Pressure vessel steel plate with excellent low-temperature performance for mobile tank car and manufacturing method of pressure vessel steel plate
By using specific chemical composition and process design in steel plates for pressure vessels, the problems of insufficient strength, toughness and resistance to hydrogen-induced cracking in low temperature, high pressure and hydrogen environments have been solved, and high-performance steel plates have been manufactured to meet the needs of large-scale and Demand for high-performance pressure-bearing equipment.
Patent Information
- Application Number
- CN202411041070.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-31
Smart Images

Figure BDA0004972391310000081 
Figure BDA0004972391310000091 
Figure BDA0004972391310000092
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal materials, and in particular to a pressure vessel steel plate for a mobile tank truck with excellent low-temperature performance and a manufacturing method thereof. Background Art
[0002] The service environment of steel plates for pressure vessels is relatively complex, such as low temperature, high pressure, hydrogen, and acid-base environment. Therefore, when selecting the main material steel, the smelting, chemical composition, mechanical properties, metallographic structure and welding process of the steel must be strictly controlled. The performance of metal materials serving under low temperature conditions is quite different from that at room temperature. In order to ensure the reliability of the service performance of steel plates for pressure vessels under low temperature conditions, the steel plates should have good strength and toughness matching. In addition, due to the diversity of the service environment of pressure vessel steel, such as hydrogen and high pressure, it is also necessary to ensure that the steel plates have good resistance to hydrogen-induced cracking.
[0003] With the upgrading of domestic pressure-bearing manufacturing equipment, domestic petrochemical projects are developing in the direction of large-scale and high-performance. The performance and corresponding manufacturing methods of some traditional steels for pressure-bearing equipment can no longer meet the requirements of this development trend. In addition, although some grades can meet the project design requirements at this stage, there is still a need for upgrading in the long run. Therefore, it is urgent to develop a high-strength key material for pressure-bearing equipment that meets the room temperature strength, forming performance, and adapts to complex service environments (such as low temperature, high pressure, hydrogen, etc.).
[0004] The disclosed invention patent "A hydrogen corrosion resistant normalizing type mobile tank car low alloy steel and its preparation method (CN106756536A)" describes a steel plate composed of the following weight percentage components: C0.13-0.20%, Si0.20-0.50%, Mn1.20-1.70%, P≤0.030%, S≤0.010%, Ni0.10-0.45%, Nb0.010-0.050%, V0.010-0.20%, 30ppm≤N≤50ppm, H≤2ppm, 8≤w(V) / w(N)≤15, the remainder is Fe and unavoidable impurities; under the above composition, the normalizing heat treatment method is adopted to produce steel plates with thickness specifications of 6-25mm. No research has been conducted on steel plates with thickness greater than 25mm, and no content related to the control of organizational uniformity and the low temperature impact condition below -46℃ is involved, so the scope of application is narrow. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to propose a pressure vessel steel plate for mobile tank trucks with excellent low temperature performance and a manufacturing method thereof through a new chemical composition design, and adopt a two-stage controlled rolling production process combined with a short-time normalizing heat treatment method to obtain a room temperature tensile strength ≥690MPa, a yield strength ≥595Mpa, an elongation ≥24.5%, and a -60℃ transverse impact energy KV 2 ≥80J, (36~65)mm thick steel plate with excellent plate shape; good resistance to hydrogen-induced cracking, uniform and fine structure, excellent low-temperature performance, low cost, suitable for large-scale production and use, meeting the manufacturing and application requirements of high-performance pressure vessel steel.
[0006] The object of the invention is achieved in this way:
[0007] A pressure vessel steel plate for a mobile tank truck with excellent low-temperature performance, whose chemical composition ranges by mass percentage: C: 0.15%-0.19%, Si: 0.15%-0.36%, Mn: 0.79%-0.98%, P: ≤0.02%, S: ≤0.01%, Cr: 0.02%-0.09%, Ni: 0.61%-0.70%, Nb: 0.015%-0.02%, Re: 0.019%-0.028%, Mg: 0.0009%-0.0017%, and the balance is Fe and unavoidable inclusions.
[0008] Furthermore, in terms of weight percentage, Re / Nb=1-1.8.
[0009] Furthermore, the steel plate has a room temperature of 690MPa≤R m ≤780MPa、595MPa≤R el ≤635MPa, A%≥24.5, -60℃: KV 2 ≥80J, 750MPa≤Rm≤820MPa, 566MPa≤R el ≤628MPa, A%≥36.
[0010] Furthermore, the steel plate microstructure is ferrite+pearlite structure+second phase particles; in terms of volume ratio, ferrite / pearlite=2-2.5; the second phase particles are CrC, NbC, ReC, and have a size of ≤50nm.
[0011] Furthermore, according to the hydrogen induced crack (HIC) test GB / T 8650-2006 and NACE TM0284 "Evaluation Method for Hydrogen Induced Cracking Resistance of Pipeline Steel and Pressure Vessel Steel", after 96h test in solution A and solution B, the crack sensitivity CSR (%), crack length rate CLR (%), and crack width rate CTR (%) of the steel plate were all 0, and the steel plate had excellent hydrogen induced crack resistance. According to GB / T17897-2016 "Corrosion of Metals and Alloys Ferric Chloride Pitting Corrosion Test Method for Stainless Steel", the steel plate showed a corrosion rate of no more than 0.01 in solution A and solution B.
[0012] Furthermore, the thickness of the steel plate is 36-65 mm.
[0013] The reasons for the composition design of the present invention are as follows:
[0014] C: 0.15%~0.19%
[0015] C is the most important element in steel to ensure the strength of the steel plate. If the content is too low, the performance of the steel plate after heat treatment cannot be guaranteed; but if the carbon content is too high, the machining performance of the steel will be affected, and the supersaturated carbide will become the source of fracture cracks, affecting the low-temperature performance of the steel plate and the welding performance during subsequent use. Therefore, the present invention sets the C content range to: 0.15% to 0.19%.
[0016] Si: 0.15%~0.36%
[0017] Si is used as a reducing agent and deoxidizer in the steelmaking process. When the silicon content is too high, it is easy to form hard phase compounds, which increases the brittleness sensitivity of the steel plate and the brittleness of the welding heat affected zone, affects the low temperature performance, and is prone to cracks during later processing. Therefore, the present invention sets the Si content range to 0.15% to 0.36%.
[0018] Mn: 0.79%~0.98%
[0019] The effect of Mn and C is that while increasing the strength of steel, the effect on plasticity is relatively small, and it can reduce the lower critical point of steel, increase the supercooling degree when austenite is cooled, thereby refining the structure and improving the mechanical properties of the steel plate. In addition, the price is relatively cheap. However, too high a Mn content will increase the tendency of hard phase MnS inclusions in the steel, affecting the hydrogen-induced crack resistance of the steel plate, so the present invention sets the Mn content range to 0.79% to 0.98%.
[0020] P:≤0.02%, S:≤0.01%
[0021] S and P are harmful elements in steel and must be strictly controlled to ensure the purity and plasticity of the steel. It is known that MnS produced in steel will affect the strength and toughness of the steel plate, and the presence of P will increase the brittleness of the steel plate and have a negative impact on welding performance. In order to strictly control the generation of harmful inclusions in the steel plate, the present invention is limited to P≤0.02% and S≤0.01%.
[0022] Cr: 0.02%~0.09%
[0023] Cr is a stable carbide element. Its presence in steel can improve the hardenability of the steel plate. The Cr-containing carbide formed is relatively stable. When added in an appropriate amount, it can form a second phase particle with a small size and uniform dispersion, which hinders the growth of grains in the steel plate, and significantly improves the strength of the steel plate, reduces the yield point, and improves the low-temperature performance of the steel plate. At the same time, because it has a good affinity with C, N, and O, it can ensure the excellent hydrogen-induced crack resistance of the steel plate. Therefore, the present invention sets the Cr content range to 0.02% to 0.09%.
[0024] Ni: 0.61%~0.70%
[0025] As an important strengthening element in steel, Ni can improve the strength of steel plates while ensuring toughness by strengthening ferrite and increasing pearlite. When a certain amount of Ni is added to carbon steel, the dislocation density of the steel plate can be reduced, the substructure inside the steel plate can be improved, and the carbon content of the steel plate can be appropriately reduced while refining the grains, thereby improving the strength and toughness of the steel plate, thereby having a positive effect on the low-temperature toughness of the steel plate. On the other hand, if the Ni content in the steel plate is too high, it will reduce the resistance of the steel plate to stress corrosion cracking in hydrogen sulfide solutions, and considering the cost factor, the Ni content range is set at 0.61% to 0.70%.
[0026] Nb: 0.015%~0.02%
[0027] Nb is a strong carbide-forming element, and has a strong affinity with C and N in steel. It affects the performance of steel plates in two main forms. First, it dissolves into austenite structure and significantly improves the hardenability of steel. Second, when it exists in the form of carbide and oxide particles, it refines the grains and improves the strength and toughness of steel plates, especially low-temperature performance. Therefore, a certain amount of Nb is added to the steel, which has an extremely strong effect on delaying austenite recrystallization and refining grains during heat treatment processes such as controlled rolling and normalizing. However, when the Nb content in the steel is too high, large-sized second-phase particles will be generated, increasing the brittleness of the steel plate. The present invention sets the Nb content at 0.015% to 0.02%.
[0028] Re: 0.019%~0.028%
[0029] Re can improve the fluidity of steel, reduce non-metallic inclusions, and make the structure of steel dense and pure. Adding appropriate rare earth elements to steel has a good "removal of O and S" effect, and fine particles help improve the impact toughness of steel plates (especially low-temperature toughness). The addition of Re can easily combine with O to form a dense oxide film, so Re can improve the corrosion resistance of steel plates. Considering the cost factors, the present invention sets the Re content at 0.019% to 0.028%.
[0030] Mg: 0.0009%~0.0017%
[0031] The Mg element can reduce the number and size of inclusions in steel, making the distribution more uniform and the morphology improved. Trace amounts of Mg in steel can significantly improve the size and distribution of carbides in steel, making the carbide particles small and uniform, thereby improving the corrosion resistance and overall performance of the steel. The present invention sets the Mg content at 0.0009% to 0.0017%.
[0032] The study found that in order to give full play to the strengthening effect of the second phase particles in the steel plate, reduce impurity elements such as S, O, and N, further improve the purity of the steel plate, and achieve the purpose of improving the strength and toughness matching of the steel plate, the ratio of the content of Re and Nb in the steel plate by weight percentage is between 1 and 1.8.
[0033] The second technical solution of the present invention is to provide a method for manufacturing a pressure vessel steel plate for a mobile tank truck with excellent low temperature performance, including alloying smelting, continuous casting, slab heating, rolling, heat treatment, and straightening;
[0034] Smelting
[0035] Specifically, it includes molten iron pretreatment - converter smelting - outside furnace refining (LF) - vacuum degassing (VD).
[0036] Hot metal pretreatment process: To improve smelting efficiency, molten steel is smelted in a converter. To reduce production costs, high-quality scrap steel and hot metal are used as raw materials, and the hot metal content is controlled at 79-82%. To ensure that the subsequent steel plate structure is uniform and fine, the hot metal is pre-spheroidized. To reduce burnout and slag volume and reduce the manufacturing cost of the core wire, a cored wire with a Mg content of 30% to 34% is selected; to reduce the loss of steel plates during production and prevent hot metal from splashing, the height-to-diameter ratio of the hot metal column should be between 1.2 and 1.5; to ensure the spheroidization efficiency and the dense uniformity of the subsequent structure, the wire feeding length is controlled at 25-27m, and the wire feeding speed is controlled at 26-31m / min.
[0037] Converter smelting process
[0038] In order to ensure the purity of steel, effectively control the content of harmful elements P, and ensure the efficiency of decarburization, dephosphorization and decarburization are carried out separately in a converter, with oxygen blowing for dephosphorization controlled at 7 to 11 minutes, and oxygen blowing for decarburization controlled at 10 to 12 minutes, ultimately reducing the P mass fraction to less than 0.01%; deep desulfurization treatment is carried out in the LF refining furnace, and the sulfur content is strictly controlled below 0.006%; degassing is completed in the VD furnace, with a net cycle time of 10 to 15 minutes and a calming time of 3 to 6 minutes before pouring.
[0039] Slab heating
[0040] The continuous casting slab is sent to the heating furnace for heating. A four-stage heating method is adopted. The temperature range of the first heating section is controlled at 780-840°C, the temperature range of the second heating section is controlled at 906-942°C, the temperature range of the third heating section is controlled at 982-1066°C, and the heating temperature range of the fourth heating section is 1205-1234°C. The total time in the furnace is 1.5-2.4h. In order to ensure the internal quality of the steel plate and improve the heating efficiency, the heating method of segmented heating of the casting is selected, and the heating temperature range is 780-1234°C. The total heating time of the slab is controlled at 1.5-2.4h. The heating temperature in the first stage is controlled at 780-840℃ to ensure that the billet is fully preheated and to avoid excessive thermal stress inside the billet due to too fast heating speed; the second stage is controlled at 906-942℃, that is, heating within the austenite temperature range to ensure complete phase change, further release internal stress, and further improve the uniformity of the organization; the temperature range of the third heating section is controlled at 982-1066℃ to ensure uniform heating of the billet, high thermal energy utilization rate of the furnace, and reduced energy consumption. The heating temperature range used in the fourth stage is 1205-1234℃. When the heating temperature is lower than 1205℃, the coarse precipitates in the continuous casting billet cannot be dissolved, the billet austenitization is incomplete, and the final rolling temperature of the first stage cannot be guaranteed; when the heating temperature is higher than 1234℃ and the heating time in the high temperature section is too long, it is easy to cause the fine precipitates in the continuous casting billet to dissolve again and cause excessive growth of the grains.
[0041] Rolling process:
[0042] The rolling adopts two-stage controlled rolling, the rolling temperature of the recrystallization zone starts at 1120-1160℃, and the rolling end temperature is 1070-1122℃. In order to fully refine the original austenite structure, increase the number of original effective grain boundaries, and ensure the production efficiency of steel plates. Therefore, large deformation and rapid rolling are adopted, the rolling speed is 5.8-6.2m / s, and the single-pass reduction is controlled at 8%-11%; the starting rolling temperature of the non-recrystallization zone is 952-995℃, the final rolling temperature is 770-830℃, the total reduction is controlled at 38%-51%, and small deformation and multi-pass rapid rolling is adopted, the rolling speed is 5.4-5.7m / s. At this time, the austenite grains are elongated in the rolling direction, the effective grain boundary area is further increased, the internal deformation bands are increased, the ferrite phase deformation nuclei are increased, and the ferrite grain size is further reduced, thereby ensuring the uniform and fine structure of the finished steel plate. After rolling, a controlled cooling method is adopted, with the starting temperature controlled at 740-790°C, the ending temperature at 535-560°C, the cooling rate controlled at 46-52°C / min, and then cooled to room temperature.
[0043] Heat treatment process:
[0044] Short-time normalizing heat treatment is adopted. Since elements such as C, Si, Mn, P, S, Cr, Ni, Nb, and Re are added to the steel, a ferrite + pearlite structure with excellent strength and toughness can be obtained after the steel plate is rolled. The volume ratio of ferrite to pearlite structure is 2 to 2.5, but the grain size distribution of the steel plate is uneven, and there is concentration of structural stress and thermal stress, which is prone to delayed cracking during flame cutting. Therefore, heat treatment should be used in time to homogenize the structure, soften and eliminate stress. In order to further control the internal structure of the steel plate and ensure high production efficiency at the same time, the present invention adopts a short-time normalizing heat treatment method to ensure that the strength of the steel plate is not lost while having suitable plastic toughness, low temperature performance, and good processing performance. Therefore, the normalizing temperature is controlled at 890 to 920°C, the holding time is 11 to 26 minutes, and the furnace is air-cooled.
[0045] Straightening
[0046] A combination of hot and cold straightening is used. First, the plate shape is controlled by hot straightening to improve the surface quality and control the deformation between 2% and 4%. Cold straightening is further used to control the deformation between 1% and 2%, increase the proportion of special small-angle grain boundaries near the surface of the steel plate, reduce the proportion of substructures, and improve the corrosion resistance of the steel plate.
[0047] The beneficial effects of the present invention are:
[0048] (1) On the basis of strengthening elements C, Si, and Mn, by adding appropriate amounts of alloying elements Cr, Ni, Nb, and Re, while strictly controlling the content of harmful elements P and S, combined with production process optimization, a refined and pure microstructure is obtained. The microstructure is ferrite + pearlite + uniformly fine and dispersed second phase particles. By volume ratio, ferrite / pearlite = 2 to 2.5. The size of the second phase particles CrC, NbC, and ReC is less than 50nm and the ratio of the three is between (2:0.7:0.4) and (2:1:0.5), which ensures the steel plate's strong plasticity while having good low temperature performance, corrosion resistance, and processing performance.
[0049] (2) The present invention adopts a combination of advanced molten iron pretreatment + efficient billet heating process + two-stage controlled rolling method + efficient short-time normalizing heat treatment system to produce a pressure vessel steel plate with a thickness of 36 to 65 mm. The steel plate has a uniform and pure structure, good strength and toughness matching, and excellent low-temperature performance and hydrogen-induced crack resistance. Its mechanical properties are as follows: 690MPa≤R m ≤780MPa、595MPa≤R el ≤635MPa, A%≥24.5, -60℃: KV 2 ≥80J, 750MPa≤Rm≤820MPa, 566MPa≤Rel≤628MPa, A%≥36, and excellent corrosion resistance.
[0050] (3) According to the hydrogen induced crack (HIC) test GB / T 8650-2006 and NACE TM0284 "Method for evaluating the resistance of pipeline steel and pressure vessel steel to hydrogen induced cracking", after the steel plate was tested in solution A and solution B for 96 hours, the crack sensitivity CSR (%), crack length rate CLR (%), and crack width rate CTR (%) were all 0, indicating that the steel plate had excellent resistance to hydrogen induced cracking. According to GB / T 17897-2016 "Corrosion of metals and alloys - Ferric chloride pitting test method for stainless steel", the corrosion rate of the steel plate in solution A and solution B was no more than 0.01 g / m 2 .h. The results show that the steel plate has excellent corrosion resistance. DETAILED DESCRIPTION
[0051] The present invention will be further described below by way of examples.
[0052] The embodiment of the present invention carries out alloying smelting, continuous casting, slab heating, rolling, heat treatment and straightening according to the component ratio of the technical solution, and is characterized in that:
[0053] Heating process
[0054] The heating method of the ingot is four-stage heating. The temperature range of the first heating section is controlled at 780-840°C, the temperature range of the second heating section is controlled at 906-942°C, the temperature range of the third heating section is controlled at 982-1066°C, the heating temperature range of the fourth heating section is 1205-1234°C, and the total heating time is 1.5-2.4h;
[0055] Rolling process:
[0056] The rolling adopts two-stage controlled rolling. The starting rolling temperature of the recrystallization zone is 1120-1160℃, the ending rolling temperature is 1070-1122℃, large deformation rapid rolling is adopted, the rolling speed is 5.8-6.2m / s, and the single-pass reduction is controlled at 8%-11%; the starting rolling temperature of the non-recrystallization zone is 952-995℃, the final rolling temperature is 770-830℃, the total reduction is controlled at 38%-51%, and small deformation multi-pass rapid rolling is adopted, and the rolling speed is 5.4-5.7m / s. After the rolling is completed, the controlled cooling method is adopted, the starting temperature is controlled at 740-790℃, the ending temperature is 535-560℃, the cooling rate is controlled at 46-52℃ / min, and then cooled to room temperature.
[0057] Heat Treatment:
[0058] Use short-time normalizing heat treatment; control the normalizing temperature at 890-920°C, the holding time at 11-26min, and air-cool after exiting the furnace.
[0059] Furthermore, the straightening process adopts a combination of hot straightening and cold straightening, the hot straightening controls the deformation amount between 2% and 4%, and the cold straightening controls the deformation amount between 1% and 2%.
[0060] The embodiments specifically illustrate the present invention. These embodiments are only general descriptions of the present invention and are not intended to limit the present invention.
[0061] Table 1 shows the chemical composition of the embodiment of the present invention, Table 2 shows the process parameters of hot metal pretreatment, smelting and continuous casting heating of the embodiment, Table 3 shows the process parameters of steel plate rolling and heat treatment, Table 4 shows the heat treatment and straightening process of steel plate, Table 5 shows the final effect of mechanical properties of the embodiment, Table 6 shows the test results of grain size and inclusion grade evaluation of steel plate structure of the embodiment. Table 7 shows the test results of corrosion resistance (anti-hydrogen cracking test, pitting test) of the embodiment.
[0062] Table 1 Chemical composition of the examples (wt, %)
[0063]
[0064] Table 2 Example molten iron pretreatment, smelting and continuous casting billet heating process parameters
[0065] Example 1 2 3 4 5 6 7 8 9 10 Hot metal content / % 79 81 80 79 79 79 80 79 79 80 Mg content of cored wire / % 32 31 30 30 30 31 32 30 33 31 Height-to-diameter ratio of liquid iron column 1.32 1.34 1.43 1.37 1.35 1.38 1.50 1.39 1.36 1.34 Feeding line length / m 25 26 27 26 25 26 27 26 25 26 Feeding speed / (m / min) 29 27 31 30 26 28 31 29 31 28 Decarburization oxygen blowing time / min 11 11 12 10 10 12 10 12 11 12 Dephosphorization oxygen blowing time / min 11 8 9 9 10 9 11 9 10 8 Net cycle time / min 12 11 14 13 12 15 14 12 13 10 Sedation time / min 4 5 6 3 6 3 5 4 6 4 First stage heating temperature / ℃ 802 790 796 823 812 799 832 789 792 823 Second stage heating temperature / ℃ 923 932 940 933 921 912 910 922 920 909 Three-stage heating temperature / ℃ 990 994 993 1064 1052 1045 1033 1020 1011 982 Four-stage heating temperature / ℃ 1206 1211 1207 1218 1216 1212 1220 1229 1225 1224 Total heating time / h 1.9 1.8 2.3 2 1.9 1.7 2.3 2.2 2.1 1.9
[0066] Table 3 Steel plate rolling and cooling process parameters
[0067]
[0068] Table 4 Steel plate heat treatment and straightening process
[0069]
[0070] Table 5 Mechanical properties of the examples Final results
[0071]
[0072] Table 6 Test results of grain size and inclusion grade evaluation of steel plate structure in Example
[0073]
[0074] Note: According to GB / T 10561-2023 "Standard Rating Chart Microscopic Examination Method for Determination of Non-metallic Inclusion Content in Steel"
[0075] It is stipulated that Class A is sulfide inclusions, Class B is alumina inclusions, Class C is silicate inclusions, Class D is spherical oxide inclusions, and Class DS is large-particle spherical oxide inclusions.
[0076] Table 7 shows the test results of the corrosion resistance (hydrogen crack resistance test, pitting test) of the embodiment
[0077]
[0078] According to the above results, it can be concluded that the mechanical properties of the steel plate for high temperature resistant and high homogeneous pressure vessel with excellent plate shape and thickness of (36-65) mm provided by the present invention are as follows: 690 MPa≤R m ≤780MPa、595MPa≤R el ≤635MPa, A≥24.5%, -60℃: KV 2 ≥80J, 750MPa≤Rm≤820MPa, 566MPa≤R el ≤628MPa, A%≥36, with fine and uniform structure throughout the thickness, excellent plasticity and toughness, low temperature performance, corrosion resistance and good processing performance.
[0079] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.
Claims
1. A pressure vessel steel plate for mobile tank trucks with excellent low temperature performance, characterized in that: Calculated by weight percentage, it includes the following components: C: 0.15% ~ 0.19%, Si: 0.15% ~ 0.36%, Mn: 0.79% ~ 0.98%, P: ≤ 0.02%, S: ≤ 0.01%, Cr: 0.02% ~ 0.09%, Ni: 0.61% ~ 0.70%, Nb: 0.015% ~ 0.02%, Re: 0.019% ~ 0.028%, Mg: 0.0009% ~ 0.0017%, and the balance is Fe and unavoidable inclusions.
2. The pressure vessel steel plate for mobile tank trucks with excellent low temperature performance according to claim 1, characterized in that: In terms of weight percentage, Re / Nb=1-1.
8.
3. The pressure vessel steel plate for mobile tank trucks with excellent low temperature performance according to claim 1, characterized in that: The steel plate is 690MPa≤R at room temperature m ≤780MPa、595MPa≤R el ≤635MPa, A%≥24.5, at -60℃: KV2≥80J, 750MPa≤R m ≤820MPa、566MPa≤R e l≤628MPa, A%≥36.
4. The pressure vessel steel plate for mobile tank trucks with excellent low temperature performance according to claim 1, characterized in that: The steel plate microstructure is ferrite+pearlite structure+second phase particles; by volume ratio, ferrite / pearlite=2-2.5; the second phase particles are CrC, NbC, ReC, and have a size of ≤50nm.
5. The pressure vessel steel plate for mobile tank trucks with excellent low temperature performance according to claim 1, characterized in that: The thickness of the steel plate is 36-65 mm.
6. A method for manufacturing a pressure vessel steel plate for a mobile tank truck with excellent low temperature performance according to any one of claims 1 to 5, comprising alloying smelting, continuous casting, slab heating, rolling, heat treatment, and straightening, characterized in that: Heating process The ingot is heated in four stages, with the temperature range of the first heating stage controlled at 780-840°C, the temperature range of the second heating stage controlled at 906-942°C, the temperature range of the third heating stage controlled at 982-1066°C, and the temperature range of the fourth heating stage controlled at 1205-1234°C. The total heating time is 1.5-2.4h. Rolling process: The rolling adopts two-stage controlled rolling, the starting rolling temperature of the recrystallization zone is 1120-1160°C, the ending rolling temperature is 1070-1122°C, large deformation rapid rolling is adopted, the rolling speed is 5.8-6.2m / s, and the single-pass reduction is controlled at 8%-11%; the starting rolling temperature of the non-recrystallization zone is 952-995°C, the final rolling temperature is 770-830°C, the total reduction is controlled at 38%-51%, small deformation multi-pass rapid rolling is adopted, and the rolling speed is 5.4-5.7m / s; after the rolling is completed, the controlled cooling method is adopted, the starting temperature is controlled at 740-790°C, the ending temperature is controlled at 535-560°C, the cooling rate is controlled at 46-52°C / min, and then cooled to room temperature; Heat Treatment: Use short-time normalizing heat treatment; control the normalizing temperature at 890-920°C, the holding time at 11-26min, and air-cool after exiting the furnace.
7. The method for manufacturing a pressure vessel steel plate for a mobile tank truck with excellent low temperature performance according to claim 6, characterized in that: The straightening process adopts a combination of hot straightening and cold straightening. The hot straightening controls the deformation amount between 2% and 4%; the cold straightening controls the deformation amount between 1% and 2%.
Citation Information
Patent Citations
Hydrogen-corrosion-resistant normalized low-alloy steel for mobile tanker and preparation method of hydrogen-corrosion-resistant normalized low-alloy steel
CN106756536A
Acid corrosion resistant steel for soleplate in hull and production method thereof
CN102732799A
High-strength and low-yield ratio easy-to-weld movable pressure vessel steel plate and manufacturing method thereof
CN107338392A
800MPa-grade hydrogen-induced crack resistant container steel plate and production method thereof
CN115369323A
Normalizing pressure vessel steel plate easy to weld and manufacturing method
CN115896616A