Heat-treatment-free die-casting aluminum alloy and preparation method thereof
By optimizing the proportion of aluminum alloy components and low-temperature baking technology, the problem of insufficient tolerance of existing heat-free pressed aluminum alloys to impurity Fe is solved, achieving both high mechanical performance and environmental protection goals, and reducing production costs and energy consumption.
Patent Information
- Application Number
- CN202410810720.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing heat-treatment-free die-cast aluminum alloys have low tolerance for impurity element iron, which leads to increased production costs and energy consumption and is detrimental to environmental protection goals.
By optimizing the composition ratio of the aluminum alloy and adding elements such as Si, Mn, Cr, Zr, Mo and Sr, a stable α phase and dispersed phase are formed, the tolerance to the impurity Fe is improved, and the mechanical properties are improved through low-temperature baking.
It achieves high yield strength, tensile strength and elongation without heat treatment, reduces thermal stress and thermal deformation, reduces production costs and energy consumption, and promotes the recycling of aluminum alloy materials and the realization of environmental protection goals.
Smart Images

Figure CN118745541A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy materials, and in particular relates to a heat treatment-free die-casting aluminum alloy and a preparation method thereof. Background Art
[0002] Under the background of "dual carbon", the automotive industry is facing the pressure of emission reduction and the demand for sustainable development. Lightweighting has become an inevitable trend to achieve these goals, and the integrated die-casting process is gradually becoming one of the important processes in the automotive industry due to its superior efficiency and cost-effectiveness. The integrated die-casting process combines the stamping, welding, painting and assembly of traditional aluminum parts into one, greatly shortening the manufacturing cycle of castings, reducing manufacturing costs, and effectively reducing the weight of the vehicle body. Therefore, this process provides a low-cost and high-efficiency way to achieve lightweighting of automobiles.
[0003] Although integrated die-casting technology has obvious advantages, it still faces many technical barriers in practical application, mainly concentrated in the following four aspects: first, heat-treatment-free die-casting aluminum alloy materials suitable for integrated die-casting; second, the development and application of large-scale die-casting machines; third, the design and manufacture of die-casting molds; and fourth, the optimization of vacuum die-casting processes. Among them, the most critical technical difficulty lies in the development of special heat-treatment-free aluminum alloy materials suitable for integrated die-casting.
[0004] Traditional die-cast aluminum alloys usually use heat treatment technology (high-temperature solution + artificial aging) to improve the mechanical properties of the alloy, such as yield strength and elongation. However, heat treatment technology has significant limitations when applied to large integrated die-casting structural parts. Specifically, when die-casting structural parts are subjected to solid solution strengthening treatment, the castings need to be heated to a temperature close to the solidus line. However, due to the large size of integrated die-casting parts, the cooling rates of various parts vary significantly, and large thermal stresses are easily formed during the subsequent cooling process. These thermal stresses may not only cause thermal deformation of the castings, but also significantly reduce the size and position accuracy of the castings. In order to correct these deformations, it is usually necessary to introduce multiple shaping processes, which not only increases production costs, but also reduces production efficiency, and the effect is difficult to guarantee.
[0005] Therefore, the development of a new type of aluminum alloy material that can obtain ideal performance without heat treatment after die casting has become the key to realizing the large-scale application of integrated die casting process. The emergence of this heat-treatment-free die-casting aluminum alloy material has made the development and application of large-scale integrated die-casting structural parts possible, providing a new solution for the lightweight development of the automotive industry.
[0006] However, the current heat-treatment-free die-cast aluminum alloy materials still have significant problems in application. They have a low tolerance for the impurity element iron (Fe), requiring the mass percentage of iron to be controlled below 0.16%. This strict requirement requires that the raw materials used for production must be high-purity electrolytic aluminum, which increases production energy consumption and costs, and is not conducive to the recycling of aluminum alloy materials and the realization of environmental protection goals.
[0007] Therefore, it is necessary to provide a new technical solution to the above technical problems. Summary of the invention
[0008] The object of the present invention is to provide a heat-treated die-cast aluminum alloy and a preparation method thereof, which has a high tolerance to impurity Fe and excellent mechanical properties.
[0009] To achieve the above purpose, the technical solution provided by the present invention is as follows:
[0010] In a first aspect, the present invention provides a heat treatment-free die-casting aluminum alloy, comprising the following components:
[0011] Si: 7-11wt%; Mn: 0.3-0.8wt%; Mg: 0.1-0.8wt%; Cr: 0.04-0.2wt%; Zr: 0-0.3wt%; Mo: 0.06-0.2wt%; Sr: 0.01-0.04wt%; Fe: <0.8wt%; the total amount of unavoidable impurities is <0.2wt%, and the content of any single impurity element is <0.1wt%; and the balance is Al.
[0012] In one or more embodiments, at least two elements of Cr, Mo, and Zr in the aluminum alloy form a dispersed phase dispersed in the aluminum matrix.
[0013] In one or more embodiments, a bulk α-Al(Cr,Fe)Si phase is formed in the aluminum alloy.
[0014] In one or more embodiments, a rod-shaped D023-type (Al, Si) 3 Zr phase is formed in the aluminum alloy.
[0015] In one or more embodiments, the aluminum alloy is formed with an α-Al(Mo,Fe)Si phase dispersed in an aluminum matrix.
[0016] In one or more embodiments, the Cr in the aluminum alloy can change the solidification sequence of the aluminum alloy to form an α-Al(FeMnCr)Si phase dispersed in the aluminum matrix.
[0017] In a second aspect, the present invention provides a method for preparing the aforementioned heat treatment-free die-casting aluminum alloy, comprising:
[0018] The ingredients are prepared according to the composition ratio of the aluminum alloy; the prepared raw materials are added into a smelting furnace, heated and melted, and stirred evenly to obtain an alloy melt; a protective gas is applied to the alloy melt, and a refining agent is added to perform refining and impurity removal; Sr-containing raw materials are added to the refined alloy melt to perform a modification treatment; a refining agent is added to the alloy melt after the modification treatment to perform refining, degassing and impurity removal; the treated alloy melt is die-casted to obtain an aluminum alloy casting.
[0019] In one or more embodiments, the prepared raw materials are added into a smelting furnace, heated and melted, and stirred evenly to obtain an alloy melt, which specifically includes:
[0020] Add aluminum ingots and Si-containing raw materials into a smelting furnace and heat and melt them. After the aluminum ingots and Si-containing raw materials are melted, adjust the melt temperature to 720-780°C; add Cr-containing raw materials, Mn-containing raw materials, Zr-containing raw materials, and Mo-containing raw materials into the melt, and lower the temperature to 700-760°C after they are completely melted; add Mg-containing raw materials into the melt, immerse the Mg-containing raw materials below the liquid surface and melt them, stir them evenly, and obtain an alloy melt.
[0021] In one or more embodiments, the refining, degassing and impurity removal method specifically includes: degassing with a rotor and adding a refining agent, the degassing time is 5-40min, the degassing pressure is 0.1-0.5MPa, the degassing speed is 300-500r / min, the degassing temperature is 710-750°C, a refiner is added within 1-5 minutes before the end of the degassing process, and slag and impurities are removed after degassing.
[0022] In one or more embodiments, the method further comprises: baking and keeping the aluminum alloy casting obtained by die casting at a temperature range of 150-240° C. for 30-90 minutes.
[0023] Compared with the prior art, the heat treatment-free die-casting aluminum alloy and the preparation method thereof provided by the present invention have the following advantages:
[0024] (1) Mn, Cr, Mo and Fe form a stable α phase, preventing the formation of harmful phases, which can greatly improve the tolerance to impurity Fe;
[0025] (2) The yield strength of the alloy in the cast state reaches 130-160MPa, the tensile strength reaches 260-290MPa, and the elongation reaches 7-15%;
[0026] (3) After low temperature baking (150-240℃ / 30-90min), the yield strength increases by 20-30% (30-40MPa);
[0027] (4) Under the test conditions of stress ratio R=-1, loading frequency 40Hz, and 10 million cycles, the fatigue strength of the alloy in the cast state reaches 110MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 The microstructure diagram of the aluminum alloy prepared in Example 1 of the present invention;
[0030] Figure 2 The microstructure diagram of the aluminum alloy prepared in Example 1 of the present invention;
[0031] Figure 3 This is a microstructure diagram of the aluminum alloy obtained in Example 2 of the present invention;
[0032] Figure 4 This is a microstructure diagram of the aluminum alloy obtained in Example 2 of the present invention;
[0033] Figure 5 This is a microstructure diagram of the aluminum alloy obtained in Example 3 of the present invention;
[0034] Figure 6 This is a microstructure diagram of the aluminum alloy obtained in Example 3 of the present invention;
[0035] Figure 7 This is a stress-strain curve diagram of the tensile test of the aluminum alloy prepared in Example 2 of the present invention;
[0036] Figure 8 This is a graph showing the VDA test results of the aluminum alloys prepared in Examples 1 to 3 of the present invention. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0038] It should be noted that in the following description, the "%" indicating the amount is a weight basis unless otherwise specified. Unless otherwise specified, all numbers used in this specification and claims to indicate quantities and physical properties should be understood to be modified by the term "about" in all cases. Therefore, unless otherwise specified, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.2, 1.4, 1.55, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0039] Under the background of "dual carbon", lightweight development in the automotive industry has become an inevitable trend. The manufacturing process of traditional aluminum parts involves multiple links such as stamping, welding, painting and assembly, which not only increases the manufacturing cycle and cost, but also limits the further reduction of the body weight. To solve these problems, the integrated die-casting process came into being. It combines the above-mentioned multiple links, greatly shortens the manufacturing cycle, reduces costs, and significantly reduces the weight of the body. However, this technology faces multiple technical barriers, the most important of which is the development of special heat-treatment-free aluminum alloy materials suitable for integrated die-casting.
[0040] In the prior art, traditional die-cast aluminum alloys usually rely on heat treatment technology (high temperature solution + artificial aging) to improve the yield strength and elongation of the alloy. However, for larger die-cast structural parts, large thermal stress and thermal deformation are easily generated during the heat treatment process, resulting in a decrease in the position and dimensional accuracy of the castings, and the need to introduce multiple shaping processes, which further increases costs and reduces efficiency. In addition, the existing heat-treatment-free die-cast aluminum alloys have a low tolerance for impurities Fe, requiring the Fe mass percentage to be ≤0.16%, which requires that the raw materials used in production must be high-purity electrolytic aluminum, which is not conducive to reducing energy consumption and recycling of aluminum alloy materials, and also leads to high costs for corresponding products.
[0041] In view of the problems in the above-mentioned prior art, the present invention proposes a heat-treatment-free die-casting aluminum alloy. By scientifically optimizing the proportion of alloy components, especially adding elements such as Si, Mn, Mg, Cr, Zr, Mo and Sr in specific proportions, and controlling the content of Fe and other impurities, the aluminum alloy of the present invention can obtain ideal mechanical properties without heat treatment. Specifically, Si improves the strength and casting performance of the alloy, Mn, Cr, Mo and Fe form a stable α phase to prevent the formation of harmful phases, Mg improves strength and ductility through solid solution strengthening and precipitation hardening, Zr refines the grains, Mo prevents the formation of coarse intermetallic compounds, and Sr refines the eutectic silicon phase to improve the overall performance of the alloy.
[0042] Through this composition optimization design, the aluminum alloy of the present invention can obtain high strength and high ductility without high-temperature solid solution and artificial aging treatment after casting, while reducing thermal stress and thermal deformation problems, ensuring the dimensional accuracy of castings, reducing production costs and energy consumption, and achieving the goal of lightweighting. This heat-treatment-free die-casting aluminum alloy not only improves the manufacturing efficiency and performance consistency of castings, but also promotes the recycling of aluminum alloy materials, meets the requirements of environmental protection and sustainable development, and provides an efficient and low-cost solution for lightweighting in the automotive industry.
[0043] The heat-treatment-free die-casting aluminum alloy in one embodiment of the present invention comprises the following components: Si: 7-11wt%; Mn: 0.3-0.8wt%; Mg: 0.1-0.8wt%; Cr: 0.04-0.2wt%; Zr: 0-0.3wt%; Mo: 0.06-0.2wt%; Sr: 0.01-0.04wt%; Fe: <0.8wt%; the total amount of inevitable impurities <0.2wt%, and the content of any single impurity element <0.1wt%; and the balance Al. Among them, the inevitable impurities refer to other impurity elements except Fe.
[0044] It should be noted that the present invention can realize the formation of dispersed phase and the regulation of Fe phase by adding a combination of Cr, Mo and Zr elements, thereby achieving a dual improvement in alloy strength and plasticity, while also allowing the aluminum alloy to accommodate more impurity element Fe.
[0045] According to the theories of Lifshitz, Slyozov and Wagner, the ideal dispersion phase should have low interface energy (low lattice-matrix mismatch), low diffusion rate and solubility limit to prevent the body from coarsening due to diffusion at high temperature. Since the transition elements Cr, Mo and Zr have low diffusion rates in the α-Al matrix (for example, Cr, Mo and Zr at 400°C are 1.29×10 - 21 m 2 s -1 5.52×10 -23 m 2 s -1 , 1.20×10 -20 m 2 s -1 ), which is better than the commonly used dispersed phase initiator Mn (6.24×10 -19 m 2 s -1 ). Therefore, the dispersed phase containing Cr, Mo, and Zr has better anti-coarsening performance.
[0046] Adding Cr to Al-Si alloy can inhibit the tendency of sticking more effectively than Mn, and transform the needle-shaped β-Al5FeSi into a blocky α-Al(Cr,Fe)Si phase. In addition, during the heat treatment process, the supersaturated Cr solute atoms in the aluminum matrix will precipitate in the form of a dispersed phase. Zr can form a balanced rod-shaped D023 type (Al,Si)3Zr precipitate phase. Mo is a more effective Fe neutralizer than Mn, which can inhibit the transformation of β-Al5FeSi and π phases, forming a fine dispersed α-Al(Mo,Fe)Si phase, which is evenly distributed in the aluminum matrix, effectively hindering dislocation movement and improving the strength of the alloy.
[0047] In the alloy system of the present invention, Mg, Zr, and Mo can effectively improve the strength of the alloy, Mn, Mo, and Cr can effectively regulate the morphology of intermetallic compounds, and the ratio of Mn, Mo, and Cr can effectively regulate the proportion of intermetallic compounds with different morphologies. By adding Cr, the solidification sequence of a single Mo-containing component is changed, the area percentage of the α-Al(FeMnCr)Si phase is increased, and part of the Fe content in the alloy is consumed, thereby avoiding the problem of coarsening of intermetallic compound particles that is easily caused by the single addition of the Mo element, reducing the organizational differences of the alloy under different process conditions, and improving the uniformity of the casting organization and performance. On the other hand, the Cr content can effectively avoid the generation of π phase and β-Fe phase, and the needle-shaped β-Al(Fe,Cr)Si phase can also be avoided by optimizing the composition window, and only a fine α-Al(FeMnCr)Si phase is formed.
[0048] Solidification sequence refers to the order of transformation from liquid phase to solid phase of a metal or alloy during cooling. The addition of different elements will change the solidification sequence of the alloy, thereby affecting the final microstructure and phase composition. The addition of Cr (chromium) and Mo (molybdenum) elements has different effects on the solidification sequence. Mo tends to form larger intermetallic compound particles in aluminum alloys, such as β phase (β-Al5FeSi) and π phase (Al8FeMg3Si6). These large particles will gradually grow during cooling, resulting in a decrease in the strength and ductility of the material. The addition of Cr will form new intermetallic compounds, such as α-Al(FeMnCr)Si phase, so that Cr, Fe, Mn and Si form a new stable phase, thereby avoiding the large particles of intermetallic compounds produced when Mo exists alone.
[0049] α-Al(FeMnCr)Si phase is a stable intermetallic compound with a small and uniform morphology. It can be effectively dispersed in the aluminum matrix, thereby improving the strength and hardness of the alloy. By adding Cr, the formation of the α phase can be promoted and its area percentage in the alloy can be increased. The presence of this phase helps to refine the microstructure of the alloy, hinder dislocation movement, and improve the mechanical properties of the material. The addition of Cr allows a portion of Fe to form a stable α phase with Cr and other elements, thereby reducing the chance of Fe forming unfavorable β phase and π phase (β-Fe phase and π phase are usually needle-shaped, and the presence of these phases will have an adverse effect on the ductility and toughness of the material).
[0050] The present invention can eliminate the large-sized Mo-containing phase inside the alloy and reduce the alloy process sensitivity on the basis of obtaining sufficient strength (adding Mg, Zr and Mo); the addition of Cr can effectively avoid the generation of π phase and β-Fe phase, and the needle-shaped β-Al(Fe,Cr)Si phase can also be avoided by optimizing the composition window, and only a fine α-Al(FeMnCr)Si phase is formed; and by introducing the Cr element, the π phase in the alloy is greatly reduced, and while achieving Mg strengthening, the damage of the Mg element to ductility is reduced.
[0051] Chromium (Cr) has multiple functions in aluminum alloys, mainly including grain refinement, corrosion resistance enhancement and mechanical properties improvement. In aluminum alloys, Cr can form α-Al (FeMnCr) Si phase with elements such as Fe and Mn. This phase has a stable crystal structure and can effectively inhibit the formation of β phase (brittle phase). In addition, the addition of Cr can also improve the high temperature stability and creep resistance of the alloy.
[0052] In order to obtain fine and uniformly distributed α-Al(FeMnCr)Si phase during the casting process and avoid the formation of β-Al(Fe,Cr)Si phase, the present invention selects to control the Cr content within 0.04-0.2wt%. The Cr content within this range can ensure that the alloy forms the required α phase during the casting process, but does not induce excessive intermetallic compounds, thereby ensuring the toughness and ductility of the alloy.
[0053] Too low Cr content (less than 0.04wt%) will lead to insufficient formation of α-Al(FeMnCr)Si phase, which will increase the formation of β phase. The presence of β phase will significantly reduce the mechanical properties of the alloy, especially ductility and toughness. In addition, the lack of sufficient Cr will also reduce the high temperature stability and creep resistance of the alloy.
[0054] Too high Cr content (above 0.2wt%) will lead to excessive formation of intermetallic compounds. These compounds will form coarse grains and secondary phases during the casting process, resulting in a significant decrease in the toughness and ductility of the alloy. At the same time, too high Cr content will also increase the hardness of the alloy, making the processing and forming process more difficult.
[0055] Zirconium (Zr) plays a major role in aluminum alloys in refining grains and improving heat resistance. Zr can form fine (Al,Si)3Zr phases with Al. These precipitated phases can effectively hinder the movement of grain boundaries during the solid solution process, thereby refining grains and improving the mechanical properties and high-temperature properties of the alloy. In addition, the (Al,Si)3Zr phase also has a high melting point and stability, and can maintain a stable crystal structure at high temperatures to prevent grain coarsening.
[0056] The present invention chooses to control the Zr content within the range of 0-0.3wt%, with the purpose of achieving grain refinement and high-temperature performance improvement by adding Zr in an appropriate amount, while avoiding the negative effects of excessive addition. Too high Zr content (higher than 0.3wt%) will lead to the formation of a large amount of (Al,Si)3Zr phases, which may form coarse particles in an oversaturated state, weakening the ductility and toughness of the alloy. In addition, excessive Zr will increase the hardness of the alloy, making the processing and forming process more difficult.
[0057] Molybdenum (Mo) is mainly used in aluminum alloys to prevent the coarsening of intermetallic compounds and improve the high temperature resistance and strength of the alloy. Mo can form stable intermetallic compounds with other elements such as Fe, Mn, Cr, etc. These compounds have high stability at high temperatures and can effectively prevent the growth of grains. In addition, Mo also has a good solid solution strengthening effect and can improve the comprehensive mechanical properties of the alloy.
[0058] The present invention selects to control the Mo content within the range of 0.06-0.2wt%, with the purpose of achieving refinement and stabilization of intermetallic compounds by adding a proper amount of Mo, improving the high temperature performance and strength of the alloy, while avoiding the negative effects caused by excessive addition.
[0059] Too low Mo content (less than 0.06wt%) will lead to insufficient formation of intermetallic compounds and fail to effectively prevent grain coarsening, especially in high temperature environments, and the mechanical properties and dimensional stability of the alloy will be significantly reduced. In addition, the lack of sufficient Mo will also reduce the solid solution strengthening effect of the alloy, resulting in insufficient strength and hardness of the alloy.
[0060] Too high Mo content (above 0.2wt%) will lead to the formation of excessive intermetallic compounds, which may form coarse particles in the supersaturated state, weakening the toughness and ductility of the alloy. In addition, excessive Mo will significantly increase the hardness of the alloy, making the processing and forming process more difficult and may cause processing stress and cracking problems.
[0061] In a preferred embodiment of the present invention, the heat-treatment-free die-casting aluminum alloy comprises the following components: Si: 8-9wt%; Mn: 0.4-0.7wt%; Mg: 0.1-0.6wt%; Cr: 0.05-0.1wt%; Zr: 0.04-0.2wt%; Mo: 0.06-0.15wt%; Sr: 0.01-0.03wt%; Fe: <0.8wt%; the total amount of unavoidable impurities is <0.2wt%, and the content of any single impurity element is <0.1wt%; and the balance is Al.
[0062] In a more preferred embodiment of the present invention, the heat-treatment-free die-casting aluminum alloy comprises the following components: Si: 9-10wt%; Mn: 0.4-0.6wt%; Mg: 0.1-0.3wt%; Cr: 0.06-0.08wt%; Zr: 0.06-0.1wt%; Mo: 0.06-0.1wt%; Sr: 0.01-0.03wt%; Fe: <0.8wt%; the total amount of unavoidable impurities is <0.2wt%, and the content of any single impurity element is <0.1wt%; and the balance is Al.
[0063] In one embodiment of the present invention, a method for preparing the aforementioned heat-treatment-free die-casting aluminum alloy is provided, and the method specifically comprises the following steps:
[0064] S101: Mixing materials according to the composition ratio of aluminum alloy.
[0065] The raw materials may include pure Al ingots (electrolytic aluminum ingots or recycled aluminum ingots), Al-Si master alloys, either industrial pure silicon or soluble silicon, pure Mg ingots, Al-Cr master alloys, Al-Mn master alloys or manganese agents, Al-Zr master alloys, Al-Mo master alloys, Al-Sr master alloys, etc.
[0066] S102: adding the prepared raw materials into a smelting furnace, heating and melting, and stirring evenly to obtain an alloy melt.
[0067] Specifically, an aluminum ingot and a Si-containing raw material are added to a smelting furnace and heated to melt. After the aluminum ingot and the Si-containing raw material are melted, the melt temperature is adjusted to 720-780°C; a Cr-containing raw material, a Mn-containing raw material, a Zr-containing raw material, and a Mo-containing raw material are added to the melt, and after they are completely melted, the temperature is lowered to 700-760°C; then, a Mg-containing raw material is added to the melt, the Mg-containing raw material is immersed below the liquid surface and melted, and stirred evenly to obtain an alloy melt.
[0068] S103: applying protective gas to the alloy melt, adding refining agent, and performing refining and impurity removal.
[0069] Specifically, the refining agent is weighed according to 1-1.5‰ of the mass of the alloy melt, and 99.99% nitrogen / argon is used for blowing refining; the refining pressure is 0.05-0.2MPa, and the refining speed is 0.5-2kg / min; after the refining is completed, the slag is removed after standing for 5-20 minutes, and the temperature of the alloy melt is set to 720-750℃ after slag removal, and the melt temperature is stirred to make the melt temperature uniform, and then the material is left to stand and discharged into the transfer bag.
[0070] S104: adding Sr-containing raw materials to the refined alloy melt for modification.
[0071] Specifically, the transfer package is preheated to 720-750° C. and weighed, and then weighed again after the material is discharged, and Al-Sr master alloy is added according to the quality of the melt for modification.
[0072] S105: adding a refining agent to the alloy melt after the modification treatment to perform refining, degassing and impurity removal.
[0073] Specifically, use a rotor to degas and add 1-3‰ of the melt mass refining agent, the degassing time is 5-40min, the degassing pressure is 0.1-0.5MPa, the degassing speed is 300-500r / min, the degassing temperature is 710-750℃, and the refiner (Al5TiB or TCB) is added within 1-10 minutes before the end of the degassing process. After degassing, the slag is removed and impurities are removed.
[0074] It should be noted that after refining, degassing and impurity removal, the aluminum liquid in the transfer bag is poured into the machine-side furnace, and a filter is added before adding the material to the machine-side furnace; mushroom samples and K-mold samples are taken, and samples are taken for hydrogen measurement. If the composition is unqualified, it is adjusted according to the alloy composition to be qualified. If the K-mold sample is unqualified, the slag removal process is repeated. If the hydrogen content is unqualified, the rotor degassing process is repeated until the quality of the alloy melt is qualified.
[0075] S106: Die-casting the processed alloy melt to obtain an aluminum alloy casting.
[0076] Specifically, the die casting conditions include: temperature 680℃-720℃; mold vacuum controlled below 80mbar; mold temperature 170-250℃; casting pressure 40-150MPa; injection speed 0.1-0.5m / s in low speed section and 3-5m / s in high speed section. The amount of soup is adjusted according to the thickness of the material handle being 20%-30% of the barrel diameter, and the mold holding time is 1-20s.
[0077] It should be noted that, according to the actual performance requirements of the aluminum alloy casting application and the assembly process arrangement, the aluminum alloy casting can be baked and kept warm at a temperature in the range of 180℃-230℃ for 30-90min to further improve the yield strength (increase by 30-40MPa).
[0078] The present invention will be further described below in conjunction with specific embodiments.
[0079] Preparation of aluminum alloy
[0080] (1) Batching: According to the total amount of 300 kg, pure Al ingot, AlSi20 master alloy, 95% quick-dissolving silicon, pure Mg ingot, AlMn10 master alloy, AlCr10 master alloy, AlMo5 master alloy, AlZr10 master alloy, AlSr10 master alloy, AlV10 master alloy, and grain refiner TCB master alloy are weighed and set aside in sequence according to the calculated values in the batching table;
[0081] (2) Melting: first add pure Al ingot and AlSi20 master alloy into a 300 kg crucible furnace and heat up with the furnace; after they are completely melted, raise the melt temperature to 765°C, and press 95% of quick-dissolving silicon into batches using a bell jar; after the quick-dissolving silicon is completely melted, add AlCr10 master alloy, AlMn10 master alloy, AlMo5 master alloy, AlZr10 master alloy, and AlV10 master alloy according to the actual alloy ingredients, and stir evenly with a preheated spoon; after the master alloy is completely melted, cool to 720°C, press Mg ingot into the melt below the liquid surface using a bell jar, and stir evenly after the Mg ingot is completely melted;
[0082] (4) Refining and degassing: Lower the melt temperature to 710°C, add the weighed AlSr10 intermediate alloy, stir to melt it all, and keep warm for 5 minutes. Then raise the melt temperature to 720°C-730°C to start degassing. Weigh the refining agent according to 0.1%-0.15% of the melt mass, and add it to the refining agent automatic adding funnel of the rotor degasser. Use a rotor degasser for degassing, the refining agent addition speed is 500r / min, the degassing speed is 400r / min, the high-purity Ar flow rate of the degasser is 25L / min, and the degassing time is 25min. After the degassing is completed, let it stand for 10 minutes, take the alloy composition sample and the reduced pressure solidification gas measurement sample;
[0083] (5) Die casting: After the degassing meets the standard and the composition is qualified, the melt temperature is adjusted to 690℃-705℃, and die casting is carried out on a 400-ton die casting machine. The die casting parameters are: mold temperature 170℃, mold filling degree 33%, vacuum degree 60mBar, low speed section injection speed 0.2m / s, high speed section 3.9m / s, casting pressure 80MPa, and mold holding time 6s.
[0084] (6) Low temperature aging: Set the temperature of the holding furnace to 200°C, keep it warm for 1 hour to stabilize the furnace temperature, put the die casting in, and keep it warm for 60 minutes after the temperature rises to 200°C.
[0085] The ingredients of each embodiment and comparative example were prepared according to the aluminum alloy composition ratio shown in Table 1, and then the aluminum alloy of each embodiment and comparative example was prepared according to the aforementioned aluminum alloy preparation method.
[0086] Table 1- Al-Si alloy composition
[0087]
[0088]
[0089] The mechanical properties of the aluminum alloys obtained in the embodiments and comparative examples in the as-cast state and after low-temperature aging were tested, and the specific test results are shown in Table 2.
[0090] Table 2 - Performance test results of aluminum alloy in cast state and after low temperature aging
[0091]
[0092] It can be seen from Table 2 that the aluminum alloy prepared in the embodiment of the present invention can significantly improve the mechanical properties of the aluminum alloy by adding Cr.
[0093] Figure 1 and Figure 2 The aluminum alloy microstructure diagram obtained in Example 1 is shown in FIG. Figure 3 and Figure 4 This is the microstructure diagram of the aluminum alloy obtained in Example 2. Figure 5 and Figure 6 The aluminum alloy microstructure diagram obtained in Example 3. Figures 1 to 6 It can be seen that, except for the inevitable pre-crystallization in the barrel due to the high-pressure casting process itself, the alloy of the present invention has a fine structure, and the dendrite size of most α-Al is below 20 μm; the eutectic silicon modification effect is good, and most of them are fine network structures; there is almost no needle-like Fe phase, and the Fe phase is basically transformed into fine granular α-Fe phase, rather than needle-like β-Fe phase.
[0094] Figure 7is a tensile test stress-strain curve of the aluminum alloy obtained in Example 2 of the present invention, Figure 7 It can be seen that the tensile properties of the aluminum alloy obtained in Example 1 are as follows: 0.2 >140MPa, tensile strength δ b >285MPa, A%>13.
[0095] Figure 8 The VDA test results of the aluminum alloys obtained in Examples 1 to 3 of the present invention are shown in FIG. Figure 8 It can be seen that the bending angles of the aluminum alloys prepared in Examples 1 to 3 all reach above 20°.
[0096] In summary, the heat treatment-free die-casting aluminum alloy and the preparation method thereof provided by the present invention have the following advantages:
[0097] (1) Mn, Cr, Mo and Fe form a stable α phase, preventing the formation of harmful phases, which can greatly improve the tolerance to impurity Fe;
[0098] (2) The yield strength of the alloy in the cast state reaches 130-160MPa, the tensile strength reaches 260-290MPa, and the elongation reaches 7-15%;
[0099] (3) After low temperature baking (180-230℃ / 30-90min), the yield strength increases by 20-30% (30-40MPa);
[0100] (4) Under the test conditions of stress ratio R=-1, loading frequency 40Hz, and 10 million cycles, the fatigue strength of the alloy in the cast state reaches 110MPa.
[0101] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and range of equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0102] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A heat treatment-free die-casting aluminum alloy, characterized in that: Includes the following ingredients: Si: 7-11wt%; Mn: 0.3-0.8wt%; Mg: 0.1-0.8wt%; Cr: 0.04-0.2wt%; Zr: 0-0.3wt%; Mo: 0.06-0.2wt%; Sr: 0.01-0.04wt%; Fe: <0.8wt%; the total amount of inevitable impurities <0.2wt%, and the content of any single impurity element <0.1wt%; and the balance Al.
2. The heat treatment-free die-casting aluminum alloy according to claim 1, characterized in that: At least two elements among Cr, Mo and Zr in the aluminum alloy form a dispersed phase dispersed in the aluminum matrix.
3. The heat treatment-free die-casting aluminum alloy according to claim 1, characterized in that: A bulk α-Al(Cr,Fe)Si phase is formed in the aluminum alloy.
4. The heat treatment-free die-casting aluminum alloy according to claim 1, characterized in that: A rod-shaped D023 type (Al, Si) 3 Zr phase is formed in the aluminum alloy.
5. The heat treatment-free die-casting aluminum alloy according to claim 1, characterized in that: The aluminum alloy has an α-Al(Mo,Fe)Si phase dispersed in an aluminum matrix.
6. The heat treatment-free die-casting aluminum alloy according to claim 1, characterized in that: The Cr in the aluminum alloy can change the solidification sequence of the aluminum alloy to form an α-Al(FeMnCr)Si phase dispersed in the aluminum matrix.
7. A method for preparing a heat treatment-free die-casting aluminum alloy as claimed in any one of claims 1 to 6, characterized in that: include: The ingredients are prepared according to the composition ratio of the aluminum alloy; Add the prepared raw materials into a smelting furnace, heat and melt, and stir evenly to obtain an alloy melt; Applying protective gas to the alloy melt, adding refining agent, and refining and removing impurities; Adding Sr-containing raw materials to the refined alloy melt for modification; Adding a refining agent to the alloy melt after modification to perform refining, degassing and impurity removal; The treated alloy melt is die-casted to obtain an aluminum alloy casting.
8. The method for preparing heat treatment-free die-casting aluminum alloy according to claim 7, characterized in that: Add the prepared raw materials into a smelting furnace, heat and melt, and stir evenly to obtain an alloy melt, which specifically includes: Add the aluminum ingot and the Si-containing raw material into the smelting furnace and heat and melt them. After the aluminum ingot and the Si-containing raw material are melted, adjust the melt temperature to 720-780°C; Adding Cr-containing raw materials, Mn-containing raw materials, Zr-containing raw materials, and Mo-containing raw materials into the melt, and lowering the temperature to 700-760° C. after they are completely melted; Add Mg-containing raw materials into the melt, immerse the Mg-containing raw materials below the liquid surface and melt, stir evenly, and obtain an alloy melt.
9. The method for preparing heat treatment-free die-casting aluminum alloy according to claim 7, characterized in that: The specific methods of refining, degassing and impurity removal include: Use a rotor to degas and add refining agent. The degassing time is 5-40min, the degassing pressure is 0.1-0.5MPa, the degassing speed is 300-500r / min, the degassing temperature is 710-750℃, and the refiner is added within 1-5 minutes before the end of the degassing process. After degassing, the slag is removed and impurities are removed.
10. The method for preparing heat treatment-free die-casting aluminum alloy according to claim 7, characterized in that: The method further comprises: The aluminum alloy casting obtained by die casting is baked and kept warm at a temperature range of 150-240°C for 30-90 minutes.
Citation Information
Patent Citations
Heat-treatment-free die-casting aluminum alloy and preparation method thereof
CN115198149A
Aluminum alloy ingot produced by secondary aluminum and used for integrated die casting and production method of aluminum alloy ingot
CN117026020A
High-toughness heat-treatment-free die-casting aluminum alloy and preparation method thereof
CN117144206A
Low-cost heat-treatment-free high-toughness die-casting aluminum alloy and preparation method thereof
CN117987697A
Cited By
High-bending-performance heat-treatment-free die-casting aluminum alloy and preparation method thereof
CN121023320A
High-bending-performance heat-treatment-free die-casting aluminum alloy and preparation method thereof
CN121023320B
Heat-treatment-free die-casting aluminum alloy, and preparation method therefor and use thereof
WO2025260793A1