Preparation method of high-deformation twin crystal density alpha titanium alloy plate

By adding Fe element to Ti-Al-B series titanium alloy and using vacuum consumable melting and high-pass deformation hot rolling process, a high-density deformation twin plate is prepared, which solves the problem of poor strength and toughness matching in titanium alloys. problem, achieving the generation of deformation twins in titanium alloys and improving the mechanical properties of the alloy.

CN118745535APending Publication Date: 2024-10-08CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411076750.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

There is a lack of effective preparation methods for α-titanium alloy sheets with high deformation twin density in the existing technology. Especially in Ti-Al-B series titanium alloys, the strength and toughness match is poor, and the existing methods are mainly aimed at β-titanium alloys and do not involve Preparation of twins in α titanium alloy.

Method used

By adding a β-stabilizing element Fe element to the micro-alloying design, and using three vacuum consumable melting and direct rolling blanking + high-pass deformation two-fire hot rolling process, a high-density deformation twin plate is prepared to ensure a uniform structure of the alloy. Matching toughness and performance.

Benefits of technology

It achieves the generation of deformation twins in titanium alloys, improves the mechanical properties of the alloy, coordinates strength and toughness, reduces costs, and changes the stacking fault energy through the addition of Fe element, promotes the emergence of twins, and improves the alloy comprehensive mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745535A_ABST
    Figure CN118745535A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of titanium alloys, and discloses a preparation method of a high-deformation twin crystal density alpha titanium alloy plate, which comprises the following steps: adding sponge titanium, aluminum shots, titanium diboride, Ti-32Fe and titanium dioxide as raw materials into a smelting furnace, and carrying out vacuum consumable smelting for three times to obtain a cast ingot; the phase transformation point T beta of the Ti-Al-B series alloy is measured through a differential thermal analysis method, and a cast ingot is subjected to two-heating-number hot rolling to obtain a plate blank; and the plate blank is heated to the temperature of T beta, heat preservation is conducted for the first time, then water cooling is conducted, then the plate blank is heated to the temperature of (T beta-200) DEG C, heat preservation is conducted for the second time, air cooling is conducted to the room temperature, and the plate is obtained. The high-density deformation twin crystal plate is prepared by adding a beta stable element Fe element microalloying design for a Ti-Al-B series alpha titanium alloy through three times of vacuum consumable smelting and adopting a direct rolling cogging and high-pass deformation three-heating-number hot rolling process, and the structure uniformity of the alloy and obdurability matching of the performance are guaranteed with low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium alloys, and in particular to a method for preparing a high-deformation twin density alpha titanium alloy plate. Background Art

[0002] Ti-Al-B series α titanium alloy is an ideal structural material for seawater environment due to its excellent corrosion resistance, moderate strength, good plasticity and toughness, and excellent weldability. It has been widely used in various mechanical parts in the shipbuilding industry. Generally speaking, with the increase of the content of impurity elements such as Fe and O, the strength and hardness of titanium alloys increase, and the plasticity and toughness decrease significantly. The degree of influence of different impurity elements on the strength, plasticity and toughness of Ti-Al-B series α titanium alloys varies greatly. Therefore, the purpose of improving the comprehensive mechanical properties of the alloy can be achieved by reasonably regulating the content of impurity elements in the alloy.

[0003] CN115747690 A discloses a method for preparing a close-packed hexagonal metal material containing ultra-high density twins. The metal material prepared by this method has ultra-dense twins and a more obvious strengthening and toughening effect. However, this invention is only aimed at metal blocks of pure metal, which are small in size and belong to laboratory trial production, and has limitations in practical application fields. CN115537695 A discloses a method for preparing a TB8 titanium alloy with a nano-twin structure. The TB8 titanium alloy is treated with a high-voltage electric pulse to obtain a nano-twin structure, so that its tensile strength and plasticity have good matching, and the metastable β-type TB8 titanium alloy has excellent comprehensive material properties. However, this invention is aimed at the preparation method of β-titanium alloy twins, and does not involve the preparation method of α-titanium alloy twins.

[0004] Therefore, there is a need in the prior art for improving the preparation method of high deformation twin density α titanium alloy sheet. Summary of the invention

[0005] In view of this, the purpose of the embodiment of the present invention is to propose a method for preparing a high deformation twin density α titanium alloy plate. For Ti-Al-B series α titanium alloy, a micro-alloying design of adding β-stabilizing element Fe element is adopted, and a high-density deformation twin plate is prepared through three vacuum consumable smelting and direct rolling blanking + high-pass deformation three-fire hot rolling process, which ensures the uniformity of the alloy's organization and the toughness matching of the performance at a relatively low cost.

[0006] Based on the above purpose, an embodiment of the present invention provides a method for preparing a high deformation twin density α titanium alloy plate, comprising the following steps: S1 smelting: using sponge titanium, aluminum beans, titanium diboride, Ti-32Fe, and titanium dioxide as raw materials and adding them into the smelting furnace, three vacuum consumable smeltings are performed to obtain ingots; S2 hot rolling: The phase transition point T of Ti-Al-B alloy was measured by differential thermal analysis. β , the ingot is hot-rolled twice to obtain a slab; S3 solution aging heat treatment: heat the slab to Tβ temperature, keep it warm for the first time, then water cool it, and then heat the slab to (T β -200)℃ for the second heat preservation and then air-cooled to room temperature to obtain the plate.

[0007] Among them, the first hot rolling is direct rolling, and the heating temperature is T β +100℃, holding time is 100~120min, rolling passes are 2~3 times, deformation of the first pass is ≥50%, deformation of the remaining passes is ≥30%, and the slab is rolled into 40~55mm thick; the heating temperature of the second rolling is T β ±10℃, holding time is 80~100min, rolling passes are 5~6 times, deformation of each pass is ≥18%, total deformation of the second rolling is ≥70%, and the slab is rolled into 5~15mm thick.

[0008] In some embodiments, in S1, the element addition amounts, in mass percentage, include: 3.3%≤[Al]%≤4.8%, 0.2%≤[Fe]%≤0.4%, 0.005%≤[B]%≤0.007%, and the balance is titanium element and unavoidable impurities.

[0009] In some embodiments, the titanium sponge is grade 0A titanium sponge, and the impurity element content is [C]%≤0.01%, [N]%≤0.01%, [O]%≤0.04%, [H]%≤0.001%, and [Fe]%≤0.02%.

[0010] In some embodiments, in Ti-32Fe, the impurity element content is [C]%≤0.2%, [N]%≤0.1%, [O]%≤0.2%, and [Si]%≤0.1%.

[0011] In some embodiments, in S1, the purity of aluminum beans is ≥99.7%, the purity of Ti-32Fe is ≥99.8%, and the purity of titanium dioxide is ≥99.5%.

[0012] In some embodiments, in S2, during the smelting process, the vacuum degree in the vacuum consumable furnace is ≤3.0 Pa, the arc stabilization current is 5-12 A, the smelting voltage in the smelting stage is 20-40 V, and the smelting current is 3-10 kA.

[0013] In some embodiments, in S2, the ingot is subjected to peeling, flattening, and surface polishing processes.

[0014] In some embodiments, in S3, the first insulation time is 100-120 min, and the second insulation time is 80-100 min.

[0015] In some embodiments, in S3, the heating rate of the solution aging heat treatment is 20°C / s.

[0016] In some embodiments, in S3, the target grain size of α grains grown during the aging process is 20-40 μm.

[0017] The present invention has at least the following beneficial technical effects: The present invention aims at the problem of poor matching of strength and toughness of Ti-Al-B series titanium alloy in α titanium alloy, and adopts the design of adding β-stabilizing element Fe and element microalloying to improve the strength and toughness matching of the material; adopts three vacuum consumable melting methods to ensure the uniformity of the composition of titanium alloy ingot; adopts direct rolling and high-pass deformation two-pass hot rolling to obtain a plate with a thickness of 5-15mm, which further promotes the generation of deformation twins. The addition of Fe element changes the stacking fault energy of the alloy, thereby causing growth twins (the appearance of twins is closely related to the stacking fault energy, and growth twins are not common in titanium alloys. Twins appearing in titanium alloys are generally deformation twins, and the appearance of twins can improve the mechanical properties of the alloy), and adopts high-pass deformation hot rolling to further promote the generation of deformation twins. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.

[0019] Figure 1 A flow chart of a method for preparing a high deformation twin density α titanium alloy plate according to an embodiment of the present invention; Figure 2 A schematic diagram of a microstructure embodiment of Example 1 provided by the present invention; Figure 3 A schematic diagram of a microstructure embodiment of Example 2 provided by the present invention; Figure 4 A schematic diagram of a microstructure embodiment of Example 4 provided by the present invention; Figure 5 This is a schematic diagram of the microstructure embodiment of Comparative Example 1 provided by the present invention. DETAILED DESCRIPTION

[0020] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0021] The terms "including" and "having" and any variations thereof in the specification and claims of the present invention and the above-mentioned drawings are intended to cover non-exclusive inclusions; the terms "first", "second", etc. in the specification and claims of the present invention or the above-mentioned drawings are used to distinguish different objects rather than to describe a specific order. "Multiple" means two or more, unless otherwise clearly and specifically defined.

[0022] In addition, reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0023] The present invention is aimed at Ti-Al-B series α titanium alloy, adopts the design of adding β stabilizing element Fe element microalloying, and prepares high-density deformed twin plate through three vacuum consumable smelting and direct rolling blanking + high-pass deformation two-pass hot rolling process, which ensures the uniformity of alloy structure and the toughness matching of performance at a relatively low cost. Figure 1 As shown, the specific method includes the following steps: S1 smelting: using sponge titanium, aluminum beans, titanium diboride, Ti-32Fe, and titanium dioxide as raw materials and adding them into the smelting furnace, three vacuum consumable smeltings are performed to obtain ingots; S2 hot rolling: The phase transition point T of Ti-Al-B alloy was measured by differential thermal analysis. β , the ingot is hot-rolled twice to obtain a slab; S3 solution aging heat treatment: heat the slab to Tβ temperature, keep it warm for the first time, then water cool it, and then heat the slab to (T β -200)℃ for the second heat preservation and then air-cooled to room temperature to obtain the plate.

[0024] Among them, the first hot rolling is direct rolling, and the heating temperature is T β +100℃, holding time is 100~120min, rolling passes are 2~3 times, deformation of the first pass is ≥50%, deformation of the remaining passes is ≥30%, and the slab is rolled into 40~55mm thick; the heating temperature of the second rolling is T β±10℃, holding time is 80~100min, rolling passes are 5~6 times, deformation of each pass is ≥18%, total deformation of the second rolling is ≥70%, and the slab is rolled into 5~15mm thick.

[0025] Furthermore, in S1, 0A-grade titanium sponge, aluminum beans (purity ≥ 99.7%), titanium diboride, Ti-32Fe (purity ≥ 99.8%), and titanium dioxide (≥ 99.5%) are used as raw materials. Aiming at the problem of poor strength-toughness matching of Ti-Al-B series titanium alloy, the method of adding β-stabilizing element Fe is adopted to reduce the stacking fault energy of the alloy, thereby generating growth twins. The twin boundaries hinder the crack propagation, thereby improving the strength and toughness of the alloy and achieving the purpose of coordinating the strength-toughness matching of the alloy. 0A-grade titanium sponge is selected, and the impurity element content [C]%≤0.01%, [N]%≤0.01%, [O]%≤0.04%, [H]%≤0.001%, [Fe]%≤0.02%; Ti-32Fe is selected, and the impurity element content [C]%≤0.2%, [N]%≤0.1%, [O]%≤0.2%, and [Si]%≤0.1%. .

[0026] Furthermore, in S1, the element addition amount is 3.3%≤[Al]%≤4.8%, 0.2%≤[Fe]%≤0.4%, 0.005%≤[B]%≤0.007% by mass percentage, and the remainder is titanium and unavoidable impurities. According to this ratio, the raw materials are subjected to three vacuum consumable smeltings. During the smelting process, the vacuum degree in the vacuum consumable furnace is ≤3.0Pa, the arc stabilization current is 5~12A, the smelting voltage in the smelting stage is 20~40V, and the smelting current is 3~10kA. The ingot of Ф250mm*300mm is obtained, and the skin and flattening are carried out to remove the surface oxides and impurities, and the surface is polished and then hot processed. The vacuum consumable furnace smelting method is adopted. The vacuum consumable smelting has good non-metallic impurity removal ability, which ensures the purity and composition uniformity of the titanium alloy ingot.

[0027] Furthermore, in S2, the phase transition point T of the Ti-Al-B alloy is measured by differential thermal analysis. β The ingot is processed into a square billet of 120~170mm*200mm*300mm, and then rolled into a slab of 5~15mm thickness through two-roll hot rolling test machine. The first hot rolling adopts direct rolling to open the billet, eliminating the forging process, thus saving processing costs; the first hot rolling adopts a large deformation, which can refine the grains and improve the strength of the plate on the one hand, and on the other hand, the high deformation can provide more storage energy, which can promote the generation of deformation twins, thereby improving the strength and toughness matching of the alloy.

[0028] Further, in S3, solution aging: the hot-rolled slab is heated to T βKeep the temperature for 60-90 minutes and then cool with water, and then heat the slab to (T β -200)℃ for 2~4h and then air-cooled to room temperature. In some embodiments, the heat treatment heating rate is 20℃ / s, and the temperature rises with the furnace. The solution aging heat treatment process is adopted to ensure that the β phase is completely retained to room temperature during the solution process. Due to the rapid cooling, the grains have no time to grow, thereby obtaining uniform and fine grains; the aging process allows the β phase after the solution to slowly decompose and precipitate, which plays a role of dispersion strengthening and improves the strength of the alloy. In addition, the primary α grains slowly grow to the target grain size of 20~40µm during the aging process. The grain size is moderate, which can not only improve the strength and plasticity of the grains, but also better prevent the expansion of cracks, thereby increasing the impact toughness of the alloy.

[0029] The present invention is further explained below in conjunction with specific embodiments.

[0030] Example 1 ① Composition design: Fe element microalloying is used to improve the strength and toughness matching of Ti-Al-B titanium alloy. The element addition amount is (mass percentage): [Al]%=4.3%, [Fe]%=0.25%, [B]%=0.005%, and the balance is titanium element and unavoidable impurities.

[0031] ② Vacuum consumable furnace smelting: Use 0A grade titanium sponge, aluminum beans (purity ≥99.7%), titanium diboride, Ti-32Fe (purity ≥99.8%), titanium dioxide (≥99.5%) as raw materials, mix according to the mass percentage in step ①, and carry out three vacuum consumable smeltings. During the smelting process, the vacuum degree in the vacuum consumable furnace is ≤3.0Pa. The three vacuum melting arc stabilization currents are 6A, 9A, and 11A respectively. The melting voltages in the smelting stage are 28V, 32V, and 35V. The three vacuum melting currents are 5kA, 8kA, and 10kA. Obtain an ingot of Ф250*300mm, peel and flatten the head, remove surface oxides and impurities, and perform hot processing after surface polishing.

[0032] ③Hot rolling: The phase transition point T of Ti-Al-B alloy is measured by differential thermal analysis. β=994.8℃, the ingot obtained in step ② is processed into a square billet of 170mm*200mm*300mm. The heating temperature of the first rolling (straight rolling blanking) is 1094.8℃, the holding time is 100min, the rolling passes are 3, the deformation of the first pass is 50%, the deformation of the remaining passes are 30.6% and 32.3% respectively, the total deformation of the first rolling is 76.5%, the final rolling temperature is 820℃, and the rolling is a 40mm thick slab; the heating temperature of the second rolling is 994.8℃, the holding time is 80min, the rolling passes are 6, the deformation of the 6 passes are 18%, 19.2%, 18.1%, 19.35%, 19.4%, 18.4% respectively, the total deformation of the second rolling is 71.25%, the final rolling temperature is 832℃, and the rolling is a 11.5mm thick slab.

[0033] ④Solution aging treatment: Heat the hot-rolled plate to 994.8℃ for 60min and then water-cool. Then heat the plate to 794.8℃ for 4h and then air-cool to room temperature.

[0034] Example 2 ① Composition design: Fe element microalloying is used to improve the strength and toughness matching of Ti-Al-B titanium alloy. The element addition amount is (mass percentage): [Al]%=4.3%, [Fe]%=0.25%, [B]%=0.005%, and the balance is titanium element and unavoidable impurities.

[0035] ② Vacuum consumable furnace smelting: Use 0A grade titanium sponge, aluminum beans (purity ≥99.7%), titanium diboride, Ti-32Fe (purity ≥99.8%), titanium dioxide (≥99.5%) as raw materials, mix according to the mass percentage in step ①, and carry out three vacuum consumable smeltings. During the smelting process, the vacuum degree in the vacuum consumable furnace is ≤3.0Pa. The three vacuum melting arc stabilization currents are 6A, 9A, and 11A respectively. The melting voltages in the smelting stage are 28V, 32V, and 35V. The three vacuum melting currents are 5kA, 8kA, and 10kA. Obtain an ingot of Ф250*300mm, peel and flatten the head, remove surface oxides and impurities, and perform hot processing after surface polishing.

[0036] ③ Hot rolling: The phase transition point Tβ=994.8°C of the Ti-Al-B alloy is measured by differential thermal analysis, and the ingot obtained in step ② is processed into a square billet of 150 mm*200 mm*300 mm. The heating temperature of the first rolling (straight rolling for opening the blank) is 1094.8℃, the holding time is 100min, the rolling passes are 2, the deformation of the first pass is 50%, and the deformation of the remaining passes is 40%. The total deformation of the first rolling is 70%, the final rolling temperature is 803℃, and the rolled plate is 45mm thick; the heating temperature of the second rolling is 994.8℃, the holding time is 80min, the rolling passes are 6, and the deformations of the 6 passes are 20%, 19.4%, 20.7%, 21.7%, 19.4%, and 20.7% respectively. The total deformation of the second rolling is 74.4%, the final rolling temperature is 812℃, and the rolled plate is 11.5mm thick.

[0037] ④Solution aging treatment: Heat the hot-rolled plate to 993.1℃, keep it warm for 60min and then water-cool it. Then heat the plate to 794.8℃, keep it warm for 4h and then air-cool it to room temperature.

[0038] Example 3 ① Composition design: Fe element microalloying is used to improve the strength and toughness matching of Ti-Al-B titanium alloy. The element addition amount is (mass percentage): [Al]%=4.3%, [Fe]%=0.35%, [B]%=0.005%, and the balance is titanium element and unavoidable impurities.

[0039] ② Vacuum consumable furnace smelting: Use 0A grade titanium sponge, aluminum beans (purity ≥99.7%), titanium diboride, Ti-32Fe (purity ≥99.8%), titanium dioxide (≥99.5%) as raw materials, mix according to the mass percentage in step ①, and carry out three vacuum consumable smeltings. During the smelting process, the vacuum degree in the vacuum consumable furnace is ≤3.0Pa. The three vacuum melting arc stabilization currents are 6A, 9A, and 11A respectively. The melting voltages in the smelting stage are 28V, 32V, and 35V. The three vacuum melting currents are 5kA, 8kA, and 10kA. Obtain an ingot of Ф250*300mm, peel and flatten the head, remove surface oxides and impurities, and perform hot processing after surface polishing.

[0040] ③ Hot rolling: The phase transition point Tβ=993.1°C of the Ti-Al-B alloy was measured by differential thermal analysis, and the ingot obtained in step ② was processed into a square billet of 150 mm*200 mm*300 mm. The heating temperature of the first rolling (straight rolling for opening the blank) is 1093.1℃, the holding time is 100min, the rolling passes are 2, the deformation of the first pass is 50%, and the deformation of the remaining passes is 40%. The total deformation of the first rolling is 70%, the final rolling temperature is 803℃, and the rolled plate is 45mm thick; the heating temperature of the second rolling is 993.1℃, the holding time is 80min, the rolling passes are 6, and the deformations of the 6 passes are 20%, 19.4%, 20.7%, 21.7%, 19.4%, and 20.7% respectively. The total deformation of the second rolling is 74.4%, the final rolling temperature is 812℃, and the rolled plate is 11.5mm thick.

[0041] ④Solution aging treatment: Heat the hot-rolled plate to 993.1℃, keep it warm for 60min and then water-cool it. Then heat the plate to 793.1℃, keep it warm for 3h and then air-cool it to room temperature.

[0042] Comparative Example 1 ① Composition design: Fe element microalloying is used to improve the strength and toughness matching of Ti-Al-B titanium alloy. The element addition amount is (mass percentage): [Al]%=4.3%, [Fe]%=0.05%, [B]%=0.005%, and the balance is titanium element and unavoidable impurities.

[0043] ② Vacuum consumable furnace smelting: Use 0A grade titanium sponge, aluminum beans (purity ≥99.7%), titanium diboride, Ti-32Fe (purity ≥99.8%), titanium dioxide (≥99.5%) as raw materials, mix according to the mass percentage in step ①, and carry out three vacuum consumable smeltings. During the smelting process, the vacuum degree in the vacuum consumable furnace is ≤3.0Pa. The three vacuum melting arc stabilization currents are 6A, 9A, and 11A respectively. The melting voltages in the smelting stage are 28V, 32V, and 35V. The three vacuum melting currents are 5kA, 8kA, and 10kA. Obtain an ingot of Ф250*300mm, peel and flatten the head, remove surface oxides and impurities, and perform hot processing after surface polishing.

[0044] ③ Hot rolling: The phase transition point Tβ=998.1°C of the Ti-Al-B alloy is measured by differential thermal analysis, and the ingot obtained in step ② is processed into a square billet of 150 mm*200 mm*300 mm. The heating temperature of the first rolling (straight rolling for opening the blank) is 1098.1℃, the holding time is 100min, the rolling passes are 3, the deformation of the first pass is 30%, and the deformations of the other passes are 30% and 25.2%. The total deformation of the first rolling is 63.2%, the final rolling temperature is 803℃, and the rolled slab is 55mm thick; the heating temperature of the second rolling is 998.1℃, the holding time is 80min, the rolling passes are 7, and the deformations of the 7 passes are 20%, 20%, 19.9%, 19.9%, 19.9%, 19.9%, and 20.7% respectively. The total deformation of the second rolling is 79%, the final rolling temperature is 812℃, and the rolled slab is 11.5mm thick.

[0045] ④Solution aging treatment: Heat the hot-rolled plate to 998.1℃, keep it warm for 60min and then water-cool it. Then heat the plate to 798.1℃, keep it warm for 3h and then air-cool it to room temperature.

[0046] The tensile properties and impact properties of the Ti-Al-B series titanium alloy plates after solution aging in Examples 1 and 2 and the comparative example were tested, and the microstructures were observed and analyzed as shown in Tables 1 and Figure 2-5 As shown. Figure 2-5 It can be seen that the Fe content of the titanium alloy plates prepared according to Examples 1 and 2 of the present invention is equal, and the twin content in Example 1 is higher than that in Example 2, which can be explained that high deformation and one-time rolling can promote the formation of twins; the plate prepared in Example 3 has a higher twin content in the microstructure. Compared with the plate prepared in Example 2, the two plates have the same deformation, but the Fe content in Example 3 is higher. It can be inferred that the higher the Fe content, the more twin content; the comparative example has almost no twins, which is due to the low Fe content of the comparative example plate and the insufficient deformation of one-time rolling. Comparing the mechanical properties of the plates in the examples and comparative examples in the table, it can be seen that the more twin content the plate has, the higher the strength and toughness match of the alloy, and the better the comprehensive mechanical properties.

[0047] Table 1 Test data of tensile properties and impact properties

[0048] The above are exemplary embodiments disclosed in the present invention, but it should be noted that various changes and modifications may be made without departing from the scope disclosed in the embodiments of the present invention as defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.

[0049] It should be understood that, as used herein, the singular forms "a", "an" are intended to include the plural forms as well, unless the context clearly supports an exception. It should also be understood that, as used herein, "and / or" refers to any and all possible combinations including one or more of the associated listed items.

[0050] The serial numbers of the embodiments disclosed in the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.

[0051] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the above embodiments of the present invention, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for preparing a high deformation twin density α titanium alloy sheet, characterized in that: include: S1 smelting: using sponge titanium, aluminum beans, titanium diboride, Ti-32Fe, and titanium dioxide as raw materials and adding them into the smelting furnace, three vacuum consumable smeltings are performed to obtain ingots; S2 hot rolling: The phase transition point T of Ti-Al-B alloy was measured by differential thermal analysis. β , hot rolling the ingot twice to obtain a slab; S3 solution aging heat treatment: The slab is heated to T β The temperature is first kept warm and then water cooled, and then the slab is heated to (T β -200)℃ for the second heat preservation and then air-cooled to room temperature to obtain the plate. Among them, the first hot rolling is direct rolling, and the heating temperature is T β +100℃, holding time is 100~120min, rolling passes are 2~3 times, deformation of the first pass is ≥50%, deformation of the remaining passes is ≥30%, and the slab is rolled into 40~55mm thick; the heating temperature of the second rolling is T β ±10℃, holding time is 80~100min, rolling passes are 5~6 times, deformation of each pass is ≥18%, total deformation of the second rolling is ≥70%, and the slab is rolled into 5~15mm thick.

2. The method for preparing a high deformation twin density α titanium alloy sheet according to claim 1, characterized in that: In S1, the element addition amounts, in mass percentage, include: 3.3%≤[Al]%≤4.8%, 0.2%≤[Fe]%≤0.4%, 0.005%≤[B]%≤0.007%, and the balance is titanium and unavoidable impurities.

3. The method for preparing a high deformation twin density α-titanium alloy sheet according to claim 2, characterized in that: The sponge titanium is 0A grade sponge titanium, and the impurity element content is [C]%≤0.01%, [N]%≤0.01%, [O]%≤0.04%, [H]%≤0.001%, and [Fe]%≤0.02%.

4. The method for preparing a high deformation twin density α titanium alloy sheet according to claim 2, characterized in that: In the Ti-32Fe, the impurity element contents are [C]%≤0.2%, [N]%≤0.1%, [O]%≤0.2%, and [Si]%≤0.1%.

5. The method for preparing a high deformation twin density α-titanium alloy sheet according to claim 1, characterized in that: In S1, the purity of aluminum beans is ≥99.7%, the purity of Ti-32Fe is ≥99.8%, and the purity of titanium dioxide is ≥99.5%.

6. The method for preparing a high deformation twin density α-titanium alloy sheet according to claim 1, characterized in that: In S1, during the smelting process, the vacuum degree in the vacuum consumable furnace is ≤3.0Pa, the arc stabilization current is 5~12A, the smelting voltage is 20~40V, and the smelting current is 3~10kA.

7. The method for preparing a high deformation twin density α titanium alloy sheet according to claim 1, characterized in that: In S2, after two rounds of hot rolling, the ingot is subjected to peeling, flattening and surface polishing treatments.

8. The method for preparing a high deformation twin density α titanium alloy sheet according to claim 1, characterized in that: In S3, the first insulation time is 100~120min, and the second insulation time is 80~100min.

9. The method for preparing a high deformation twin density α titanium alloy sheet according to claim 1, characterized in that: In S3, the heating rate of the solution aging heat treatment is 20°C / s.

10. The method for preparing a high deformation twin density α titanium alloy sheet according to claim 1, characterized in that: In S3, the target grain size of α grains grown during the aging process is 20~40µm.

Citation Information

Cited By

  • High-performance titanium alloy material capable of promoting spheroidization and preparation method of high-performance titanium alloy material

    CN121428325A

  • METHOD FOR PREPARING a-TITANIUM ALLOY SHEET HAVING HIGH DEFORMATION TWIN DENSITY

    EP4759950A1

  • Method for preparing α-titanium alloy sheet having high deformation twin density

    WO2026031765A1