Method for reducing inclusion level of Q345 steel billet finished steel plate
Through the smelting, VD vacuum treatment and LF refining steps, combined with the use of lime, refining slag, silicon manganese, aluminum granules and carbonized rice husk, the problem of high inclusion levels in Q345 billet finished steel plates was solved, significantly reducing Class B inclusions content, improving product quality and production efficiency.
Patent Information
- Application Number
- CN202410759824.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-08
AI Technical Summary
The level of inclusions in the Q345 billet finished steel plate is relatively high, which affects product quality. In the existing technology, the excessive temperature of the molten steel during the steelmaking process leads to serious secondary oxidation, which increases the number of inclusions.
Adopt the steps of smelting → VD vacuum treatment → LF refining → continuous casting, control the temperature of the molten steel by adding lime, refining slag, silicon manganese and aluminum particles, vacuum treatment and soft blowing of argon gas to raise the temperature, and add carbonized rice during the LF refining process The shell is insulated, and the Al content and vacuum degree are adjusted to reduce inclusions.
It effectively reduces the content of Class B inclusions in steel, shortens the production cycle, and reduces production costs. The proportion of Class B inclusions in steel plates below grade C1.5 reaches 99%, and the proportion below grade C0.5 reaches 94%. %above.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, in particular to a method for reducing the inclusion level of a Q345 steel billet finished steel plate. Background Art
[0002] Carbon structural steel Q345 is a low alloy steel (C≤0.20) with good comprehensive mechanical properties, acceptable low temperature performance, good cold stamping performance, plasticity, welding performance and machinability. It is widely used in bridges, vehicles, ships, buildings, pressure vessels, special equipment, etc. Q represents the yield strength of this material, and the following 345 refers to the yield value of this material, which is about 345 MPa; and the yield value will decrease with the increase of the thickness of the material.
[0003] The conventional steelmaking production process of Q345 steel is converter (electric furnace) → LF → VD → continuous casting. In order to ensure smooth continuous casting, the temperature of the molten steel reaches 1650℃ at the end of LF, and it takes a long time to supply electricity for heating. Excessive temperature leads to serious secondary oxidation of the molten steel and a large number of inclusions in the steel. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for reducing the inclusion level of Q345 steel billet and finished steel plate to improve product quality.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: comprising smelting, VD vacuum treatment, LF refining and continuous casting steps performed in sequence;
[0006] The smelting step comprises: adding lime, refined slag, silicon manganese and aluminum particles along with the steel flow during the steel tapping process, and the temperature of the steel liquid at the tapping temperature is ≥1580°C;
[0007] The VD vacuum treatment step: determine whether to add aluminum wire before VD according to the Al content of the converter steel, and control the Al content to reach 0.050% at the beginning of VD; during the vacuum treatment, the vacuum degree is 66Pa or less and is maintained for ≥15min;
[0008] The LF refining steps include: soft blowing of argon gas, supplying electricity to increase the temperature of the molten steel to the liquidus line of the steel grade + (50-60)°C, stopping the supply of electricity and shutting off the argon gas, and adding carbonized rice husks to the surface of the molten steel for heat preservation.
[0009] Furthermore, in the smelting step, 800-1200 kg of lime, 200-500 kg of refined slag and 100-200 kg of aluminum particles are added with the steel flow.
[0010] Furthermore, in the LF refining step, the amount of carbonized rice husk added is 150-200 kg.
[0011] The beneficial effects of adopting the above technical solution are: the present invention changes the production process to converter → VD → LF → continuous casting, reduces the aluminum consumption in the VD process, reduces the Class B inclusions in the steel, shortens the LF heating time, and reduces the inclusions caused by the secondary oxidation of the molten steel. The present invention can shorten the production cycle, reduce the production cost, and significantly reduce the content of Class B inclusions in the steel. The rolled 20-60 mm steel plate is rated according to the A method in GB / T 10561-2005, and the Class B inclusions in the steel plate account for 99% below the C1.5 level and more than 94% below the C0.5 level. DETAILED DESCRIPTION
[0012] The present invention is further described in detail below in conjunction with specific implementation modes.
[0013] The method for reducing the inclusion level of Q345 steel billet and finished steel plate comprises smelting, VD vacuum treatment, LF refining and continuous casting steps performed in sequence; the process of each step is as follows:
[0014] (1) Smelting steps: using converter or electric furnace; slag washing, deoxidation and alloying are carried out before steel is tapped, and 800-1200 kg of lime, 200-500 kg of refined slag, and 100-200 kg of silicon manganese and aluminum particles are added with the steel flow. The amount of silicon manganese added is added to meet the internal control requirements of the steel grade to be produced; the temperature of the molten steel at tapping is ≥1580°C; after tapping, the molten steel is sampled to ensure that the C, Mn and Si elements meet the internal control requirements of the steel grade to be produced, and the slag is well deoxidized and yellow-white.
[0015] (2) VD vacuum treatment steps: The molten steel from the converter is directly fed into the VD furnace. The addition of aluminum wire before VD is determined based on the Al content of the steel sample from the converter. The Al content is controlled to be 0.050% at the beginning of VD. Vacuum treatment is performed, and the vacuum degree is maintained at 66 Pa or below for ≥15 min. The composition of the molten steel sample after vacuum is controlled to meet the internal control requirements of the steel grade.
[0016] (3) LF refining step: After VD is completed, the molten steel enters the LF position and is heated by electricity until the temperature of the molten steel reaches the liquidus line of the steel grade + (50-60)°C; during the heating process, argon gas is soft-blown to ensure that the molten steel is not exposed; after the heating process is completed, the power supply is stopped and the argon gas is turned off, and 150-200 kg of carbonized rice husks are added to the surface of the molten steel for insulation.
[0017] (4) Continuous casting step: LF is refined and continuously cast to obtain Q345 steel plate.
[0018] (5) This method is applicable to Q345 steel. The obtained steel plate is graded according to the A method in GB / T 10561-2005. The Class B inclusions in the steel plate are below C1.5 and account for 99%, and above 94% of the Class B inclusions are below C0.5.
[0019] Example 1: This example produces a 30 mm thick steel plate with a grade of Q345R and a furnace number of 24303925. The specific process steps are as follows:
[0020] (1) Smelting steps: During the steel tapping process, 800 kg of lime, 400 kg of refined slag, 2200 kg of silicon manganese, and 120 kg of aluminum particles are added along with the steel flow. The temperature of the molten steel after tapping is 1598°C.
[0021] (2) VD vacuum treatment steps: 150 m aluminum wire is fed before VD, and the Al content is controlled to reach 0.050% at the beginning of VD; the vacuum degree is kept below 66 Pa for 16 minutes, and the temperature is measured at 1531°C after VD;
[0022] (3) LF refining step: The LF ladle is put into the LF position and powered on to heat up for 17 minutes. The temperature is measured at 1573°C, reaching the liquidus line +57°C. During the heating process, the dual-path argon gas flow rates are controlled at 120 dL / min + 110 dL / min respectively to ensure that the molten steel is not exposed during the process. After the heating process is completed, 150 kg of carbonized rice husk is added for insulation, and then continuous casting is performed.
[0023] (4) The Q345R steel plate obtained in this example was sampled and tested for inclusions, and the results are shown in Table 1;
[0024] Table 1: Inclusion detection results of Q345R steel plate obtained in Example 1
[0025] A thick A thin B thick B thin C thick C Thin D thick D Thin Ds 0 0 0 0.5 0 0 0.5 0.5 0.5
[0026] The chemical composition and mass percentage of the obtained Q345R steel plate are: C 0.17%, Mn 1.49%, Si 0.32%, P 0.012%, S 0.002%, Al 0.035%, Nb 0.018%, and the balance is Fe and unavoidable impurities.
[0027] Embodiment 2: This embodiment produces 40mm thick steel plate, grade Q345E, furnace number 24402678, and the specific process steps are as follows:
[0028] (1) Smelting steps: During the steel tapping process, 900 kg of lime, 300 kg of refined slag, 2000 kg of silicon manganese, and 120 kg of aluminum particles are added along with the steel flow. The temperature of the molten steel after tapping is 1607°C.
[0029] (2) VD vacuum treatment steps: 200 m aluminum wire is fed before VD, and the Al content is controlled to reach 0.050% at the beginning of VD; the vacuum degree is kept below 66 Pa for 15 minutes, and the temperature is measured at 1536°C after VD;
[0030] (3) LF refining step: The ladle is put into the LF position and powered on for 15 minutes. The temperature is measured at 1570°C, reaching the liquidus line + 55°C. During the heating process, the dual-path argon gas flow rates are controlled at 100 dL / min + 100 dL / min respectively, and the molten steel is not exposed during the process. After the heating process is completed, 150 kg of carbonized rice husk is added for insulation, and then continuous casting is performed.
[0031] (4) The Q345E steel plate obtained in this example was sampled and tested for inclusions, and the results are shown in Table 2;
[0032] Table 2: Inclusion detection results of Q345E steel plate obtained in Example 2
[0033] A thick A thin B thick B thin C thick C Thin D thick D Thin Ds 0 0 0 0 0 0 0 0.5 0.5
[0034] The chemical composition and mass percentage of the obtained Q345E steel plate are: C 0.15%, Mn 1.45%, Si 0.36%, P 0.015%, S 0.003%, Al 0.041%, Nb 0.016%, and the balance is Fe and unavoidable impurities.
[0035] Embodiment 3: This embodiment produces 28mm thick steel plate, grade Q345D, furnace number 24403179, and the specific process steps are as follows:
[0036] (1) Smelting steps: During the steel tapping process, 1000 kg of lime, 300 kg of refined slag, 2100 kg of silicon manganese, and 120 kg of aluminum particles are added along with the steel flow. The temperature of the molten steel after tapping is 1615°C.
[0037] (2) VD vacuum treatment steps: 180 m aluminum wire is fed before VD, and the Al content is controlled to reach 0.050% at the beginning of VD; the vacuum degree is kept below 66 Pa for 15 minutes, and the temperature is measured at 1530°C after VD;
[0038] (3) LF refining step: The ladle was put into the LF position and powered on for 18 minutes. The temperature was measured at 1573°C, reaching the liquidus line +58°C. During the heating process, the flow rates of the two-way argon gas were controlled at 100 dL / min + 100 dL / min respectively, and the molten steel was not exposed during the process. After the heating process was completed, 170 kg of carbonized rice husk was added for insulation, and then continuous casting was performed.
[0039] (4) The Q345D steel plate obtained in this example was sampled and tested for inclusions, and the results are shown in Table 3;
[0040] Table 3: Inclusion detection results of Q345D steel plate obtained in Example 3
[0041] A thick A thin B thick B thin C thick C Thin D thick D Thin Ds 0 0 0 1.0 0 0 0.5 0.5 0.5
[0042] The chemical composition and mass percentage of the obtained Q345D steel plate are: C 0.16%, Mn 1.48%, Si 0.30%, P 0.018%, S 0.002%, Al 0.029%, Nb 0.015%, the balance is Fe and unavoidable impurities
[0043] Embodiment 4: This embodiment produces 50mm thick steel plate, grade Q345GJD, furnace number 24404408, and the specific process steps are as follows:
[0044] (1) Smelting steps: During the steel tapping process, 800 kg of lime, 500 kg of refined slag, 1900 kg of silicon manganese, and 180 kg of aluminum particles are added along with the steel flow. The temperature of the molten steel after tapping is 1588°C.
[0045] (2) VD vacuum treatment steps: 200 m aluminum wire is fed before VD, and the Al content is controlled to reach 0.050% at the beginning of VD; the vacuum degree is kept below 66 Pa for 15 minutes, and the temperature is measured at 1535°C after VD;
[0046] (3) LF refining step: The ladle was put into the LF position and powered on for 17 minutes. The temperature was measured at 1566°C, reaching the liquidus line + 51°C. During the heating process, the dual-path argon gas flow rates were controlled at 100 dL / min + 100 dL / min, respectively, and the molten steel was not exposed during the process. After the heating process was completed, 190 kg of carbonized rice husks were added for insulation, and then continuous casting was performed.
[0047] (4) The Q345GJD steel plate obtained in this example was sampled and tested for inclusions, and the results are shown in Table 4;
[0048] Table 4: Inclusion detection results of Q345GJD steel plate obtained in Example 4
[0049] A thick A thin B thick B thin C thick C Thin D thick D Thin Ds 0 0 0 0.5 0 0 0 0.5 0.5
[0050] The chemical composition and mass percentage of the obtained Q345GJD steel plate are: C 0.12%, Mn 1.39%, Si 0.25%, P 0.013%, S 0.002%, Al 0.033%, Nb 0.017%, and the balance is Fe and unavoidable impurities.
[0051] Embodiment 5: This embodiment produces 36mm thick steel plate, grade Q345D, furnace number 24303752, and the specific process steps are as follows:
[0052] (1) Smelting steps: During the steel tapping process, 900 kg of lime, 300 kg of refined slag, 2000 kg of silicon manganese, and 100 kg of aluminum particles are added along with the steel flow. The temperature of the molten steel after tapping is 1599°C.
[0053] (2) VD vacuum treatment steps: 200 m aluminum wire is fed before VD, and the Al content is controlled to reach 0.050% at the beginning of VD; the vacuum degree is kept below 66 Pa for 15 minutes, and the temperature is measured at 1532°C after VD;
[0054] (3) LF refining step: The ladle was put into the LF position and powered on for 15 minutes. The temperature was measured at 1568°C, reaching the liquidus line +53°C. During the heating process, the flow rates of the two-way argon gas were controlled at 100 dL / min + 100 dL / min respectively, and the molten steel was not exposed during the process. After the heating process was completed, 160 kg of carbonized rice husk was added for insulation, and then continuous casting was switched to pouring steel.
[0055] (4) The Q345D steel plate obtained in this example was sampled and tested for inclusions, and the results are shown in Table 5;
[0056] Table 5: Inclusion detection results of Q345D steel plate obtained in Example 5
[0057] A thick A thin B thick B thin C thick C Thin D thick D Thin Ds 0 0 0 1 0 0 0 0.5 0.5
[0058] The chemical composition and mass percentage of the obtained Q345D steel plate are: C 0.17%, Mn 1.44%, Si 0.28%, P 0.017%, S 0.003%, Al 0.040%, Nb 0.016%, and the balance is Fe and unavoidable impurities.
[0059] Example 6: This example produces a 40 mm thick steel plate with a grade of Q345R and a furnace number of 24404150. The specific process steps are as follows:
[0060] (1) Smelting steps: During the steel tapping process, 1200 kg of lime, 200 kg of refined slag, 2200 kg of silicon manganese, and 150 kg of aluminum particles are added along with the steel flow. The temperature of the molten steel after tapping is 1580°C.
[0061] (2) VD vacuum treatment steps: 200 m aluminum wire is fed before VD, and the Al content is controlled to reach 0.050% at the beginning of VD; the vacuum degree is kept below 66 Pa for 15 minutes, and the temperature is measured at 1530°C after VD;
[0062] (3) LF refining step: The ladle was put into the LF position and powered on for 19 minutes. The temperature was measured at 1570°C, reaching the liquidus line + 55°C. During the heating process, the flow rates of the two-way argon gas were controlled at 100 dL / min + 100 dL / min respectively, and the molten steel was not exposed during the process. After the heating process was completed, 200 kg of carbonized rice husks were added for insulation, and then continuous casting was switched to pouring steel.
[0063] (4) The Q345R steel plate obtained in this example was sampled and tested for inclusions. The results are shown in Table 6;
[0064] Table 6: Inclusion detection results of Q345R steel plate obtained in Example 6
[0065] A thick A thin B thick B thin C thick C Thin D thick D Thin Ds 0 0 0 0 0 0 0 0 0.5
[0066] The chemical composition and mass percentage of the obtained Q345R steel plate are: C 0.16%, Mn 1.47%, Si 0.37%, P 0.011%, S 0.002%, Al 0.030%, Nb 0.018%, and the balance is Fe and unavoidable impurities.
[0067] Embodiment 7: This embodiment produces 25mm thick steel plate, grade Q345E, furnace number 24404954, and the specific process steps are as follows:
[0068] (1) Smelting steps: During the steel tapping process, 1100 kg of lime, 200 kg of refined slag, 2000 kg of silicon manganese, and 200 kg of aluminum particles are added along with the steel flow. The temperature of the molten steel after tapping is 1589°C.
[0069] (2) VD vacuum treatment steps: 200 m aluminum wire is fed before VD, and the Al content is controlled to reach 0.050% at the beginning of VD; the vacuum degree is kept below 66 Pa for 15 minutes, and the temperature is measured at 1537°C after VD;
[0070] (3) LF refining step: The ladle was put into the LF position and powered on for 18 minutes. The temperature was measured at 1571°C, reaching the liquidus line +56°C. During the heating process, the flow rates of the two-way argon gas were controlled at 100 dL / min+100 dL / min respectively, and the molten steel was not exposed during the process. After the heating process was completed, 180 kg of carbonized rice husks were added for insulation, and then continuous casting was performed.
[0071] (4) The Q345E steel plate obtained in this example was sampled and tested for inclusions. The results are shown in Table 7;
[0072] Table 7: Inclusion detection results of Q345E steel plate obtained in Example 7
[0073] A thick A thin B thick B thin C thick C Thin D thick D Thin Ds 0 0 0 0.5 0 0 0 0.5 0.5
[0074] The chemical composition and mass percentage of the obtained Q345E steel plate are: C 0.16%, Mn 1.4%, Si 0.29%, P 0.012%, S 0.002%, Al 0.045%, Nb 0.016%, and the balance is Fe and unavoidable impurities.
Claims
1. A method for reducing the inclusion level of Q345 steel billet and finished steel plate, characterized in that: It includes the steps of smelting, VD vacuum treatment, LF refining and continuous casting carried out in sequence; The smelting step comprises: adding lime, refined slag, silicon manganese and aluminum particles along with the steel flow during the steel tapping process, and the temperature of the steel liquid at the tapping temperature is ≥1580°C; The VD vacuum treatment step: determine whether to add aluminum wire before VD according to the Al content of the converter steel, and control the Al content to reach 0.050% at the beginning of VD; during the vacuum treatment, the vacuum degree is 66Pa or less and is maintained for ≥15min; The LF refining steps include: soft blowing of argon gas, supplying electricity to increase the temperature of the molten steel to the liquidus line of the steel grade + (50-60)°C, stopping the supply of electricity and shutting off the argon gas, and adding carbonized rice husks to the surface of the molten steel for heat preservation.
2. The method for reducing the inclusion level of Q345 steel billet and finished steel plate according to claim 1, characterized in that: In the smelting step, 800-1200 kg of lime, 200-500 kg of refined slag and 100-200 kg of aluminum particles are added along with the steel flow.
3. A method for reducing the inclusion level of Q345 steel billet and finished steel plate according to claim 1 or 2, characterized in that: In the LF refining step, the amount of carbonized rice husk added is 150-200 kg.