Strengthening and toughening heat treatment process suitable for 20CrMnTi steel building pipe

Through the strengthening and toughening heat treatment process of induction heating and controlled cooling, the problem of matching strength and plasticity in 20CrMnTi steel construction pipes has been solved, and the comprehensive mechanical properties of high strength, high plasticity and low yield-strength ratio have been achieved, expanding the use of the material and improving improve production efficiency and cost-effectiveness.

CN118745505AActive Publication Date: 2024-10-08HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410737407.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-08
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

The existing heat treatment process is difficult to achieve the matching of high strength, high plasticity and high toughness in 20CrMnTi steel construction pipes, and the yield-strength ratio is difficult to reach the low value required for building structures.

Method used

The toughening heat treatment process of induction heating and controlled cooling is adopted, and the temperature is raised to 860-900°C at 15-30°C/s, and then cooled to 360-400°C at a rate of 30-50°C/s, and is naturally exposed to air. Cooling, combined with water spray or water cooling to obtain martensite and austenite structures, ensuring simultaneous improvement of strength and plasticity.

Benefits of technology

Achieving good strength and plasticity matching of 20CrMnTi steel construction pipes, the yield strength is 500~550MPa, the tensile strength is 1100~1180MPa, the elongation after break is ≥12%, and the yield ratio is ≤0.5, which meets the requirements of high strength, toughness and low temperature of building structures. Yield-to-strength ratio requirements, and has the advantages of simple operation and stable performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745505A_ABST
    Figure CN118745505A_ABST
Patent Text Reader

Abstract

The invention relates to a strengthening and toughening heat treatment process suitable for a 20CrMnTi steel building pipe. The heat treatment process comprises the two steps of heating and controlled cooling. In the heating step, the 20CrMnTi steel building pipe is heated to 860-900 DEG C at the speed of 15-30 DEG C / s, heat preservation is not needed after heating is completed, and the 20CrMnTi steel building pipe directly enters the controlled cooling step; and a controlled cooling step: cooling the 20CrMnTi steel building pipe subjected to induction heating to 360-400 DEG C at the speed of 30-50 DEG C / s in a water spraying or water penetrating manner, and then naturally cooling to room temperature in air. The 20CrMnTi steel building pipe prepared through the method has good strength and plasticity matching, the yield strength ranges from 500 MPa to 550 MPa, the tensile strength ranges from 1100 MPa to 1180 MPa, the percentage elongation after fracture can reach 12% or above, and the yield ratio is lower than 0.5; on the basis of meeting the requirements of building structural steel for high toughness and low yield ratio, the application of the 20CrMnTi steel is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a heat treatment process capable of effectively improving the comprehensive mechanical properties of 20CrMnTi steel building pipes. Background Art

[0002] In the field of building structures, various types of steel pipe products are widely used. In recent years, with the development trend of large-scale, high-rise and lightweight building structures, higher and higher requirements have been put forward for the comprehensive mechanical properties of building steel pipes, such as strength and plasticity; at the same time, in order to meet the seismic resistance and safety performance, building steel pipes generally require a lower yield strength ratio (usually below 0.6); in addition, the selection of materials and processing technology of building steel pipes also need to take into account factors such as cost and efficiency.

[0003] 20CrMnTi steel is a commonly used low-carbon low-alloy steel. According to GB / T 3077-2015 "Alloy Structural Steel", the chemical composition of 20CrMnTi steel is: C 0.17-0.23%, Si 0.17-0.37%, Mn 0.80-1.10%, Cr 1.00-1.30%, Ti 0.04-0.10, and the balance is Fe and inevitable impurities. 20CrMnTi steel has good hardenability, and carburizing + quenching + low-temperature tempering is usually used as the preferred heat treatment process for various gears, shafts and other parts. From the perspective of strength, material cost and welding performance, 20CrMnTi steel can theoretically be used as a candidate material for the preparation of construction steel pipes. However, when using conventional heat treatment processes, if the tensile strength exceeds 1000MPa, quenching + low-temperature tempering heat treatment must be used to achieve it. At this time, since the microstructure is tempered martensite with high strength and poor plasticity, the elongation after fracture is difficult to exceed 10%, and the yield strength ratio is difficult to reach below 0.6. Therefore, it is necessary to develop a heat treatment process suitable for industrial production to achieve a good match and simultaneous improvement of high strength, high plasticity and high toughness.

[0004] In this regard, the present invention proposes a heat treatment process that can effectively improve the comprehensive mechanical properties of 20CrMnTi steel building pipes, aiming to meet the requirements of building structural steel for high strength and toughness and low yield ratio, and further expand the use of 20CrMnTi steel. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a heat treatment process which is suitable for 20CrMnTi steel building pipes and can effectively improve the comprehensive mechanical properties.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a strengthening and toughening heat treatment process suitable for 20CrMnTi steel building pipes, the heat treatment process includes two steps of heating and controlled cooling; in the heating step, the 20CrMnTi steel building pipes are heated to 860-900°C at a rate of 15-30°C / s, and after the heating is completed, no insulation is required and the cooling step is directly entered.

[0007] In the heating step of the present invention, the heating method is induction heating.

[0008] In the controlled cooling step of the present invention, the 20CrMnTi steel building pipe after induction heating is cooled to 360-400°C at a rate of 30-50°C / s, and then naturally cooled to room temperature in air to obtain a finished building pipe.

[0009] In the controlled cooling step of the present invention, the cooling method is water spray cooling or water penetration cooling.

[0010] The 20CrMnTi steel building pipe obtained by the heat treatment process of the present invention has good strength and plasticity matching, a yield strength of 500-550MPa, and a tensile strength of 1100-1180MPa.

[0011] The 20CrMnTi steel building pipe obtained by the heat treatment process of the present invention has an elongation after fracture of ≥12% and a yield strength ratio of ≤0.5.

[0012] The heat treatment process of the present invention is applicable to 20CrMnTi steel building pipes with a wall thickness of 3.0 to 5.5 mm.

[0013] The strengthening and toughening heat treatment process for 20CrMnTi steel building pipes includes two steps: induction heating and controlled cooling. The design ideas are as follows: 1) The temperature of the heating step is controlled within a reasonable range that can ensure that the pipe structure is completely austenitized and avoid the rapid thickening of the oxide scale on the surface, thereby ensuring the strength and surface quality of the finished product. At the same time, a reasonable heating rate range is adopted to match the conditions of commonly used industrial induction heating equipment. After the heating step, there is no conventional insulation or soaking stage, which can effectively inhibit the growth of austenite grains. The surface oxide scale of Yamato is thickened, which can maximize the production rhythm and reduce the electricity consumption cost; 2) Controlled cooling successively undergoes two stages: water spraying or water cooling, and natural cooling in the air. The termination temperature of the water spraying or water cooling stage is controlled in the optimal range between the Ms point and the Mf point of 20CrMnTi steel, and the cooling rate is controlled in the range of 30-50℃ / s to obtain martensite and austenite structure. In the subsequent natural cooling stage in the air, carbon distribution can be achieved, thereby obtaining and retaining the residual austenite structure, and achieving the simultaneous improvement of strength and plasticity. If the termination temperature of the water spraying or water penetration cooling stage is lower than 360℃, it is difficult to obtain enough residual austenite structure, resulting in insufficient plasticity; if the termination temperature of the water spraying or water penetration cooling stage is higher than 400℃, it is difficult to obtain enough martensite structure, resulting in insufficient strength; if the cooling rate of the water spraying or water penetration cooling stage is less than 30℃ / s, it is impossible to obtain enough martensite structure, and it is difficult to obtain sufficiently high strength; if the cooling rate exceeds 50℃ / s, it will not only increase the risk of cracking and deformation, but also make it difficult to accurately control the termination temperature of the water spraying or water penetration cooling stage within a reasonable range. In addition, if the wall thickness specification of the building pipe is less than 3.0mm, the pipe is prone to deformation and bending during the water spraying or water penetration cooling stage; if the wall thickness specification exceeds 5.5mm, it is difficult to ensure the uniformity of microstructure and mechanical properties due to the large difference in cooling rate inside and outside the pipe.

[0014] The beneficial effect of adopting the above technical solution is that the 20CrMnTi steel building pipe obtained by the present invention has good strength and plasticity matching, the yield strength is in the range of 500-550MPa, the tensile strength is in the range of 1100-1180MPa, the elongation after fracture can reach more than 12%, and the yield strength ratio is not higher than 0.5, which meets the requirements of building structural steel for high strength and low yield strength ratio. The present invention expands the use of 20CrMnTi steel and has the advantages of simple operation and stable performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 Schematic diagram of the time-temperature system of the heat treatment process of the present invention. DETAILED DESCRIPTION

[0016] The present invention is further described in detail below in conjunction with specific implementation modes.

[0017] The process of each step of this heat treatment method is as follows: (1) Induction heating step: The induction heating step is to heat the 20CrMnTi steel construction pipe to 860-900℃ at a rate of 15-30℃ / s by induction heating. Among them, the heating rate of 15-30℃ / s can match the conditions of commonly used industrial induction heating equipment, especially the power conditions, so as to realize industrial mass production; the end temperature of heating is controlled within the range of 860-900℃ because the measured value of the Ac3 temperature (complete austenitization temperature) of 20CrMnTi steel is about 810℃. Controlling the end temperature of heating and the insulation temperature within the range of 50-90℃ of the Ac3 temperature can ensure that the pipe is completely austenitized during the heating process, so as to obtain the martensite and austenite structure required for high strength and high plasticity in the subsequent controlled cooling process. If the heating temperature is lower than 860℃, the pipe is likely to be difficult to achieve complete austenitization, resulting in fluctuations and instability in mechanical properties; if the heating temperature is higher than 900℃, the iron oxide scale on the surface of the pipe will rapidly thicken, thereby affecting the surface quality of the finished product.

[0018] (2) Controlled cooling step: The controlled cooling step is to first cool the induction heated 20CrMnTi steel building pipe to 360-400°C by spraying or penetrating water at a rate of 30-50°C / s, and then cool it naturally to room temperature in the air. Among them, during the cooling process of the pipe by water spraying or water penetration, the cooling rate can reach more than 30℃ / s, which can meet the cooling rate requirements for the martensitic transformation of 20CrMnTi steel; the termination temperature of the water spraying or water penetration cooling stage is controlled in the range of 360-400℃, because when the cooling rate is controlled in the range of 30-50℃ / s, the Ms point (the martensitic transformation start temperature of the steel) and the Mf point (the martensitic transformation end temperature of the steel) of 20CrMnTi steel are measured to be 405℃ and 292℃ respectively. By controlling the termination temperature of the water spraying or water penetration cooling stage in a reasonable range between the Ms point and the Mf point, the martensite and austenite structures required for high strength and high plasticity can be obtained; in the subsequent natural cooling process in the air, carbon distribution can be achieved, thereby obtaining and retaining the residual austenite structure, and achieving the simultaneous improvement of strength and plasticity. Example 1

[0019] The 20CrMnTi steel building pipe in this embodiment is a seamless round pipe with a wall thickness of 5 mm and a diameter of 42 mm. The heat treatment method is specifically described as follows.

[0020] (1) Induction heating step: The 20CrMnTi steel seamless round tube is heated to 900° C. at a rate of 30° C. / s by induction heating.

[0021] (2) Controlled cooling step: The induction heated 20CrMnTi steel seamless round tube is cooled to 380°C at a rate of 50°C / s by passing through water, and then naturally cooled to room temperature in air to obtain a finished 20CrMnTi steel building pipe.

[0022] The main mechanical properties of the pipe were measured by longitudinal tensile test and are shown in Table 1. It can be seen that the yield strength (R p0.2 ) is 531MPa, the tensile strength is 1144MPa, the elongation after break is 14.54%, and the yield strength ratio is 0.46. Example 2

[0023] The 20CrMnTi steel building pipe in this embodiment is a high-frequency resistance welded round steel pipe with a wall thickness of 3.5 mm and a diameter of 25 mm. The heat treatment method is specifically described as follows.

[0024] (1) Induction heating step: The 20CrMnTi steel high frequency resistance welded circular steel pipe is heated to 860° C. at a rate of 23° C. / s by induction heating.

[0025] (2) Controlled cooling step: The 20CrMnTi steel high-frequency resistance welded circular steel pipe after induction heating is cooled to 400°C at a rate of 45°C / s by passing through water, and then naturally cooled to room temperature in air to obtain a finished 20CrMnTi steel building pipe.

[0026] The main mechanical properties of the pipe were measured by longitudinal tensile test and are shown in Table 1. It can be seen that the yield strength (R p0.2 ) is 523MPa, the tensile strength is 1127MPa, the elongation after break is 13.16%, and the yield strength ratio is 0.46. Example 3

[0027] The 20CrMnTi steel building pipe in this embodiment is a high-frequency resistance welded rectangular steel pipe with a wall thickness of 5.5 mm and a cross-sectional size of 140 mm×80 mm. The heat treatment method is specifically described as follows.

[0028] (1) Induction heating step: The 20CrMnTi steel high frequency resistance welded rectangular steel pipe is heated to 880° C. at a rate of 15° C. / s by induction heating.

[0029] (2) Controlled cooling step: The 20CrMnTi steel high-frequency resistance welded circular steel pipe after induction heating is cooled to 360°C at a rate of 35°C / s by spraying water, and then naturally cooled to room temperature in air to obtain a finished 20CrMnTi steel building pipe.

[0030] By cutting A50 plate-shaped tensile specimens along the longitudinal direction of the pipe and conducting tensile tests on them, the main mechanical properties measured are shown in Table 1. It can be seen that the yield strength (R p0.2 ) is 542MPa, the tensile strength is 1163MPa, the elongation after break is 12.47%, and the yield strength ratio is 0.47. Example 4

[0031] The 20CrMnTi steel building pipe in this embodiment is a round seamless steel pipe with a wall thickness of 3.0 mm and an outer diameter of 50 mm. The heat treatment method is specifically described as follows.

[0032] (1) Induction heating step: The 20CrMnTi steel seamless pipe is heated to 900° C. at a rate of 20° C. / s by induction heating.

[0033] (2) Controlled cooling step: The induction heated 20CrMnTi steel round seamless steel pipe is cooled to 360°C at a rate of 40°C / s by spraying water, and then naturally cooled to room temperature in air to obtain a finished 20CrMnTi steel building pipe.

[0034] The main mechanical properties of the pipe were measured by longitudinal tensile test and are shown in Table 1. It can be seen that the yield strength (R p0.2 ) is 528MPa, the tensile strength is 1101MPa, the elongation after break is 13.36%, and the yield strength ratio is 0.48. Example 5

[0035] The 20CrMnTi steel building pipe in this embodiment is a round high-frequency resistance welded steel pipe with a wall thickness of 4.0 mm and an outer diameter of 100 mm. The heat treatment method is specifically described as follows.

[0036] (1) Induction heating step: The 20CrMnTi steel circular high-frequency resistance welded steel pipe is heated to 860° C. at a rate of 25° C. / s by induction heating.

[0037] (2) Controlled cooling step: The 20CrMnTi steel high-frequency resistance welded circular steel pipe after induction heating is cooled to 380°C at a rate of 30°C / s by spraying water, and then naturally cooled to room temperature in air to obtain a finished 20CrMnTi steel building pipe.

[0038] The main mechanical properties of the pipe were measured by longitudinal tensile test and are shown in Table 1. It can be seen that the yield strength (R p0.2 ) is 513MPa, the tensile strength is 1138MPa, the elongation after break is 12.68%, and the yield strength ratio is 0.45. Example 6

[0039] The 20CrMnTi steel building pipe in this embodiment is a high-frequency resistance welded rectangular steel pipe with a wall thickness of 4.75 mm and a cross-sectional size of 60 mm×60 mm. The heat treatment method is specifically described as follows.

[0040] (1) Induction heating step: The 20CrMnTi steel high frequency resistance welded rectangular steel pipe is heated to 880° C. at a rate of 28° C. / s by induction heating.

[0041] (2) Controlled cooling step: The 20CrMnTi steel high-frequency resistance welded circular steel pipe after induction heating is cooled to 370°C at a rate of 35°C / s by spraying water, and then naturally cooled to room temperature in air to obtain a finished 20CrMnTi steel building pipe.

[0042] By cutting A50 plate-shaped tensile specimens along the longitudinal direction of the pipe and conducting tensile tests on them, the main mechanical properties measured are shown in Table 1. It can be seen that the yield strength (R p0.2 ) is 546MPa, the tensile strength is 1162MPa, the elongation after break is 14.33%, and the yield strength ratio is 0.47.

[0043] Table 1 Mechanical properties of 20CrMnTi steel building pipes in Examples 1-5

[0044] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A toughening heat treatment process suitable for 20CrMnTi steel building pipes, characterized in that: The heat treatment process comprises two steps of heating and controlled cooling; in the heating step, the 20CrMnTi steel construction pipe is heated to 860-900°C at a rate of 15-30°C / s.

2. A toughening heat treatment process for 20CrMnTi steel building pipes according to claim 1, characterized in that: In the heating step, the heating method is induction heating.

3. A toughening heat treatment process for 20CrMnTi steel building pipes according to claim 1, characterized in that: In the controlled cooling step, the 20CrMnTi steel building pipe after induction heating is cooled to 360-400°C at a rate of 30-50°C / s, and then naturally cooled to room temperature in air to obtain a finished building pipe.

4. A toughening heat treatment process for 20CrMnTi steel building pipes according to any one of claims 1 to 3, characterized in that: In the controlled cooling step, the cooling method is water spray cooling or water penetration cooling.

5. A toughening heat treatment process for 20CrMnTi steel building pipes according to any one of claims 1 to 3, characterized in that: The 20CrMnTi steel building pipe obtained by the heat treatment process has a yield strength of 500-550MPa and a tensile strength of 1100-1180MPa.

6. A toughening heat treatment process for 20CrMnTi steel building pipes according to any one of claims 1 to 3, characterized in that: The 20CrMnTi steel building pipe obtained by the heat treatment process has an elongation after fracture of ≥12% and a yield strength ratio of ≤0.

5.

7. A toughening heat treatment process for 20CrMnTi steel building pipes according to any one of claims 1 to 3, characterized in that: The heat treatment process is applicable to 20CrMnTi steel building pipes with a wall thickness specification of 3.0 to 5.5 mm.

Citation Information

Patent Citations

  • Production process of rebar for concrete

    CN102061370A

  • Method for manufacturing transformation induced plasticity steel seamless tube on line

    CN102363833A

  • Crankshaft timing gear manufacturing method

    CN103056628A

  • Manufacturing technology of scraper of special scraper conveyer for coal mine