Method for improving performance of niobium-containing precipitated phase of superaustenitic stainless steel by regulating and controlling boron and niobium

By adding B and Nb to super austenitic stainless steel to form (Nb, Mo) (B, C, N) precipitated phase, and through slow cooling and heat preservation aging treatment, the segregation and segregation of Mo during the solidification process of super austenitic stainless steel are solved. The problem of narrow thermal processing window has improved the strength and corrosion resistance to meet the engineering needs of high strength, toughness and high corrosion resistance.

CN118745503AActive Publication Date: 2024-10-08TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410837423.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-08
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Super austenitic stainless steel has severe Mo segregation during the solidification process, a narrow hot processing window, and difficulty in manufacturing. It is difficult to improve its strength and corrosion resistance at the same time with existing technology, especially when the strength is increased through precipitation phases, the corrosion resistance will be affected. .

Method used

By adding B and Nb to super austenitic stainless steel, the (Nb, Mo) (B, C, N) precipitation phase is formed, and the grain boundary segregation effect of B is used to suppress the precipitation of σ and reduce and refine the grain boundary precipitation phase. , and its distribution is controlled through slow cooling and thermal insulation aging treatment, delaying the formation of Mo precipitated phase, and improving the strength and corrosion resistance of the material.

Benefits of technology

It effectively improves the strength and corrosion resistance of super austenitic stainless steel, meets the engineering needs of high strength, toughness and high corrosion resistance, and solves the problem of precipitation affecting corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745503A_ABST
    Figure CN118745503A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the performance of a niobium-containing precipitated phase of superaustenitic stainless steel through boron and niobium regulation and control, and belongs to the technical field of stainless steel preparation. The microelements B and Nb are introduced, B and Mo are dissolved in a Nb (C, N) precipitated phase, and a (Nb, Mo) (B, C, N) precipitated phase is formed; the crystal boundary segregation effect of B is used for inhibiting sigma formation, so that a crystal boundary precipitated phase is reduced and finer; through slow cooling, heat preservation and aging treatment, fine and dispersed distribution of (Nb, Mo) (B, C and N) is further regulated and controlled; and meanwhile, precipitation of the Mo-containing precipitated phase at the grain boundary is delayed, and Mo precipitated phase grains are reduced. The strength and corrosion resistance of the superaustenitic stainless steel are improved through the combination of (Nb, Mo) (B, C, N) and Mo-rich precipitated phases which are fine in intergranular and grain boundary and are distributed in a dispersed manner.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of stainless steel preparation, and in particular to a method for regulating the niobium-containing precipitation phase of super austenitic stainless steel by boron and niobium to improve performance. Background Art

[0002] Super austenitic stainless steel is austenitic stainless steel with high Cr and Mo content. It has high corrosion resistance and mechanical properties and has been widely used in high-end equipment manufacturing fields such as energy conservation and environmental protection, marine engineering, and petrochemicals. With the development of these fields, higher requirements are placed on the strength, toughness, and corrosion resistance of materials.

[0003] Super austenitic stainless steel is one of the most technically difficult types of stainless steel to produce. It has severe Mo segregation during solidification, is sensitive to precipitation phases during hot rolling, has a particularly narrow hot processing window, and is very difficult to manufacture. The reason is closely related to the sensitivity to precipitation phases. How to inhibit the precipitation of precipitation phases and simultaneously improve the strength and corrosion resistance of super austenitic stainless steel has become a serious problem restricting its development, and relevant research is urgently needed.

[0004] In stainless steel, alloying elements such as Ni, Mn, Ce, and N can stabilize the austenite structure of super austenitic stainless steel and inhibit the precipitation of precipitation phases. Microalloying element B can affect the microstructure, corrosion resistance, and mechanical properties of super austenitic stainless steel. Microalloying elements with extremely low content can significantly improve material properties. Usually, precipitation strengthening is the most effective way to improve material strength, but given that precipitation phases affect corrosion resistance, super austenitic stainless steel mainly uses solid solution strengthening to improve strength, and almost no precipitation strengthening is used to improve strength. However, the strength improvement by solid solution strengthening alone is limited, and it is difficult to meet the higher strength requirements of super austenitic stainless steel. Summary of the invention

[0005] The purpose of the present invention is to provide a method for improving the performance of super austenitic stainless steel containing niobium by composite regulation of boron and niobium, so as to solve the problems existing in the above-mentioned prior art. The present invention combines the beneficial effects of B and Nb in super austenitic stainless steel, utilizes B and Mo to dissolve in Nb(C,N) precipitation phase, and forms (Nb,Mo)(B,C,N) precipitation phase; utilizes the grain boundary segregation effect of B to inhibit the formation of σ, so that the number of grain boundary precipitation phases is reduced and finer. Through slow cooling and heat preservation aging treatment, the fine and dispersed distribution of (Nb,Mo)(B,C,N) is further regulated; at the same time, the precipitation of Mo-containing precipitation phase at the grain boundary is delayed, so that the grain size of Mo precipitation phase is reduced; through the combination of fine and dispersed (Nb,Mo)(B,C,N) and Mo-rich precipitation phases in the grain and grain boundary, the strength and corrosion resistance of super austenitic stainless steel are improved, meeting the higher demand of "high strength and high corrosion resistance" of super austenitic stainless steel for engineering.

[0006] To achieve the above object, the present invention provides the following solutions:

[0007] One of the technical solutions of the present invention: a method for improving the performance of super austenitic stainless steel by regulating the niobium-containing precipitation phase of boron and niobium, comprising the following steps: homogenizing a super austenitic stainless steel ingot containing element B and element Nb and rolling it into a steel plate, then performing a solid solution treatment and a slow cooling and heat preservation aging treatment in sequence, and finally water cooling to room temperature to obtain super austenitic stainless steel.

[0008] Furthermore, the content of element B in the super austenitic stainless steel is 0.003-0.011 wt.%, and the content of element Nb in the super austenitic stainless steel is 0.04-0.15 wt.%.

[0009] Furthermore, the super austenitic stainless steel has the following chemical composition, in mass percentage: C: 0.01-0.03%, Si: 0.5-1.0%, P: 0.01-0.03%, S: 0.005-0.01%, Mn: 1.5-2.0%, Cr: 19-24%, Ni: 17.0-22.0%, Mo: 5.5-6.5%, Cu: 0.5-1.5%, N: 0.15-0.3%, B: 0.003-0.011%, Nb: 0.04-0.15%, and the remainder is Fe and other inevitable impurity elements.

[0010] Furthermore, the temperature of the homogenization treatment is 1200-1260° C., and the time is 16-24 hours.

[0011] Furthermore, the rolling temperature is 1000-1220°C.

[0012] Furthermore, the temperature of the solution treatment is 1160-1240° C., and the time is 3-8 hours.

[0013] Furthermore, the slow cooling and heat preservation aging treatment specifically includes: cooling to 1020-1100° C. at a cooling rate of 250-300° C. / h after the solution treatment, and keeping the temperature for 10-60 minutes.

[0014] The main function of C element is to stabilize and strengthen the austenite phase. Reducing the content of C element can reduce the precipitation of Cr carbides, thereby reducing the Cr-poor area formed by Cr carbides and improving the corrosion resistance of the material. It combines with Nb and N elements to form a fine and dispersed Nb (C, N) phase, which plays a role of precipitation strengthening.

[0015] The Si element has a strong deoxidation ability. Adding a certain amount of Si to steel helps to reduce the oxygen content in the steel. The Si element helps to form a dense SiO2 oxide film between the stainless steel matrix and the oxide layer, thereby improving the oxidation resistance of austenitic stainless steel. When austenitic stainless steel containing Si is in a chloride corrosion medium, Si can move the pitting potential of the stainless steel toward the positive potential, thereby improving the corrosion resistance of the stainless steel.

[0016] Mn is an element that stabilizes austenite. Mn and Ni work together to effectively increase the solubility of N in austenitic stainless steel.

[0017] The Cr element can significantly improve the corrosion resistance of austenitic stainless steel. The reaction of Cr and O can generate a complete and dense Cr2O3 passivation film. The dense oxide film can prevent the stainless steel matrix from being penetrated by corrosive media, thereby improving the corrosion resistance of austenitic stainless steel.

[0018] Ni is a typical austenitizing element. Ni can promote the formation of austenite in stainless steel, reduce the precipitation of σ phase in super austenitic stainless steel, and improve the strength and hot working performance of super austenitic stainless steel. Ni can also improve the structure and performance of the passivation film on the surface of stainless steel, and improve the thermodynamic stability and high temperature oxidation resistance.

[0019] The Mo element can significantly improve the ability of super austenitic stainless steel to resist sulfur and chloride ion corrosion, and significantly improve the pitting corrosion resistance and intergranular corrosion resistance of super austenitic stainless steel.

[0020] Cu can improve the corrosion resistance of stainless steel in reducing corrosive media. Cu is easily concentrated in the passivation film, preventing oxygen from diffusing into the stainless steel matrix and protecting the matrix.

[0021] Nitrogen is a commonly used austenite stabilizing element that can expand the austenite region in steel. It has a significant solid solution strengthening effect in stainless steel, improving the strength, creep performance, fatigue resistance and work hardening ability of stainless steel. Nitrogen also simultaneously improves the stability of the passivation film in super austenitic stainless steel and improves the corrosion resistance of steel.

[0022] As a microalloying element, B is usually difficult to dissolve in the Fe matrix and is easily distributed at the grain boundary, thereby increasing the grain boundary strength and improving the high-temperature hot working performance. The present invention utilizes the fact that B is easily distributed at the grain boundary, thereby affecting the segregation of elements such as Cr, Mo, and Nb at the grain boundary and controlling the precipitation of the precipitated phase.

[0023] As a precipitation strengthening element, Nb is hardly added to super austenitic stainless steel. The formation of Nb(C,N) will reduce the corrosion resistance. The present invention utilizes the (Nb,Mo)(B,C,N) precipitation phase formed by the composite regulation of B and Nb to make up for the shortcomings of Nb(C,N) in terms of weak corrosion resistance.

[0024] The present invention adds microalloying elements B and Nb to the composition of the currently used super austenitic stainless steel, appropriately increases the content of C and N, and dissolves B and Mo in the Nb(C,N) precipitation phase to form the (Nb,Mo)(B,C,N) precipitation phase; utilizes the grain boundary segregation effect of B to inhibit the precipitation of σ, so that the number of grain boundary precipitation phases is reduced and the particles are fine. Utilizes slow cooling and heat preservation aging treatment to further regulate the fine and dispersed precipitation of (Nb,Mo)(B,C,N); delays the precipitation of Mo-containing precipitation phases at grain boundaries, so that the precipitation at grain boundaries is reduced and becomes finer. The strength and corrosion resistance of super austenitic stainless steel are improved by the combination of fine and dispersed (Nb,Mo)(B,C,N) and Mo-rich precipitation phases in the grains and at the grain boundaries.

[0025] The second technical solution of the present invention: a super austenitic stainless steel prepared by the above method.

[0026] The third technical solution of the present invention: an application of the above-mentioned super austenitic stainless steel in the fields of energy conservation and environmental protection, marine engineering or petrochemical industry.

[0027] The present invention discloses the following technical effects:

[0028] The method of the present invention can improve the strength and corrosion resistance of super austenitic stainless steel, and can meet the higher requirements of "high strength, high toughness and high corrosion resistance" of super austenitic stainless steel for engineering use. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 The grain boundary precipitation phase diagrams of the super austenitic stainless steel prepared in Example 1 and Comparative Examples 1-2 of the present invention, wherein (a) is the super austenitic stainless steel sample prepared in Comparative Example 1, (b) is the super austenitic stainless steel sample prepared in Comparative Example 2, and (c) is the super austenitic stainless steel sample prepared in Example 1;

[0031] Figure 2 This is a phase diagram of Nb precipitation in the crystal of the super austenitic stainless steel prepared in Example 1 of the present invention;

[0032] Figure 3 This is the energy spectrum of the Nb precipitation phase in the crystal of the super austenitic stainless steel prepared in Example 1 of the present invention.

[0033] Figure 4The polarization curve of the super austenitic stainless steel prepared in Example 1 of the present invention;

[0034] Figure 5 The stress-strain curve of the super austenitic stainless steel prepared in Example 1 of the present invention;

[0035] Figure 6 2 are the grain boundary precipitation phase diagrams of the super austenitic stainless steel samples prepared in Examples 2 to 3 of the present invention and Comparative Example 3, (a) is the super austenitic stainless steel sample prepared in Example 2, (b) is the super austenitic stainless steel sample prepared in Example 3, and (c) is the super austenitic stainless steel sample prepared in Comparative Example 3. DETAILED DESCRIPTION

[0036] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0037] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0038] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0039] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0040] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0041] Example 1

[0042] A method for improving the performance of super austenitic stainless steel by regulating the niobium-containing precipitation phase with boron and niobium:

[0043] Super austenitic stainless steel is composed of the following components, by mass percentage: C: 0.03%, Si: 0.8%, P: 0.03%, S: 0.01%, Mn: 2.0%, Cr: 20%, Ni: 18%, Mo: 6%, Cu: 1%, N: 0.25%, B: 0.005%, Nb: 0.05%, and the balance is Fe and other inevitable impurity elements.

[0044] (1) According to the above mass percentages, the component raw materials are evenly mixed and smelted in a vacuum induction furnace (vacuumed after power-on and temperature-controlled at 1500-1600° C.), and then cast into ingots under vacuum conditions. When cooled to room temperature, the ingots are demoulded to obtain super austenitic stainless steel ingots.

[0045] (2) The super austenitic stainless steel ingot was homogenized at 1250°C for 20 h and then rolled into steel plates at 1200°C.

[0046] (3) A 10×10 mm steel plate sample was cut and solution treated (treatment temperature was 1200°C for 4 h), then cooled to 1050°C in a furnace at a cooling rate of 250°C / h, kept at that temperature for 30 min (slow cooling and aging treatment), and then water-cooled to room temperature to obtain a super austenitic stainless steel sample.

[0047] Comparative Example 1

[0048] The same as Example 1, except that the super austenitic stainless steel does not contain B and Nb.

[0049] Comparative Example 2

[0050] The same as Example 1, except that the super austenitic stainless steel does not contain Nb.

[0051] The super austenitic stainless steel samples prepared in Example 1 and Comparative Examples 1-2 were polished with different types of sandpaper, then mechanically polished and metallographically etched. The microstructure of the samples aged at 1050°C for 30 minutes was analyzed using a scanning electron microscope. The analysis results are shown in Figure 1 (Grain boundary precipitation phase diagram). Figure 1 (a) is the super austenitic stainless steel sample (0B sample) prepared in Comparative Example 1, (b) is the super austenitic stainless steel sample (B sample) prepared in Comparative Example 2, and (c) is the super austenitic stainless steel sample (B+Nb sample) prepared in Example 1.

[0052] from Figure 1It can be seen from the figure that after aging at 1050℃ for 30min, coarse precipitates appear at the grain boundaries of the 0B sample; after adding B, compared with the 0B sample, the precipitation at the grain boundaries of the B sample becomes less and the size of the precipitates decreases. After adding Nb on the basis of B, compared with the 0B sample and the B sample, the amount of precipitation at the grain boundaries of the B+Nb sample is further reduced, and the size of the precipitates changes from micrometer level to nanometer level.

[0053] In the B+Nb sample, B and Nb work together, B and Mo dissolve in the Nb(C,N) precipitate phase, consume the Mo element, reduce the element enrichment at the grain boundary, and use the grain boundary segregation effect of B to inhibit the precipitation of σ, making the grain boundary precipitate phase smaller in number and smaller in size. The slow cooling and heat preservation aging treatment is used to further control the fine and dispersed distribution of (Nb,Mo)(B,C,N); at the same time, the precipitation of Mo-containing precipitates at the grain boundary is delayed, and the strength and corrosion resistance of super austenitic stainless steel are improved through the combination of fine and dispersed (Nb,Mo)(B,C,N) and Mo-rich precipitates in the grain and at the grain boundary.

[0054] The phase diagram of Nb precipitation in the crystal of the super austenitic stainless steel prepared in Example 1 is shown in Figure 2 .

[0055] from Figure 2 It can be seen that after B+Nb aging, there are finely dispersed (Nb, Mo) (B, C, N) precipitates in the crystal. The size of the precipitates is at the nanoscale, which plays a good role in dispersion precipitation strengthening, pins dislocations, and improves mechanical properties.

[0056] The energy spectrum of the Nb precipitate phase in the crystal of the super austenitic stainless steel prepared in Example 1 is shown in Figure 3 .

[0057] from Figure 3 It can be seen that the size of some intracrystalline ((Nb, Mo)(B, C, N) precipitates is about 20 nm. When analyzing its composition, it is found that the precipitates contain Nb, Mo, B, C, N and other elements, indicating that in the formation process of Nb(C, N) precipitates, B and Mo are dissolved in Nb(C, N) precipitates to form (Nb, Mo)(B, C, N) precipitates. The fine and dispersed distribution of the precipitates in the crystal plays a good precipitation strengthening role, while affecting the distribution of grain boundary elements, reducing the precipitation of Mo-containing precipitates at the grain boundaries, and refining the size of the grain boundary precipitates.

[0058] Electrochemical experiments were carried out on the B sample and the B+Nb sample in a three-electrode corrosion cell equipped with a platinum foil counter electrode and a saturated calomel (SCE) reference electrode. Figure 4 .

[0059] from Figure 4It can be seen that the current density of the B+Nb sample is smaller, indicating that the dissolution rate of the passivation film is slower, the structure is denser, and the corrosion resistance of the sample is better. The self-corrosion potential of the B sample is relatively low, indicating that the formation rate of the passivation film is slow and the stability is poor; therefore, the passivation film on the surface of the B+Nb sample is more stable, and the material has better pitting resistance.

[0060] The stress-strain curves of the B sample and the B+Nb sample were measured using a small tensile machine. Figure 5 .

[0061] from Figure 5 It can be seen that compared with the B sample, the yield strength and tensile strength of the B+Nb sample are improved. Although the plasticity is slightly reduced, the overall plasticity is good.

[0062] Example 2

[0063] The same as Example 1, except that step (3) specifically includes cutting a 10×10 mm steel plate sample for solution treatment (treatment temperature is 1200° C., time is 4 h), then cooling to 1050° C. at a rate of 300° C. / h, keeping the temperature for 30 min (slow cooling and aging treatment), and then cooling to room temperature with water to obtain a super austenitic stainless steel sample. The grain boundary precipitation phase diagram is shown in FIG. Figure 6 .

[0064] Example 3

[0065] Same as Example 1, except that the mass percentage of B is 0.01%, the mass percentage of Nb is 0.15%, and the grain boundary precipitation phase diagram is shown in Figure 6 .

[0066] Comparative Example 3

[0067] The same as Example 1, except that step (3) is as follows: a 10×10 mm steel plate sample is cut and subjected to solution treatment (treatment temperature is 1200°C, time is 4 h), and the sample after solution treatment is directly subjected to 1050°C, kept for 30 min, and then water-cooled to room temperature without slow cooling and heat preservation, to obtain a super austenitic stainless steel sample. The sample is ground, polished, and metallographically etched and then the structure is observed (see Figure 6 ).

[0068] Figure 6 , (a) is a grain boundary precipitation phase (B+Nb) diagram of the super austenitic stainless steel sample prepared in Example 2, (b) is a grain boundary precipitation phase (B+Nb) diagram of the super austenitic stainless steel sample prepared in Example 3, and (c) is a grain boundary precipitation phase (B+Nb) diagram of the super austenitic stainless steel sample prepared in Comparative Example 3.

[0069] from Figure 6It can be seen that the samples prepared in Examples 2 and 3 are the same as those prepared in Example 1, while Comparative Example 3 does not undergo slow cooling and heat preservation treatment, and no ((Nb, Mo)(B, C, N) precipitation phase appears in the crystal. Therefore, the Mo element segregates to the grain boundaries. Compared with Examples 1 to 3, the number of precipitated phases at the grain boundaries increases and the size of some precipitated phases is larger.

[0070] The embodiments described above are only descriptions of the preferred embodiments of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for improving the performance of super austenitic stainless steel by regulating the niobium-containing precipitation phase by boron and niobium, characterized in that: The following steps are involved: The super austenitic stainless steel ingot containing element B and element Nb is homogenized and then rolled into a steel plate, and then subjected to a solid solution treatment and a slow cooling and heat preservation aging treatment in sequence, and finally water-cooled to room temperature to obtain the super austenitic stainless steel.

2. The method according to claim 1, characterized in that The content of element B in the super austenitic stainless steel is 0.003-0.011 wt. %, and the content of element Nb in the super austenitic stainless steel is 0.04-0.15 wt. %.

3. The method according to claim 1, characterized in that The super austenitic stainless steel has the following chemical composition, in percentage by mass: C: 0.01-0.03%, Si: 0.5-1.0%, P: 0.01-0.03%, S: 0.005-0.01%, Mn: 1.5-2.0%, Cr: 19-24%, Ni: 17.0-22.0%, Mo: 5.5-6.5%, Cu: 0.5-1.5%, N: 0.15-0.3%, B: 0.003-0.011%, Nb: 0.04-0.15%, and the remainder is Fe and other inevitable impurity elements.

4. The method according to claim 1, characterized in that: The temperature of the homogenization treatment is 1200-1260° C., and the time is 16-24 hours.

5. The method according to claim 1, characterized in that The rolling temperature is 1000-1220°C.

6. The method according to claim 1, characterized in that The temperature of the solution treatment is 1160-1240° C., and the time is 3-8 hours.

7. The method according to claim 1, characterized in that The slow cooling and heat preservation aging treatment specifically includes: cooling to 1020-1100° C. at a cooling rate of 250-300° C. / h after the solution treatment, and keeping the temperature for 10-60 minutes.

8. Super austenitic stainless steel prepared by the method according to any one of claims 1 to 7.

9. Application of the super austenitic stainless steel according to claim 8 in the fields of energy conservation and environmental protection, marine engineering or petrochemical industry.

Citation Information

Patent Citations

  • Heat-resistant corrosion-resistant austenitic stainless steel and preparation method thereof

    CN109930067A

  • Age hardening austenitic stainless steel and preparation method thereof

    CN110499455A

  • High-strength high-corrosion-resistance super austenitic stainless steel and preparation method thereof

    CN112143973A

  • Method for regulating and controlling grain boundary boron redistribution to improve grain boundary second phase precipitation of super-austenitic stainless steel

    CN113802064A

  • Austenitic stainless steel alloy for fuel cladding of supercritical gas cooled reactor and preparation method of austenitic stainless steel alloy

    CN115233105A