and stir evenly for later use;

[0114] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain the insulating oil-resistant coating for the storage tank.

[0115] The modified nano powder in step 1 is prepared by the following method:

[0116] 20 g of nano-silica was added to 200 g of a 40 wt% ethylene glycol aqueous solution and then mixed and then subjected to 60 kHz ultrasonic dispersion for 30 min. During the dispersion process, 10 g of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane was added to modify the nano-silica to obtain a modified nano-silica mixed dispersion. The dispersion was dried at 80° C. for 8 h, and the dried nano-silica was added to a mortar for grinding and then passed through a 100-mesh sieve to obtain a modified nano-silica mixed dispersion.

[0117] The modified waterborne epoxy resin in step 1 is prepared by the following method:

[0118] S1: Dissolve 10 g of 2-aminoethanesulfonic acid in 100 g of water, and add 40 wt % NaOH aqueous solution to adjust the pH to 9;

[0119] S2: Add 10 g of bisphenol A epoxy resin and 1 g of tetrabutylammonium bromide into 40 g of water, stir at 80° C. and 800 rpm for 5 min, then add into the solution obtained in step S1 and react for 6 h.

[0120] The auxiliary agent is dispersant SH-201-1000 dimethyl silicone oil.

[0121] The waterborne epoxy resin curing agent is polyetheramine D230.

[0122] Example 7

[0123] A method for preparing an insulating oil-resistant coating for a storage tank comprises the following steps:

[0124] Step 1: Ultrasonic disperse 10g of graphene / modified polystyrene in 60g of water, then add 90g of modified waterborne epoxy resin, stir evenly and set aside;

[0125] Step 2: Mix 30g of water-based epoxy resin curing agent, 2g of auxiliary agent and 60g of water and stir evenly for later use;

[0126] Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain the insulating oil-resistant coating for the storage tank.

[0127] The graphene / modified polystyrene described in step 1 is prepared by the following method:

[0128] (1) Preparation of polystyrene dispersion: 0.1 g of octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate was added to 80 g of water in a three-necked flask equipped with a stirrer and a water bath, and stirred for 10 min until a uniform solution was formed; then the temperature was raised to 60° C., 0.1 g of initiator potassium persulfate was added, and after the initiator was dissolved, 1 g of styrene monomer was slowly added, and the temperature was raised to 70° C., and the reaction was maintained at 300 rpm for 2 h under insulation conditions to obtain a polystyrene dispersion;

[0129] (2) Preparation of graphene / modified polystyrene: 0.1 g of N,N'-methylenebisacrylamide was added to a beaker containing 20 g of water, heated to 50°C and stirred until dissolved, then added to the polystyrene dispersion and reacted at 70°C for 4 h.

[0130] The modified waterborne epoxy resin in step 1 is prepared by the following method:

[0131] S1: Dissolve 10 g of 2-aminoethanesulfonic acid in 100 g of water, and add 40 wt % NaOH aqueous solution to adjust the pH to 9;

[0132] S2: Add 10 g of bisphenol A epoxy resin and 1 g of tetrabutylammonium bromide into 40 g of water, stir at 80° C. and 800 rpm for 5 min, then add into the solution obtained in step S1 and react for 6 h.

[0133] The auxiliary agent is dispersant SH-201-1000 dimethyl silicone oil.

[0134] The waterborne epoxy resin curing agent is polyetheramine D230.

[0135] Test Example 1

[0136] The insulation oil-resistant coatings for storage tanks with different formulations were tested for the following properties, and the results are listed in Table 1:

[0137] Test the adhesion of the coating according to GB / T 5210-2006 "Determination of adhesion of paints and varnishes by pull-off method";

[0138] Test the pencil hardness of the coating according to GB / T 6739-2022 "Determination of film hardness of paints and varnishes by pencil method";

[0139] Test the impact resistance of the coating according to GB / T 1732-2020 "Determination of impact resistance of paint films" standard;

[0140] Test the acid and alkali resistance of the coating according to GB / T 1763 "Determination of chemical corrosion resistance of paint films" standard;

[0141] Test the oil resistance of the coating according to HG / T3343-1985 "Determination of Oil Resistance of Paint Film";

[0142] The volume resistivity and dielectric strength are tested according to GB / T 31838.2-2019 "Dielectric and resistance properties of solid insulating materials".

[0143] Table 1

[0144]

[0145] By comparing Examples 1-7, it can be found that Example 1 has the best performance, which may be due to the combined effect of the addition of modified basalt fiber and modified waterborne epoxy resin. Because the basalt fiber can remove the surface oxide layer and impurities by stirring and soaking in hydrochloric acid solution, increase the roughness of its fiber surface and increase the reaction sites, add octadecylamine and cyclohexylamine and stir to attach amino chemical functional groups to its surface, then add 4,4'-methylenebis(phenyl isocyanate), and use addition polymerization to achieve in-situ growth of polyurea nanofibers on the surface of basalt fiber, which can wrap the basalt fiber well, and the modified waterborne epoxy resin and modified basalt fiber react to form a chemical bond to connect more tightly and the resin can be better dispersed in water to form a uniform coating, which helps the coating to form a uniform and tough bonding layer with the substrate surface. The polyurea nanofibers grown on the surface of basalt fiber can form chemical bonds with modified waterborne epoxy resin to reduce the effect of micro defects at the interface between basalt fiber and coating, delay the diffusion of corrosive media during immersion, and improve the adhesion of basalt fiber at the coating interface. The modified basalt fiber is more firmly present in the composite coating, and the anti-corrosion performance is improved without losing the tribological properties of the coating. When the coating is subjected to an applied external force, the surface composite fiber layer can bear the vertical pressure and radial cutting force of the friction pair, and the inner composite fiber pins the deformed resin, thereby reducing the initiation and expansion of cracks during friction, reducing the amount of coating peeling, and achieving the effect of improving the tribological properties of the composite coating. Basalt fiber itself has excellent electrical insulation properties. The modified basalt fiber forms polyurea and forms chemical bonds with the modified waterborne epoxy resin to form a highly cross-linked three-dimensional network structure. The close entanglement between the molecular chains in this structure reduces the movement of charge carriers, thereby improving the insulation performance.

Claims

1. An insulating oil-resistant coating for a storage tank, characterized in that: Calculated by weight, the invention comprises 10-20 parts of modified basalt fiber, 70-90 parts of modified waterborne epoxy resin, 2-4 parts of auxiliary agent, 80-160 parts of water and 10-30 parts of waterborne epoxy resin curing agent.

2. The insulating oil-resistant coating for storage tanks according to claim 1, characterized in that: The modified basalt fiber is prepared by the following method: by weight: (1) Weighing 5-15 parts of chopped basalt fibers, adding them to 400-600 parts of 5-15wt% hydrochloric acid, stirring at 600-800 rpm and room temperature for 16-24 hours, then ultrasonically cleaning them in anhydrous ethanol for 10-30 minutes, filtering, and drying the filter cake at 40-60° C. for later use to obtain acid-treated chopped basalt fibers; (2) ultrasonically dissolving 5-15 parts of octadecylamine and 3-8 parts of cyclohexylamine in 150-300 parts of anhydrous ethanol; adding 5-15 parts of the acid-treated chopped basalt fibers of step (1), and then stirring at 40-60° C. and 800-1200 rpm for 20-40 min, removing the basalt fibers and placing them in 100-300 parts of water and continuing to stir to obtain a basalt fiber suspension; (3) dissolving 15-20 parts of 4,4'-methylenebis(phenyl isocyanate) in 200-400 parts of ethyl acetate, and then slowly dropping it into the basalt fiber suspension of step (2) within 40-80 minutes. After the dropping is completed, the temperature of the mixed solution is raised to 70-90°C. After reacting for 4-6 hours, the basalt fiber is fished out and dried at 40-60°C for 4-6 hours to obtain the modified basalt fiber.

3. The insulating oil-resistant coating for storage tanks according to claim 1, characterized in that: The modified waterborne epoxy resin is prepared by the following method: by weight: S1: Dissolve 5-10 parts of 2-aminoethanesulfonic acid in 100-200 parts of water, and add 30-40 wt% NaOH aqueous solution to adjust the pH to 8-10; S2: Add 10-15 parts of epoxy resin and 1-3 parts of phase transfer catalyst to 20-40 parts of water, stir at 60-80° C. and 800-1200 rpm for 5-10 min, then add to the solution obtained in step S1 and react for 6-8 h.

4. The insulating oil-resistant coating for a storage tank as claimed in claim 1, characterized in that: The auxiliary agent is at least one of a defoamer, a dispersant and an antioxidant.

5. The insulating oil-resistant coating for a storage tank as claimed in claim 1, characterized in that: The waterborne epoxy resin curing agent is at least one of polyetheramine and waterborne amine curing agent.

6. A method for preparing the insulating oil-resistant coating for storage tanks according to any one of claims 1 to 5, characterized in that: The steps include: Step 1: Ultrasonic disperse 10-20 parts of modified basalt fiber in 40-80 parts of water, then add 70-90 parts of modified waterborne epoxy resin, stir evenly and set aside; Step 2: Mix 10-30 parts of waterborne epoxy resin curing agent, 2-4 parts of auxiliary agent and 40-80 parts of water and stir evenly for later use; Step 3: Stir and mix the mixture obtained in step 1 and step 2 to obtain the insulating oil-resistant coating for the storage tank.

Citation Information

Patent Citations

  • Preparation method and application of basalt fiber surface modified coating

    CN107640913A

  • Basalt scale solvent-free heavy anticorrosive coating and method for preparing same

    CN108441083A

  • Phenylamine tripolymer modified basalt scale self-repairing anticorrosive coating and preparation method thereof

    CN114539874A