Method for preparing low-impurity rare earth feed liquid by self-mixing rare earth carbonate

Through the mixing, transformation activation and acid-controlled dissolution of self-mixing rare earth carbonates, combined with the use of adsorbents, the problem of removing impurities such as aluminum in the rare earth material liquid is solved, and the efficient preparation of low-impurity rare earth material liquid is achieved, reducing the It reduces production costs and process complexity, and improves rare earth separation capabilities and product quality.

CN118745531APending Publication Date: 2024-10-08CHINA MINMETALS BEIJING RES INST OF RE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410714137.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

It is difficult to balance the aluminum impurity removal rate and rare earth loss in the rare earth material liquid with the existing technology, and the production cost is high and the process flow is complex, making it difficult to achieve efficient preparation of low impurity rare earth material liquid.

Method used

A method of preparing low-impurity rare earth liquids using self-mixing rare earth carbonates, through mixing and slurrying, transformation activation, controlled acid dissolution and solid-liquid separation, combined with the use of adsorbents, to control the pH value and acidic dissolution reaction to achieve aluminum, Low-content removal of iron, uranium, thorium and other impurities simplifies the process flow.

Benefits of technology

It has achieved a significant reduction in the content of impurities such as aluminum, iron, uranium and thorium in the rare earth material liquid, saved production costs, simplified the process flow, improved the rare earth separation capacity and product quality, and reduced the extraction cost and radioactive content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745531A_ABST
    Figure CN118745531A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing low-impurity rare earth feed liquid by self-mixing rare earth carbonate, which comprises the following steps of: mixing a mixed rare earth carbonate raw material, an adsorbent and an activating agent according to a proportion in a size mixing process, and increasing the solubility difference between rare earth and non-rare earth impurities such as aluminum, iron, uranium, thorium and the like through transformation activation treatment; the dissolution of impurity elements such as aluminum and the like is effectively inhibited in combination with an acid-controlled dissolution reaction process; a small amount of non-rare earth impurities dissolved out along with rare earth in the dissolving process can be precipitated and adsorbed on the surface of the adsorbent through pH value control in the dissolving process, dissolving and impurity removal can be carried out synchronously, feed liquid is further purified, and then low-impurity rare earth feed liquid is directly prepared through solid-liquid separation. The filter residue is recycled as an adsorbent after being soaked and regenerated by dilute acid. The method provided by the invention can be used for preparing the rare earth feed liquid with low content of common non-rare earth impurities such as aluminum, iron, uranium and thorium, and is beneficial to the proceeding of a rare earth separation process and the improvement of product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rare earth hydrometallurgy, and in particular relates to a method for preparing low-impurity rare earth liquid from mixed rare earth carbonate. Background Art

[0002] Ionic adsorption rare earth ores are currently mined mainly by in-situ leaching. The low-concentration rare earth sulfate leaching mother liquor is usually precipitated into carbonate or oxalate, and then burned to obtain mixed rare earth oxide concentrate. Among them, the rare earth oxide concentrate obtained by oxalate precipitation has a low impurity content, but the cost is relatively high; while the carbonate of mixed rare earth can be used without burning into oxides, and the production cost is relatively low, but the content of impurities such as aluminum is higher.

[0003] Ionic rare earth ore separation production uses the above-mentioned mixed rare earth oxides or carbonate concentrates as raw materials, and produces rare earth oxide products of required specifications through processes such as raw material dissolution, impurity removal, extraction separation, precipitation conversion and calcination. Among them, in order to ensure the working conditions of the extraction and separation process, the feed liquid obtained by dissolving the mixed rare earth concentrate, including the feed liquid obtained by dissolving the rare earth oxides in the oxalate precipitation path, needs to be purified and impurities such as aluminum and iron are removed, and the removal of aluminum impurities is particularly critical.

[0004] Some methods have been developed to utilize the different precipitation pHs of rare earth and aluminum hydroxide to remove aluminum impurities from rare earth feed solutions by alkaline precipitation. The Chinese patent "Southern Ionic Rare Earth Ore Leaching Solution Impurity Removal Process (Application No. CN201610406145.0)" uses alkali solution to treat rare earth concentrates after rare earths are enriched in the mine leachate with magnesium oxide precipitation, and removes aluminum impurities therein, and produces A1(0H)3 products. This method has a higher rare earth recovery rate than traditional processes. The Chinese patent "A New Method for Neutralizing and Removing Aluminum from Rare Earth Feed and High-Value Utilization of Aluminum Resources (Application No. CN 201910791350.7)" uses alkaline solution to neutralize and remove aluminum from rare earth feed solutions, and by strengthening process control conditions, achieves complete removal of aluminum at a lower pH, and prepares pseudo-boehmite products, achieving efficient recovery of rare earth valuable elements and commercialization of aluminum impurities. The Chinese patent "A method for removing impurities from rare earth leaching solution (application number CN 202010430679.3)" adopts the method of adding alkaline solution to the rare earth leaching solution by atomization feeding to adjust the pH and precipitate to remove iron, aluminum, and silicon impurities to obtain a rare earth leaching solution with low impurity content and an impurity precipitate slag with low rare earth content. The method has the advantages of simple process, low cost, high impurity removal rate, good filtration performance of precipitate slag, and low rare earth content in slag.

[0005] CN202111439114.2)" provides a method for purifying and removing impurities by adding coconut oil glucoside as a complexing impurity remover to an ionic rare earth ore leachate to adjust the pH value, which can significantly solve the problems of difficulty in removing impurity ions in rare earth leachate, high rare earth loss rate in the impurity removal process, and serious ammonia nitrogen pollution. However, when using the hydroxide precipitation method to remove aluminum impurities, it is difficult to balance the aluminum impurity removal rate and rare earth loss. Usually, in order to reduce the rare earth loss, it is difficult to effectively remove aluminum impurities.

[0006] There are also some methods that utilize the different extraction orders of rare earth and aluminum in different extraction systems to achieve the removal of aluminum impurities in rare earth feed liquid. The Chinese patent "A method for removing aluminum from rare earth feed liquid (application number CN 201010547720.1)" discloses a method for extracting and removing aluminum from rare earth feed liquid using cyclopentane acid-alcohol-kerosene as an organic phase. The method has low aluminum removal cost, high rare earth recovery rate, convenient operation and control, simple process, and low equipment investment. The Chinese patent "A method for continuously removing impurities from rare earth chloride feed liquid using an extraction tank (application number CN 201711230682.5)" provides a method for continuously removing impurities from rare earth chloride feed liquid using an extraction tank. Using a special extractant, the iron ion, aluminum ion and heavy metal ion impurities in the rare earth feed liquid can be effectively reduced. In the above methods, especially the cyclopentane acid extraction system, it is required that the pH value of the rare earth chloride feed liquid must be strictly controlled during the extraction process, otherwise it is easy to emulsify, which seriously affects the production conditions. Summary of the invention

[0007] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate. Starting from the mixed rare earth carbonate, the low-impurity rare earth liquid is directly prepared through mixing and slurry adjustment, transformation activation, controlled acid dissolution, and solid-liquid separation. The content of common non-rare earth impurities such as aluminum, iron, uranium, and thorium in the prepared rare earth liquid can be lower, especially the content of aluminum is lower; and there is no need to burn the mixed rare earth carbonate to rare earth oxides, thereby saving production costs and shortening the process flow.

[0008] To achieve the above purpose, the technical solution adopted by the present invention is: a method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate, the method comprising the following steps:

[0009] S1. Mixing and slurry preparation: Mixing the mixed rare earth carbonate, the adsorbent and the activator in proportion to make them uniformly mixed to prepare a slurry material;

[0010] S2, transformation activation: heating the slurry to the transformation activation reaction temperature and maintaining it for a certain period of time to obtain an activated material;

[0011] S3, acid controlled dissolution: slurrying the activated material with clean water to a solid-liquid ratio of 1:3 to 1:10, and then adding an acidic solution thereto for dissolution reaction, and controlling the pH value of the dissolution reaction system to avoid dissolution of impurities such as aluminum, thereby obtaining a low-impurity rare earth liquid;

[0012] S4, solid-liquid separation: the dissolution reaction system in step S3 is subjected to solid-liquid separation, the filtrate is the low-impurity rare earth feed liquid, and the filter residue is mainly the added adsorbent;

[0013] S5, adsorbent regeneration: soak the filter residue in step S4 in a dilute acid solution, and the regenerated adsorbent is recycled in step S1.

[0014] Furthermore, the raw material of the mixed rare earth carbonate is selected from one or more of light rare earth ore, southern yttrium-poor ore, medium yttrium or yttrium-rich rare earth ore.

[0015] Further, the activator is selected from MC1 X 、N(NO3) Y One or more types of activators;

[0016] Wherein, X and Y are each independently selected from 1, 2 or 3;

[0017] M and N are each independently selected from H + NH4 + , Ca 2+ Mg 2+ , Fe 3+ 、A1 3+ or Re 3+ .

[0018] Furthermore, the molar ratio of the activator to the rare earth element in the mixed rare earth carbonate is 1:10 to 5:1.

[0019] Furthermore, the adsorbent is a cerium-based material, including one or more of cerium dioxide, cerium hydroxide, cerium dioxide-non-cerium rare earth composite materials, cerium hydroxide-non-cerium rare earth composite materials, cerium dioxide-non-rare earth metal composite materials, cerium hydroxide-non-rare earth metal composite materials, cerium dioxide-containing slag, and cerium hydroxide-containing slag.

[0020] Furthermore, the mass ratio of the adsorbent to the mixed rare earth carbonate is 1:100 to 1:1.

[0021] Furthermore, in step S2, the transformation activation reaction temperature is 200-300° C., and the activation reaction time of the slurry material at the transformation activation reaction temperature is 1-240 hours to obtain an activated material.

[0022] Further, in step S3, the acidic solution is a hydrochloric acid solution and / or a nitric acid solution, and the total concentration of the acidic solution is 1 to 10 mol / L.

[0023] Furthermore, in step S3, the temperature of the dissolution reaction is 20 to 90° C.; and the time of the dissolution reaction is 1 to 8 hours.

[0024] Furthermore, in step S3, the specific method for controlling the pH value of the dissolution reaction system is: controlling the pH value of the dissolution reaction system to be between 3 and 5 when the end point of the dissolution reaction is reached.

[0025] Further, in step S4, the impurities in the low-impurity rare earth solution include aluminum, iron, uranium, and thorium, wherein the aluminum content is 1-300 mg / L, the iron content is 1-100 mg / L, the uranium content is 0.01-5 mg / L, and the thorium content is 0.01-20 mg / L.

[0026] Further, in step S5, the dilute acid solution is a hydrochloric acid solution and / or a nitric acid solution, and the total concentration of the dilute acid solution is 0.001 to 10 mol / L.

[0027] The beneficial effects of the present invention are: the method for preparing a low-impurity rare earth liquid from a self-mixed rare earth carbonate provided by the present invention can prepare a low-impurity rare earth liquid with lower content of common non-rare earth impurities such as aluminum, iron, uranium, and thorium, especially lower content of aluminum. The beneficial effects of the present invention are specifically embodied in:

[0028] (1) Low-impurity rare earth liquid can be directly prepared from mixed rare earth carbonates without burning them into rare earth oxides for use, thus saving production costs and simplifying the process;

[0029] (2) The solubility difference between rare earth and non-rare earth impurities such as aluminum, iron, uranium, and thorium is increased through transformation and activation treatment, and the dissolution of impurity elements such as aluminum is effectively suppressed in combination with the controlled acid dissolution reaction process;

[0030] (3) During the dissolution process, a small amount of non-rare earth impurities dissolved with rare earth can be precipitated and adsorbed on the adsorbent surface by controlling the pH value during the dissolution process, so that dissolution and impurity removal can be carried out simultaneously, so that the feed liquid can be further purified;

[0031] (4) The preparation of low-impurity rare earth liquid is beneficial to the rare earth separation process, increases the extraction and separation capacity, and reduces the extraction cost;

[0032] (5) The prepared low-impurity rare earth liquid has lower uranium and thorium contents, and the radioactivity of the product is reduced.

[0033] The present invention innovatively uses carbonate containing mixed rare earths as raw material, introduces an activator to transform and activate the raw material under certain temperature conditions, thereby increasing the difference in dissolution activity between rare earth elements in the rare earth carbonate and non-rare earth impurities such as aluminum, iron, uranium, thorium, etc., so that in the further controlled acid dissolution process, the rare earths are quickly dissolved, the dissolution of non-rare earth impurities is reduced, and the selective dissolution of rare earths is achieved.

[0034] The method provided by the present invention can produce a rare earth liquid with low content of common non-rare earth impurities such as aluminum, iron, uranium, and thorium, which is conducive to the rare earth separation process and the improvement of product quality. At the same time, the method provided by the present invention is in line with the current process of southern mine separation enterprises, with a short process flow and significant impurity removal effect, and realizes efficient separation of rare earth and impurities such as aluminum; and can save the cost of burning mixed rare earth hydrochloride and the cost of subsequent extraction and separation processes, reduce the overall production cost of rare earth products, and increase product added value. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic flow chart of a method for preparing a low-impurity rare earth liquid from a mixture of rare earth carbonates according to an embodiment of the present invention. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention will be further clearly and completely described below in conjunction with the drawings and embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0037] Most of the existing ionic rare earth ore separation methods remove aluminum impurities after they enter the liquid together with the rare earths during the acid dissolution process. However, if the dissolution of aluminum impurities can be suppressed from the source during the concentrate dissolution process, it should be the most ideal process solution. The Chinese patent "A method for removing aluminum from ionic rare earth concentrates (application number CN 202211726241.5)" adjusts the amount of hydrochloric acid added during acid dissolution and the pH of the acid dissolution system to ensure the rare earth dissolution rate while reducing the aluminum dissolution rate, thereby achieving effective separation of aluminum and the rare earth liquid entering the tank. Chinese patent "A method for preparing a low-impurity rare earth liquid (application number CN 202110178949.0)"

[0038] In order to more effectively inhibit the dissolution of aluminum impurities, the rare earth oxides in the rare earth oxide concentrate were activated while being acid-dissolved, which improved the dissolution activity of the rare earths and magnified the solubility difference between the rare earths and impurities such as aluminum. The low-impurity rare earth liquid prepared by direct acid dissolution has lower contents of common non-rare earth impurities such as aluminum, iron, uranium, and thorium, especially aluminum.

[0039] In a method for directly preparing a low-impurity rare earth feed solution from a mixed rare earth carbonate provided in this embodiment, starting from a rare earth carbonate concentrate, the rare earth carbonate concentrate is activated under certain conditions by adding a rare earth solution, so that the rare earth carbonate is decomposed and transformed, the dissolution activity of the rare earth is improved, and the acid dissolution activity between the rare earth and the main impurity aluminum and the like is increased, so as to achieve the selective dissolution of the rare earth at a relatively low acidity. This method can directly prepare a rare earth solution with low common non-rare earth impurities such as aluminum, iron, and thorium from a mixed rare earth carbonate, and can be used without burning the mixed rare earth carbonate into rare earth oxides, and the prepared feed solution has a lower content of common non-rare earth impurities such as aluminum, iron, uranium, and thorium, especially a lower content of aluminum; it can save production costs and shorten the process flow.

[0040] like Figure 1 As shown, an embodiment of the present invention provides a method for directly preparing a low-impurity rare earth liquid from a mixed rare earth carbonate, the method comprising the following steps:

[0041] S1. Mixing and slurry preparation: Mixing the mixed rare earth carbonate, the adsorbent and the activator in proportion to make them uniformly mixed to prepare a slurry material;

[0042] Optionally, the raw material of the mixed rare earth carbonate is selected from one or more of light rare earth ore, southern yttrium-poor ore, medium yttrium or yttrium-rich rare earth ore.

[0043] Optionally, the activator is selected from MC1 X 、N(NO3) Y One or more of the types of activators; wherein X and Y are independently selected from 1, 2 or 3, and X and Y may be equal or unequal; M and N are independently selected from H + NH4 + , Ca 2+ Mg 2+ , Fe 3+ 、A1 3+ or Re 3+ etc., M and N may be the same or different.

[0044] In a specific embodiment, the molar ratio of the activator to the rare earth element in the mixed rare earth carbonate is 1:10 to 5:1.

[0045] Optionally, the adsorbent is a cerium-based material, including one or more of cerium dioxide, cerium hydroxide, cerium dioxide-non-cerium rare earth composite material, cerium hydroxide-non-cerium rare earth composite material, cerium dioxide-non-rare earth metal composite material, cerium hydroxide-non-rare earth metal composite material, slag containing cerium dioxide, slag containing cerium hydroxide; in the adsorbent, cerium dioxide / cerium hydroxide accounts for 1%-100%

[0046] In a specific embodiment, the mass ratio of the adsorbent to the mixed rare earth carbonate is 1:100 to 1:1.

[0047] S2, transformation activation: heating the slurry to the transformation activation reaction temperature and maintaining it for a certain period of time to obtain an activated material;

[0048] Specifically, in step S2, the activator has substantially no activation effect on common non-rare earth impurities such as aluminum, iron, uranium, and thorium in the rare earth carbonate concentrate.

[0049] Optionally, the transformation activation reaction temperature is 200-300° C., and the activation reaction time of the slurry material at the transformation activation reaction temperature is 1-240 hours to obtain an activated material.

[0050] S3, acid controlled dissolution: slurrying the activated material with clean water to a solid-liquid ratio of 1:3 to 1:10, and then adding an acidic solution thereto for dissolution reaction, and controlling the pH value of the dissolution reaction system to avoid dissolution of impurities such as aluminum, thereby obtaining a low-impurity rare earth liquid;

[0051] Optionally, in step S3, the activated material is mixed with an acidic solution of a certain concentration, and a dissolution reaction is carried out at a certain temperature with a controlled pH value. Since the highly active rare earth reacts preferentially with the acid and dissolves quickly, the dissolution of non-rare earth impurities is reduced, thereby achieving selective dissolution of rare earths. At the same time, a small amount of dissolved non-rare earth impurities can be precipitated under high pH conditions and adsorbed on the surface of the adsorbent, thereby obtaining a rare earth solution with low impurities in the solution.

[0052] Optionally, in step S3, the acidic solution is a hydrochloric acid solution and / or a nitric acid solution, and the total concentration of the acidic solution is 1 to 10 mol / L.

[0053] Optionally, in step S3, the temperature of the dissolution reaction is 20 to 90°C; the time of the dissolution reaction is 1 to 8 hours; the specific method for controlling the pH value of the dissolution reaction system is: controlling the pH value of the dissolution reaction system to be between 3 and 5 when the end point of the dissolution reaction is reached.

[0054] S4, solid-liquid separation: the dissolution reaction system in step S3 is subjected to solid-liquid separation, the filtrate is the low-impurity rare earth feed liquid, and the filter residue is mainly the added adsorbent;

[0055] Optionally, in step S4, the dissolution reaction system mixture after controlled acid dissolution is subjected to solid-liquid separation, and the obtained low-impurity rare earth feed liquid is used for subsequent extraction and separation steps.

[0056] Specifically, the impurities in the low-impurity rare earth solution include aluminum, iron, uranium and thorium, wherein the aluminum content is 1 to 300 mg / L, the iron content is 1 to 100 mg / L, the uranium content is 0.01 to 5 mg / L, and the thorium content is 0.01 to 20 mg / L.

[0057] S5, adsorbent regeneration: soak the filter residue in step S4 with a dilute acid solution, and the regenerated adsorbent is recycled in step S1;

[0058] Optionally, in step S5, the dilute acid solution is a hydrochloric acid solution and / or a nitric acid solution, and the total concentration of the dilute acid solution is 0.001 to 10 mol / L.

[0059] The method for directly preparing low-impurity rare earth feed liquid from the self-mixed rare earth carbonate provided by the present embodiment can start from the mixed rare earth carbonate, and the mixed rare earth carbonate raw material, the adsorbent and the activator are mixed in proportion through the mixing and slurrying process, and the solubility difference between the rare earth and non-rare earth impurities such as aluminum, iron, uranium, and thorium is increased through the transformation and activation treatment, and the dissolution of impurity elements such as aluminum is effectively suppressed in combination with the controlled acid dissolution reaction process; a small amount of non-rare earth impurities accompanying the dissolution of rare earth during the dissolution process can be precipitated and adsorbed on the surface of the adsorbent by controlling the pH value during the dissolution process, and the dissolution and impurity removal can be carried out simultaneously, so that the feed liquid is further purified, and then the low-impurity rare earth feed liquid is directly prepared by solid-liquid separation. The method provided in the present embodiment prepares a low-impurity rare earth feed liquid, which is conducive to the rare earth separation process, increases the extraction and separation capacity, and reduces the extraction cost; and the prepared low-impurity rare earth feed liquid has lower uranium and thorium contents, which reduces the radioactivity of the product.

[0060] The specific implementation modes of the present invention are further described below through examples.

[0061] Example 1 When the mixed rare earth carbonate is a mixture of light rare earth ore and southern yttrium ore, the following method steps are used to prepare a low-impurity rare earth liquid

[0062] (1) Mixing and slurry preparation: Mixing the mixed rare earth carbonate, the adsorbent and the activator in proportion to prepare a slurry preparation;

[0063] (2) Transformation activation: heating the slurry to the transformation activation reaction temperature and maintaining it for a certain period of time to obtain an activated material;

[0064] (3) Controlled acid dissolution: The activated material is slurried with water to a solid-liquid ratio of 1:3 to 1:10, and then an acid solution is added thereto for dissolution reaction. By controlling the pH value of the dissolution reaction system, impurities such as aluminum are prevented from being dissolved, thereby obtaining a low-impurity rare earth liquid;

[0065] (4) solid-liquid separation: the dissolution reaction system in step (3) is subjected to solid-liquid separation, the filtrate is the low-impurity rare earth feed liquid, and the filter residue is mainly the added adsorbent;

[0066] (5) Regeneration of adsorbent: soak the adsorbent in step (4) in a dilute acid solution, and regenerate the adsorbent and reuse it in step (1).

[0067] Wherein, the mixed rare earth carbonate is a mixed ore of light rare earth ore and southern yttrium-rich ore.

[0068] The activator is MC1 X 、N(NO3) Y A mixed solution composed of: M and N are NH4 + 、Re 3+ The total cation concentration of M and N is 2.5 mol / L, of which NH4 + The ion concentration is 0.5 mol / L, Re 3+ The ion concentration is 2 mol / L. The activator and the rare earth element of the mixed rare earth carbonate are mixed and reacted in a molar ratio of 5: 1. The adsorbent is cerium dioxide, and the mass ratio of the adsorbent to the mixed rare earth carbonate is 1:100.

[0069] The transformation activation reaction temperature is 200° C., and the transformation activation reaction time is 24 hours.

[0070] The acid solution is 5 mol / L hydrochloric acid. The temperature of the dissolution reaction is 20° C.; the time of the dissolution reaction is 8 hours; and the pH value of the dissolution reaction system is controlled to be 3 when the end point of the dissolution reaction is reached.

[0071] By performing solid-liquid separation by suction filtration, a low-impurity rare earth feed solution with a low impurity content as shown in Table 1 can be prepared; the adsorbent cerium dioxide is regenerated by soaking in 0.01 mol / L hydrochloric acid, and the adsorbent is recycled after regeneration.

[0072] Table 1 Rare earth and impurity concentrations in the prepared rare earth solution

[0073]

[0074] Example 2 When the mixed rare earth carbonate is yttrium ore from the southern mine, the following method steps are used to prepare a low-impurity rare earth feed liquid

[0075] (1) Mixing and slurry preparation: Mixing the mixed rare earth carbonate, the adsorbent and the activator in proportion to prepare a slurry preparation;

[0076] (2) Transformation activation: heating the slurry to the transformation activation reaction temperature and maintaining it for a certain period of time to obtain an activated material;

[0077] (3) Controlled acid dissolution: The activated material is slurried with water to a solid-liquid ratio of 1:3 to 1:10, and then an acid solution is added thereto for dissolution reaction. By controlling the pH value of the dissolution reaction system, impurities such as aluminum are prevented from being dissolved, thereby obtaining a low-impurity rare earth liquid;

[0078] (4) solid-liquid separation: the dissolution reaction system in step (3) is subjected to solid-liquid separation, the filtrate is the low-impurity rare earth feed liquid, and the filter residue is mainly the added adsorbent;

[0079] (5) Regeneration of adsorbent: soak the adsorbent in step (4) in a dilute acid solution, and regenerate the adsorbent and reuse it in step (1).

[0080] Wherein, the mixed rare earth carbonate is yttrium ore from the southern mine.

[0081] The activator is MC1 X solution; where M is Mg 2+ , Fe 3+ , H + The total cation concentration of M is 0.5 mol / L, including Mg 2+ The ion concentration is 0.1 mol / L, Fe 3+ The ion concentration is 0.1 mol / L, H + The ion concentration is 0.3 mol / L. The activator and the rare earth element of the mixed rare earth carbonate are mixed and reacted in a molar ratio of 1:5. The adsorbent is cerium dioxide, and the mass ratio of the adsorbent to the mixed rare earth carbonate is 1:10.

[0082] The transformation activation reaction temperature is 300° C., and the transformation activation reaction time is 1 hour.

[0083] The acid solution is 10 mol / L hydrochloric acid. The temperature of the dissolution reaction is 90°C; the time of the dissolution reaction is 4 hours; the pH value of the dissolution reaction system is controlled to be 5 when the end point of the dissolution reaction is reached. The dissolution rate of rare earth is significantly accelerated during the above-mentioned acid-controlled dissolution process, and the dissolution of impurities such as aluminum, iron, uranium, and thorium is reduced.

[0084] By performing solid-liquid separation by filter pressing, a low-impurity rare earth feed solution with a low impurity content as shown in Table 2 can be prepared; the adsorbent cerium dioxide is regenerated by soaking in 0.01 mol / L hydrochloric acid, and the adsorbent is recycled after regeneration.

[0085] Table 2 Rare earth and impurity concentrations in the prepared rare earth solution

[0086]

[0087] Example 3 When the mixed rare earth carbonate is a yttrium-rich ore from a southern mine, the following method steps are used to prepare a low-impurity rare earth feed solution

[0088] (1) Mixing and slurry preparation: Mixing the mixed rare earth carbonate, the adsorbent and the activator in proportion to prepare a slurry preparation;

[0089] (2) Transformation activation: heating the slurry to the transformation activation reaction temperature and maintaining it for a certain period of time to obtain an activated material;

[0090] (3) Controlled acid dissolution: The activated material is slurried with water to a solid-liquid ratio of 1:3 to 1:10, and then an acid solution is added thereto for dissolution reaction. By controlling the pH value of the dissolution reaction system, impurities such as aluminum are prevented from being dissolved, thereby obtaining a low-impurity rare earth liquid;

[0091] (4) solid-liquid separation: the dissolution reaction system in step (3) is subjected to solid-liquid separation, the filtrate is the low-impurity rare earth feed liquid, and the filter residue is mainly the added adsorbent;

[0092] (5) Regeneration of adsorbent: soak the adsorbent in step (4) in a dilute acid solution, and regenerate the adsorbent and reuse it in step (1).

[0093] Wherein, the mixed rare earth carbonate is the yttrium-rich ore of the southern mine.

[0094] The activator is MC1 X Solution; where M consists of Al 3+ , Fe 3+ 、Re 3+ The total cation concentration of M is 0.12 mol / L, of which Al 3+ The ion concentration is 0.01mol / L, Fe 3+ The ion concentration is 0.01mol / L, Re 3+ The ion concentration is 0.1 mol / L. The activator and the rare earth element in the mixed rare earth carbonate are mixed and reacted in a molar ratio of 2:1. The adsorbent is cerium dioxide, and the mass ratio of the adsorbent to the mixed rare earth carbonate is 1:1.

[0095] The transformation activation reaction temperature is 280° C., and the transformation activation reaction time is 6 hours.

[0096] The acid solution is 8 mol / L hydrochloric acid. The temperature of the dissolution reaction is 60°C; the time of the dissolution reaction is 4 hours; the pH value of the dissolution reaction system is controlled to be 4 when the end point of the dissolution reaction is reached. The dissolution rate of rare earth is significantly accelerated during the above-mentioned acid-controlled dissolution process, and the dissolution of impurities such as aluminum, iron, uranium, and thorium is reduced.

[0097] By performing solid-liquid separation by suction filtration, a low-impurity rare earth feed solution with a low impurity content as shown in Table 3 can be prepared; the adsorbent cerium dioxide is regenerated by soaking in 0.01 mol / L hydrochloric acid, and the adsorbent is recycled after regeneration.

[0098] Table 3 Rare earth and impurity concentrations in the prepared rare earth solution

[0099]

[0100] The method described in the present invention is not limited to the specific embodiments described. The above embodiments are only examples of the present invention. The present invention can also be implemented in other specific ways or other specific forms without departing from the gist or essential features of the present invention. Therefore, the described embodiments should be regarded as illustrative rather than restrictive in any respect. The scope of the present invention should be described by the attached claims, and any changes equivalent to the intent and scope of the claims should also be included in the scope of the present invention.

Claims

1. A method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate, characterized in that: The method comprises the following steps: S1. Mixing and slurry preparation: Mixing the mixed rare earth carbonate, the adsorbent and the activator in proportion to make them uniformly mixed to prepare a slurry material; S2, transformation activation: heating the slurry to the transformation activation reaction temperature and maintaining it for a certain period of time to obtain an activated material; S3, acid controlled dissolution: slurrying the activated material with clean water to a solid-liquid ratio of 1:3 to 1:10, and then adding an acidic solution thereto for dissolution reaction, and controlling the pH value of the dissolution reaction system to avoid dissolution of impurities such as aluminum, thereby obtaining a low-impurity rare earth liquid; S4, solid-liquid separation: the dissolution reaction system in step S3 is subjected to solid-liquid separation, the filtrate is the low-impurity rare earth feed liquid, and the filter residue is mainly the added adsorbent; S5, adsorbent regeneration: soak the filter residue in step S4 in a dilute acid solution, and the regenerated adsorbent is recycled in step S1.

2. The method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to claim 1, characterized in that: The raw material of the mixed rare earth carbonate is selected from one or more of light rare earth ore, southern yttrium-poor ore, medium yttrium or yttrium-rich rare earth ore.

3. The method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to claim 1, characterized in that: The activator is selected from MC1 X 、N(NO3) Y One or more types of activators; Wherein, X and Y are each independently selected from 1, 2 or 3; M and N are each independently selected from H + NH4 + , Ca 2+ Mg 2+ , Fe 3+ 、A1 3+ or Re 3+ .

4. The method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to claim 1, characterized in that: The molar ratio of the activator to the rare earth element in the mixed rare earth carbonate is 1:10 to 5:

1.

5. The method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to claim 1, characterized in that: The adsorbent is a cerium-based material, including one or more of cerium dioxide, cerium hydroxide, cerium dioxide-non-cerium rare earth composite materials, cerium hydroxide-non-cerium rare earth composite materials, cerium dioxide-non-rare earth metal composite materials, cerium hydroxide-non-rare earth metal composite materials, cerium dioxide-containing slag, and cerium hydroxide-containing slag.

6. The method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to claim 1, characterized in that: The mass ratio of the adsorbent to the mixed rare earth carbonate is 1:100 to 1:

1.

7. The method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to claim 1, characterized in that: In step S2, the transformation activation reaction temperature is 200-300°C, and the activation reaction time of the slurry material at the transformation activation reaction temperature is 1-240h to obtain an activated material.

8. The method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to claim 1, characterized in that: In step S3, the acidic solution is a hydrochloric acid solution and / or a nitric acid solution, and the total concentration of the acidic solution is 1 to 10 mol / L.

9. The method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to claim 1, characterized in that: In step S3, the temperature of the dissolution reaction is 20 to 90° C.; the time of the dissolution reaction is 1 to 8 hours.

10. A method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to any one of claims 1 to 9, characterized in that: In step S3, the specific method of controlling the pH value of the dissolution reaction system is: controlling the pH value of the dissolution reaction system to be between 3 and 5 at the end point of the dissolution reaction.

11. The method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to claim 10, characterized in that: In step S4, the impurities in the low-impurity rare earth solution include aluminum, iron, uranium and thorium, wherein the content of aluminum is 1 to 300 mg / L, the content of iron is 1 to 100 mg / L, the content of uranium is 0.01 to 5 mg / L, and the content of thorium is 0.01 to 20 mg / L.

12. The method for preparing a low-impurity rare earth liquid from a mixed rare earth carbonate according to claim 10, characterized in that: In step S5, the dilute acid solution is a hydrochloric acid solution and / or a nitric acid solution, and the total concentration of the dilute acid solution is 0.001 to 10 mol / L.

Citation Information

Patent Citations

  • Ionic type rare-earth fine ore acid leaching process

    CN104328290A

  • Preparation method of low-impurity rare earth solution

    CN113046578A

  • Method for regenerating adsorbent

    JP2007167756A