Method for extracting gallium in short process
Through short process methods, including acid leaching, reduction, alkaline leaching and electrolytic treatment, the problem of long gallium extraction process and high cost is solved, efficient enrichment and removal of gallium is achieved, and the obtained gallium products meet industrial standards.
Patent Information
- Application Number
- CN202410800822.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-08
AI Technical Summary
The existing gallium extraction method has a long process and high cost, and the gallium extraction efficiency in the vanadium extraction tailings in the Panxi area is low, making it impossible to achieve industrialization.
A short process method is adopted, including acid leaching treatment, reduction treatment, solid-liquid separation, alkaline leaching and electrolysis treatment. By adjusting the pH value and using strong oxidants for iron ion precipitation, the efficient enrichment and removal of gallium is achieved.
The gallium extraction process is shortened, the purity of by-products is improved, and the economic value is increased. The obtained metallic gallium meets industrial standards and is easy to use.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of extraction of metallic gallium, and in particular relates to a method for extracting gallium in a short process. Background Art
[0002] Rare metal gallium is an important strategic resource. A series of compound semiconductor materials, electronic optical materials, new functional materials, special alloys and organic metal compounds prepared with gallium metal as the matrix are important basic supporting materials in the fields of modern electronic computers, communications, aerospace, new energy, medicine and health, military industry and other high-tech fields. At present, about 90% of the gallium in the world is recovered from the production process of alumina, with a mature industrial chain. At the same time, gallium is also enriched in the process of smelting zinc or coal ash, but the gallium enriched in these two raw materials has not been industrialized due to the long extraction process and high cost.
[0003] There are many kinds of valuable metals in the Panxi region of my country. Gallium is associated with V, Fe, Ti and other elements in the Panxi mine. At present, the extraction of gallium is mainly carried out using vanadium tailings as raw materials. In the gallium extraction process, the vanadium tailings have a complex composition, a low direct acid leaching rate, high acid consumption, a large number of by-products that are difficult to use, and a long process route. Therefore, this route has not actually been put into industrial production. In addition, CN106957963A discloses a method for treating vanadium tailings, which can obtain metallic gallium, but due to its complicated steps and poor economic efficiency, it is impossible to realize industrial extraction of gallium. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a method for extracting gallium in a short process, which has a short gallium extraction process and is conducive to industrial production.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] The present invention provides a method for extracting gallium in a short process, comprising:
[0007] S1: subjecting the gallium-containing iron slag to acid leaching, reduction treatment, and solid-liquid separation to obtain a liquid containing gallium and iron;
[0008] S2: mixing the liquid containing gallium and iron with an alkaline substance, adjusting the pH to 2-6, and performing solid-liquid separation to obtain a solid;
[0009] S3: The solid obtained in step S2, 5-30 wt% alkaline solution and a strong oxidant are mixed, and the solid-liquid separation is performed to obtain an alkaline leaching solution, and then impurities are removed, the solid-liquid separation is performed, and the obtained liquid is electrolyzed to obtain metallic gallium.
[0010] Preferably, the gallium-containing iron slag comprises, by mass fraction, 85-95wt% Fe2O3, 0-2wt% SiO2, 1-5wt% ZnO and a combination of any one or more of Na2O, MgO, CaCO3, Al2O3, TiO2, V2O5, Cr2O3, MnO, PbO, CuO, NiO, chlorides or sulfides with a total amount less than 10wt%.
[0011] Preferably, the gallium content in the gallium-containing iron slag is 100-500 g / t.
[0012] Preferably, the acidic reagent used in the acid leaching treatment is any one or more of sulfuric acid, hydrochloric acid, oxalic acid, nitric acid or phosphoric acid.
[0013] Preferably, the concentration of the acid reagent used in the acid leaching treatment is 1 to 8 mol / L.
[0014] Preferably, the mass ratio of the acidic reagent to the gallium-containing iron slag is (0.5-15):1.
[0015] Preferably, the gallium leaching rate after the acid leaching treatment is 90-99%.
[0016] Preferably, the acid leaching treatment time is 0.5 to 6 hours.
[0017] Preferably, the reduction treatment is carried out using any one or more of reduced iron powder, sodium sulfite, ferrous sulfite or ascorbic acid.
[0018] Preferably, the molar ratio of Fe ions to reduced iron powder in the solution obtained after the acid leaching treatment is (0.5-1.1):1.
[0019] Preferably, the mixing pressure in step S2 is 0.1-0.2 MPa, the temperature is 0-60° C., and the time is 0.1-0.5 h.
[0020] Preferably, the mixing pressure in step S3 is 0.1-0.2 MPa, the temperature is 0-50° C., and the time is 0.5-6 h.
[0021] Preferably, the strong oxidizing agent is selected from potassium permanganate.
[0022] Preferably, the liquid-to-solid ratio of the solid obtained in step S2 to the 5-30 wt % alkaline solution is (0.5-20):1.
[0023] Preferably, the amount of the strong oxidant used is 20-30 wt % of the mass of the solid obtained in step S2.
[0024] Preferably, the gallium content in the alkaline leaching solution is above 0.1 g / L.
[0025] Preferably, the anode in the electrolytic treatment is selected from any one of graphite, platinum, stainless steel, lead, silver, titanium alloy, tungsten or molybdenum.
[0026] Preferably, the cathode in the electrolytic treatment is selected from any one of copper-indium alloy, indium-gallium alloy or stainless steel.
[0027] Preferably, the temperature of the electrolytic treatment is 10-90°C.
[0028] Preferably, the current density of the electrolytic treatment is 30 to 1000 A / m 2 .
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present invention provides a short-process method for extracting gallium. Compared with the extraction method in the prior art, the cumbersome operations of stripping and multiple washing are omitted, and the extraction process is shorter. In the present invention, the method firstly performs acid leaching on gallium-containing iron slag to obtain a leachate containing gallium and trivalent iron ions, and then reduces the trivalent iron ions to divalent iron ions through reduction treatment, and obtains a liquid containing gallium and iron through solid-liquid separation; through the first alkaline leaching, part of the divalent iron ions are precipitated to remove, and then a second alkaline leaching treatment is performed using a 5-30wt% alkaline solution. At the same time, a strong oxidant is added in the process to oxidize the divalent iron ions to trivalent iron ions, and the iron ions are precipitated to remove the iron ions. Through the second alkaline leaching treatment, the iron ions can be removed more thoroughly and gallium is enriched. Finally, the alkaline leachate enriched with gallium is subjected to impurity removal and solid-liquid separation, and metallic gallium can be obtained after the liquid is electrolyzed.
[0031] The gallium extraction method provided by the present invention has a short gallium extraction process and good impurity removal effect. At the same time, the by-products produced have high purity and good economic value. After testing, the metal gallium finally obtained meets the GB / T1475-2022 industrial gallium and is easy to use. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In view of the problems in the prior art that the method for extracting gallium is poor in economic efficiency, has complicated steps, and cannot be industrialized, the present invention provides a method for extracting gallium in a short process, comprising:
[0034] S1: subjecting gallium-containing iron slag to acid leaching and reduction treatment and then solid-liquid separation to obtain a liquid containing gallium and iron;
[0035] S2: mixing the liquid containing gallium and iron with an alkaline substance, adjusting the pH to 2-6, and performing solid-liquid separation to obtain a solid;
[0036] S3: The solid obtained in step S2, 5-30 wt% alkaline solution and a strong oxidant are mixed, and the solid-liquid separation is performed to obtain an alkaline leaching solution, and then impurities are removed, the solid-liquid separation is performed, and the obtained liquid is electrolyzed to obtain metallic gallium.
[0037] In the present invention, gallium-containing iron slag is used as the extraction raw material, and the gallium-containing iron slag includes 85-95wt% Fe2O3, 0-2wt% SiO2, 1-5wt% ZnO and a total amount of less than 10wt% of any one or more of Na2O, MgO, CaCO3, Al2O3, TiO2, V2O5, Cr2O3, MnO, PbO, CuO, NiO, chlorides or sulfides in combination; preferably includes 88-90wt% Fe2O3, 0-1.5wt% SiO2, 2-4wt% ZnO and a total amount of less than 10wt% of any one or more of Na2O, MgO, CaCO3, Al2O3, TiO2, V2O5, Cr2O3, MnO, PbO, CuO, NiO, chlorides or sulfides in combination. In the present invention, the gallium content in the gallium-containing iron slag is 100-500 g / t, preferably 250-500 g / t. In some embodiments of the present invention, the gallium-containing iron slag is a vanadium-extracting converter ash waste unique to the vanadium-extracting process of vanadium-titanium magnetite in the Panxi region.
[0038] According to the present invention, the gallium-containing iron slag is first subjected to acid leaching. The acidic reagent used in the acid leaching treatment is any one or more of sulfuric acid, hydrochloric acid, oxalic acid, nitric acid or phosphoric acid. The concentration of the acidic reagent used in the acid leaching treatment is 1 to 8 mol / L, preferably 2 to 6 mol / L, and more preferably 3 to 5 mol / L. Alternatively, the concentration of the acidic reagent is 50 to 500 g / L, preferably 100 to 400 g / L, and more preferably 200 to 300 g / L. In some embodiments of the present invention, the gallium-containing iron slag is treated with the above-mentioned acidic reagent at 5 to 90°C, preferably 10 to 80°C, for acid leaching for 0.5 to 6 hours, preferably 1 to 5 hours, wherein the mass ratio of the acidic reagent to the gallium-containing iron slag is (0.5 to 15):1, preferably (3 to 12):1. The acid leaching treatment is preferably carried out under stirring conditions, the stirring form is not limited, the stirring rate is 0 to 500 rpm, preferably 100 to 400 rpm, and the mixed solution of gallium-containing iron slag and acidic reagent can also be shaken. In the present invention, after the acid leaching treatment is completed, the gallium leaching rate can reach 90 to 99%, preferably 93 to 99%.
[0039] After the acid leaching treatment is completed, the obtained leachate is subjected to reduction treatment according to the present invention. The reduction treatment is preferably carried out using reduced iron powder. In some embodiments of the present invention, the molar ratio of Fe ions to reduced iron powder in the solution obtained after the acid leaching treatment is preferably (0.5-1.1):1, more preferably (0.6-0.9):1, the leachate is mixed with the reduced iron powder, and the reduced iron powder is preferably slowly added to the leachate until the leachate is tested for no color change by thiocyanate, indicating that the trivalent iron ions are reduced to divalent iron ions. In the process of adding the reduced iron powder, stirring and heating can be performed as needed to accelerate the reaction rate of the reduced iron powder with the trivalent iron ions in the leachate. The form of the stirring is not limited, the stirring rate is 0-500rpm, preferably 100-400rpm, and the heating temperature is preferably 0-60°C, preferably 10-50°C. In the present invention, the leachate is subjected to solid-liquid separation after no color change after thiocyanate detection, and the liquid residue containing gallium and divalent iron ions can be separated from the leachate by suction filtration, filter pressing, centrifugation, etc., but is not limited to these separation methods.
[0040] Then, the liquid containing gallium and divalent iron ions obtained in the solid-liquid separation is mixed with an alkaline substance, which can be a solid or a liquid, such as a sodium hydroxide solution, a potassium hydroxide solution, or a sodium hydroxide solid, a potassium hydroxide solid, etc., but is not limited to the above solid and liquid types. The mixing pressure is 0.1-0.2MPa, preferably 0.12-0.15MPa; the temperature is 0-60°C, preferably 10-50°C; the time is 0.1-0.5h, preferably 0.2-0.4h. It should be noted that the mixing time depends on the pressure and temperature. When the pressure and temperature are high, the time can be relatively short.
[0041] It should be noted that in this step, the present invention adds an alkaline substance to perform the first alkaline leaching treatment, and adjusts the pH to 2-6, preferably a solution with a strong alkaline such as sodium hydroxide and potassium hydroxide, so as to ensure sufficient supply of hydroxide ions and make the separation of gallium and iron good and rapid. After the pH value is stabilized, solid-liquid separation is performed, which can be performed by suction filtration, filter pressing, centrifugation, etc., but is not limited to these separation methods. According to the test, the water content of the solid after solid-liquid separation is 40-85wt%.
[0042] After solid-liquid separation, the obtained solid is mixed with 5-30wt% alkaline solution and strong oxidant, and the mixing is preferably carried out under stirring conditions, and the stirring rate is 0-500rpm, preferably 100-400rpm. The stirring form is not limited, and the solution can also be shaken. Wherein, the liquid-to-solid ratio of the solid obtained in step S2 and the 5-30wt% alkaline solution is (0.5-20):1, preferably (1-15):1. The amount of the strong oxidant is 20-30wt% of the mass of the solid obtained in step S2, preferably 22-28wt%. The mixing pressure is 0.1-0.2MPa, preferably 0.15-0.18MPa, the temperature is 0-50°C, preferably 15-30°C, and the time is 0.5-6h, preferably 1-5h. It should be noted that in the first alkaline leaching treatment, the alkali solubility of ferric hydroxide and ferrous hydroxide is low, and gallium is more easily separated in the alkaline solution. In this step, a higher concentration of 5-30wt% alkaline solution is further selected for the second alkaline leaching treatment. At the same time, by adding a strong oxidant in this step, divalent iron can be converted into trivalent iron, which is conducive to the precipitation of iron, thereby accelerating the separation of gallium and iron. Wherein, the strong oxidant is selected from potassium permanganate.
[0043] In some preferred embodiments of the present invention, the alkaline solution of 5 to 30 wt% and the solid obtained in step S2 are preferably mixed in a mass ratio of (0.5 to 20):1, preferably (1 to 15):1, and after potassium permanganate is added and dissolved, the initial concentration of potassium permanganate is 0.2 to 5 g / L, preferably 0.5 to 4 g / L, and more preferably 1 to 3 g / L. It should be noted that if the initial concentration of potassium permanganate is lower than 0.2 g / L, the divalent iron will not be completely oxidized and the separation of gallium and iron will not be complete; on the contrary, if it is higher than 5 g / L, excessive manganese will be introduced, thereby affecting the electrolysis efficiency and purity of subsequent products.
[0044] In some preferred embodiments of the present invention, after the solid obtained in step S2, 5-30 wt% alkaline solution and a strong oxidant are mixed and the solid-liquid separation is performed, the solid is taken and the step is continued to be circulated until the gallium content in the obtained alkaline leaching solution is above 5 g / L, preferably above 8 g / L, in order to achieve the minimum concentration value of electrolytic gallium.
[0045] Finally, according to the present invention, the obtained alkaline leachate is subjected to impurity removal, and this step is mainly to remove heavy metal ions such as lead and zinc. In some embodiments of the present invention, the alkaline leachate is preferably mixed with a water-soluble sulfide salt, and the initial concentration of the water-soluble sulfide salt after dissolution should be controlled at 1 to 20 g / L, preferably 5 to 15 g / L. The water-soluble sulfide salt can be selected from sodium sulfide and / or potassium sulfide. Then, the solid-liquid separation, the waste residue is removed, and the obtained liquid is electrolyzed to obtain metallic gallium.
[0046] The present invention has no particular limitation on the electrolytic treatment, and it can be carried out according to the technical means familiar to those skilled in the art. In some embodiments of the present invention, the anode in the electrolytic treatment is selected from any one of graphite, platinum, stainless steel, lead, silver, titanium alloy, tungsten or molybdenum; the cathode is selected from any one of copper indium alloy, indium gallium alloy or stainless steel. The temperature of the electrolytic treatment is 10 to 90°C, preferably 20 to 80°C. The current and voltage in the electrolytic treatment vary with different types of electrodes, and the current density is usually controlled at 30 to 1000A / m 2 , preferably 100 to 600 A / m 2 The electrolysis process can be a single-stage electrolysis or a multi-stage electrolysis, which depends on the concentration of gallium in the liquid after solid-liquid separation, the electrode selection and the current density selection.
[0047] After testing, the gallium obtained by the above preparation method meets the requirements of GB / T 1475-2022 industrial gallium. Therefore, the present invention uses industrial solid waste as raw materials to realize a high-efficiency and low-cost industrial gallium extraction process.
[0048] In summary, the present invention provides a short-process method for extracting gallium, which uses a short process of trace gallium-containing waste (content below 1000ppm) to extract the valuable element gallium, and after acid leaching, the trivalent iron in the entire solution is reduced to divalent iron, and most of the gallium and iron are separated by adjusting the pH to obtain a gallium-rich material. Unlike the traditional trace element enrichment method, the present invention does not extract or ion exchange the gallium-rich solution, but performs multiple micro-positive pressure alkaline dissolutions on the gallium-rich material and adds an oxidant, and uses the different solubilities of iron hydroxide and gallium hydroxide in the alkaline solution to fully separate the gallium and iron in the solution. The obtained alkaline solution can directly enter the electrolysis process to obtain industrial gallium that complies with GB / T 1475-2022. At the same time, the present invention avoids the use of organic matter, greatly reducing environmental protection and safety issues.
[0049] In order to further illustrate the present invention, the following examples are used to provide a detailed description. The high iron slag used in the following examples of the present invention is a waste of converter ash that is unique to the vanadium extraction process of vanadium-titanium magnetite in the Panxi region.
[0050] Example 1
[0051] The gallium-extracting solid waste involved in this embodiment is high iron slag, the main components of which are 85wt% Fe2O3, 2wt% SiO2, 5wt% ZnO, and the rest are 0.8wt% Na2O, 0.6wt% MgO, 0.7wt% CaCO3, 0.8wt% Al2O3, 0.9wt% TiO2, 0.6wt% V2O5, 0.8wt% Cr2O3, 0.8wt% MnO, 0.7wt% PbO, 0.8wt% CuO, 0.2wt% NiO, 0.2wt% chloride, and 0.1wt% sulfide. The gallium content in high iron slag is 100g / t. The above solid waste is used as raw material to extract gallium, and the method is as follows:
[0052] (1) Leaching solid waste, using sulfuric acid as the leaching agent. The concentration of the leaching agent is 500 g / L. The leaching time is 0.5 h, and the mechanical stirring rate is 500 rpm. The leaching temperature is 5° C., and the liquid-solid ratio is 15. After leaching, the gallium leaching rate can reach 90%;
[0053] (2) After leaching is completed, add reduced iron powder to the leaching solution to reduce the Fe (原料) :Fe (还原铁粉) The molar ratio of 0.5 is 0.5, and the reduced iron powder is slowly added to the leachate under stirring conditions until the leachate has no color change after the thiocyanate detection;
[0054] (3) after the leachate is tested for thiocyanate and no color change is found, solid-liquid separation is performed, and the residue can be separated from the leachate by suction filtration;
[0055] (4) adding sodium hydroxide solution to the liquid after solid-liquid separation to adjust the pH to 2. After the pH value stabilizes, solid-liquid separation is performed by filter pressing, and the water content of the solid after solid-liquid separation is 85wt%;
[0056] (5) After solid-liquid separation, the undried solid in step (4) was added to a 30wt% sodium hydroxide solution for alkaline leaching, the leaching time was 0.5h, the pressure was 0.1MPa, and the stirring rate was 500rpm. The leaching temperature was 50°C, the liquid-solid ratio was 15, and potassium permanganate solid was added to dissolve, and the initial concentration of potassium permanganate in the solution was 0.2g / L;
[0057] (6) After alkaline dissolution, solid-liquid separation is performed, and the alkaline leaching solution is taken at this time, and the solid obtained by the solid-liquid separation in the fourth step is leached again in a cycle, and this step is repeated until the gallium content in the alkaline leaching solution is 5 g / L;
[0058] (7) adding sodium sulfide to an alkaline solution having a gallium content of 5 g / L, and controlling the initial concentration of the sodium sulfide after dissolving in water to be 1 g / L;
[0059] (8) Solid-liquid separation, electrolysis of the solution, and recycling of the precipitated material; during the electrolysis process, the anode material is graphite and the cathode is copper-indium alloy. The electrolysis temperature can be controlled at 90°C and the current density is usually controlled at 30A / m 2 The electrolysis process is one-stage electrolysis, and the gallium content of the product after electrolysis is 5N, which complies with GB / T 1475-2022 industrial gallium.
[0060] Example 2
[0061] The gallium-extracting solid waste involved in this embodiment is high iron slag, the main components of which are 95wt% Fe2O3, 1wt% ZnO, and the rest are 0.6wt% Na2O, 0.5wt% MgO, 0.3wt% CaCO3, 0.1wt% Al2O3, 0.5wt% TiO2, 0.3wt% V2O5, 0.1wt% Cr2O3, 0.5wt% MnO, 0.3wt% PbO, 0.2wt% CuO, 0.1wt% NiO, 0.3wt% chloride, and 0.2wt% sulfide. The gallium content of high iron slag is 500g / t. The above solid waste is used as raw material to extract gallium, and the method is as follows:
[0062] (1) Leaching solid waste, using a mixed acidic leaching agent of hydrochloric acid and nitric acid, wherein hydrochloric acid accounts for 90wt% and nitric acid accounts for 10wt%. The concentration of the leaching agent is 8mol / L. The leaching time is 6 hours without stirring. The leaching temperature is 90°C and the liquid-solid ratio is 15. After leaching, the gallium leaching rate can reach 99%;
[0063] (2) After leaching is completed, add reduced iron powder to the leaching solution to reduce the Fe (原料) :Fe (还原铁粉) The molar ratio of the reduced iron powder to the leaching solution is 1.1. The reduced iron powder is slowly added to the leaching solution under stirring until the leaching solution has no color change after thiocyanate detection; during the process of adding the reduced iron powder, stirring (200 rpm) and heating (40° C.) are performed to accelerate the reaction rate of the reduced iron powder with the trivalent iron in the leaching solution;
[0064] (3) after the leachate is tested for thiocyanate and no color change is observed, solid-liquid separation is performed, and the residue is separated from the leachate by centrifugation;
[0065] (4) adding potassium hydroxide solid to the liquid after solid-liquid separation to adjust the pH to 6. After the pH value stabilizes, solid-liquid separation is performed by suction filtration, and the water content of the solid after solid-liquid separation is 40 wt%;
[0066] (5) After solid-liquid separation, the undried solid from the fourth step was added to a 5wt% sodium hydroxide solution for alkaline leaching. The leaching time was 6 hours, the pressure was 0.2MPa, the initial concentration of the alkaline solution was 1mol / L, and it was left to stand without stirring. The leaching temperature was 0°C, the liquid-solid ratio was 0.5, and after potassium permanganate solid was added and dissolved, the initial concentration of potassium permanganate in the solution was 5g / L;
[0067] (6) After alkaline dissolution, solid-liquid separation is performed, and the alkaline leaching solution at this time is taken and recycled to leach the solid obtained by the solid-liquid separation in the fourth step again, and this step is recycled until the gallium content in the alkaline leaching solution is 8 g / L;
[0068] (7) adding potassium sulfide to an alkaline solution having a gallium content of 8 g / L, and controlling the initial concentration of potassium sulfide after dissolving in water to be 20 g / L;
[0069] (8) Solid-liquid separation, electrolysis of the solution, and recycling of the precipitated material. During the electrolysis process, the anode material is stainless steel and the cathode is indium gallium alloy. The electrolysis temperature is controlled at 10°C and the current density is controlled at 1000A / m 2 The electrolysis process can be two-stage electrolysis. The product after electrolysis is 3N gallium, which complies with GB / T 1475-2022 industrial gallium.
[0070] Comparative Example 1
[0071] The gallium-extracting solid waste involved in this comparative example is high iron slag, the main components of which are 85wt% Fe2O3, 2wt% SiO2, 5wt% ZnO, and the rest are 0.8wt% Na2O, 0.6wt% MgO, 0.7wt% CaCO3, 0.8wt% Al2O3, 0.9wt% TiO2, 0.6wt% V2O5, 0.8wt% Cr2O3, 0.8wt% MnO, 0.7wt% PbO, 0.8wt% CuO, 0.2wt% NiO, 0.2wt% chloride, and 0.1wt% sulfide. The gallium content in high iron slag is 100g / t. The above solid waste is used as raw material to extract gallium, and the method is as follows:
[0072] (1) Leaching solid waste, using sulfuric acid as the leaching agent. The concentration of the leaching agent is 500 g / L. The leaching time is 0.5 h, and the mechanical stirring rate is 500 rpm. The leaching temperature is 5° C., and the liquid-solid ratio is 15. After leaching, the gallium leaching rate can reach 90%;
[0073] (2) After leaching is completed, add reduced iron powder to the leaching solution to reduce the Fe (原料) :Fe (还原铁粉) The molar ratio of 0.5 is 0.5, and the reduced iron powder is slowly added to the leachate under stirring conditions until the leachate has no color change after the thiocyanate detection;
[0074] (3) after the leachate is tested for thiocyanate and no color change is found, solid-liquid separation is performed, and the residue can be separated from the leachate by suction filtration;
[0075] (4) adding sodium hydroxide solution to the liquid after solid-liquid separation to adjust the pH to 2. After the pH value stabilizes, solid-liquid separation is performed by filter pressing, and the water content of the solid after solid-liquid separation is 85wt%;
[0076] (5) After solid-liquid separation, the undried solid in step (4) was added to a 30wt% sodium hydroxide solution for alkaline leaching, with a leaching time of 0.5h, a pressure of 0.1MPa, and a stirring rate of 500rpm. The leaching temperature was 50°C, and the liquid-solid ratio was 15;
[0077] (6) After alkaline dissolution, solid-liquid separation is performed, and the alkaline leaching solution at this time is taken and recycled to leach the solid obtained by the solid-liquid separation in the fourth step again, and this step is recycled until the gallium content in the alkaline leaching solution is 0.1 g / L;
[0078] (7) adding sodium sulfide to an alkaline solution having a gallium content of 0.1 g / L, and controlling the initial concentration of the sodium sulfide after dissolving in water to be 1 g / L;
[0079] (8) Solid-liquid separation, electrolysis of the solution, and recycling of the precipitated material. During the electrolysis process, the anode and cathode are made of stainless steel. The electrolysis temperature is controlled at 50°C and the current density is controlled at 600A / m 2 However, due to the lack of addition of strong oxidants, the separation of gallium and iron was not complete, and the gallium content after electrolysis was only 2N, which did not meet the GB / T 1475-2022 industrial gallium standard.
[0080] Comparative Example 2
[0081] The gallium-extracting solid waste involved in this comparative example is high iron slag, the main components of which are 95wt% Fe2O3, 1wt% ZnO, and the rest are 0.6wt% Na2O, 0.5wt% MgO, 0.3wt% CaCO3, 0.1wt% Al2O3, 0.5wt% TiO2, 0.3wt% V2O5, 0.1wt% Cr2O3, 0.5wt% MnO, 0.3wt% PbO, 0.2wt% CuO, 0.1wt% NiO, 0.3wt% chloride, and 0.2wt% sulfide. The gallium content of high iron slag is 500g / t. The above solid waste is used as raw material to extract gallium, and the method is as follows:
[0082] (1) Leaching solid waste, using a mixed acidic leaching agent of hydrochloric acid and nitric acid, wherein hydrochloric acid accounts for 90wt% and nitric acid accounts for 10wt%. The concentration of the leaching agent is 8mol / L. The leaching time is 6 hours without stirring. The leaching temperature is 90°C and the liquid-solid ratio is 15. After leaching, the gallium leaching rate can reach 99%;
[0083] (2) After leaching is completed, add reduced iron powder to the leaching solution to reduce the Fe (原料) :Fe (还原铁粉) The molar ratio of the reduced iron powder to the leaching solution is 1.1. The reduced iron powder is slowly added to the leaching solution under stirring until the leaching solution has no color change after thiocyanate detection; during the process of adding the reduced iron powder, stirring (200 rpm) and heating (40° C.) are performed to accelerate the reaction rate of the reduced iron powder with the trivalent iron in the leaching solution;
[0084] (3) after the leachate is tested for thiocyanate and no color change is observed, solid-liquid separation is performed, and the residue is separated from the leachate by centrifugation;
[0085] (4) adding potassium hydroxide solid to the liquid after solid-liquid separation to adjust the pH to 6. After the pH value stabilizes, solid-liquid separation is performed by suction filtration, and the water content of the solid after solid-liquid separation is 40 wt%;
[0086] (5) After solid-liquid separation, the undried solid from the fourth step was added to a 5wt% sodium hydroxide solution for alkaline leaching. The leaching time was 6 hours, the pressure was 0.2MPa, the initial concentration of the alkaline solution was 1mol / L, and it was left to stand without stirring. The leaching temperature was 0°C, the liquid-solid ratio was 0.5, and after potassium permanganate solid was added and dissolved, the initial concentration of potassium permanganate in the solution was 5g / L;
[0087] (6) After alkaline dissolution, solid-liquid separation is performed, and the alkaline leaching solution at this time is taken and recycled to leach the solid obtained by the solid-liquid separation in the fourth step again, and this step is recycled until the gallium content in the alkaline leaching solution is 2 g / L;
[0088] (7) adding potassium sulfide to an alkaline solution having a gallium content of 2 g / L, and controlling the initial concentration of potassium sulfide after dissolving in water to be 20 g / L;
[0089] (8) Solid-liquid separation, electrolysis of the solution, and recycling of the precipitated material. During the electrolysis process, the anode material is stainless steel and the cathode is indium gallium alloy. The electrolysis temperature is controlled at 30°C and the current density is controlled at 500A / m 2 Since the initial concentration of gallium in the alkaline leaching solution is too low, the hydrogen evolution reaction is severe and gallium products cannot be electrolyzed.
[0090] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for extracting gallium in a short process, characterized in that: include: S1: subjecting gallium-containing iron slag to acid leaching and reduction treatment and then solid-liquid separation to obtain a liquid containing gallium and iron; S2: mixing the gallium- and iron-containing liquid with an alkaline substance, adjusting the pH to 2 to 6, and performing solid-liquid separation to obtain a solid; S3: mixing the solid obtained in step S2, 5-30 wt% alkaline solution and a strong oxidant, performing solid-liquid separation to obtain an alkaline leaching solution, removing impurities, performing solid-liquid separation, and electrolyzing the liquid to obtain metallic gallium; The gallium content in the alkaline leaching solution is above 5 g / L.
2. The method for extracting gallium in a short process according to claim 1, characterized in that: The gallium-containing iron slag comprises, by mass fraction, 85-95wt% Fe2O3, 0-2wt% SiO2, 1-5wt% ZnO, and a total amount of less than 10wt% of any one or more of Na2O, MgO, CaCO3, Al2O3, TiO2, V2O5, Cr2O3, MnO, PbO, CuO, NiO, chlorides or sulfides; The gallium content in the gallium-containing iron slag is 100-500 g / t.
3. The method for extracting gallium in a short process according to claim 1 or 2, characterized in that: The acidic reagent used in the acid leaching treatment is any one or more of sulfuric acid, hydrochloric acid, oxalic acid, nitric acid or phosphoric acid; The concentration of the acid reagent used in the acid leaching treatment is 1 to 8 mol / L.
4. The method for extracting gallium in a short process according to claim 3, characterized in that: The mass ratio of the acidic reagent to the gallium-containing iron slag is (0.5-15):1; The gallium leaching rate after the acid leaching treatment is 90-99%; The acid leaching treatment time is 0.5 to 6 hours.
5. The method for extracting gallium in a short process according to any one of claims 1 to 4, characterized in that: The reduction treatment is carried out by using any one or more of reduced iron powder, sodium sulfite, ferrous sulfite or ascorbic acid; The molar ratio of Fe ions to reduced iron powder in the solution obtained after the acid leaching treatment is (0.5-1.1):
1.
6. The method for extracting gallium in a short process according to claim 1 or 2, characterized in that: The mixing pressure in step S2 is 0.1-0.2 MPa, the temperature is 0-60° C., and the time is 0.1-0.5 h; The mixing pressure in step S3 is 0.1-0.2 MPa, the temperature is 0-50° C., and the time is 0.5-6 h.
7. The method for extracting gallium in a short process according to any one of claims 1 to 6, characterized in that: The strong oxidant is selected from any one or more of potassium permanganate, hydrogen peroxide, potassium dichromate or persulfate.
8. The method for extracting gallium in a short process according to any one of claims 1 to 7, characterized in that: The liquid-to-solid ratio of the solid obtained in step S2 and the 5-30 wt % alkaline solution is (0.5-20):1; The amount of the strong oxidant used is 20-30 wt % of the mass of the solid obtained in step S2.
9. The method for extracting gallium in a short process according to any one of claims 1 to 8, characterized in that: The gallium content in the alkaline leaching solution is above 8 g / L.
10. The method for extracting gallium in a short process according to any one of claims 1 to 9, characterized in that: The anode in the electrolytic treatment is selected from any one of graphite, platinum, stainless steel, lead, silver, titanium alloy, tungsten or molybdenum; The cathode in the electrolytic treatment is selected from any one of copper-indium alloy, indium-gallium alloy or stainless steel; The temperature of the electrolytic treatment is 10 to 90° C. The current density of the electrolytic treatment is 30 to 1000 A / m 2 .